Batteries and electrical equipment

By limiting the thickness difference between the main area and the thinned area of ​​the lithium battery electrode and calculating the N/P value, the problem of real-time control of the thickness detection of the thinned area during the lithium battery coating process is solved, reducing the risk of lithium plating and improving battery performance and safety.

CN118040012BActive Publication Date: 2026-11-10JIANGSU ZENIO NEW ENERGY BATTERY TECH CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410346144.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-25
Publication Date
2026-11-10
Estimated Expiration
2044-03-25

AI Technical Summary

Technical Problem

In existing technologies, the thickness of the thinned area during the coating process of lithium battery electrodes cannot be controlled in real time, resulting in large differences in the thickness of the thinned area, which affects the battery's cycle performance and safety performance, and lacks theoretical guidance.

Method used

A battery design scheme is provided, which calculates the N/P value of the thinned region by limiting the thickness difference between the main region and the thinned region of the positive and negative electrode sheets, ensuring that the ratio of ΔLca to ΔLa is greater than or equal to the ratio of (Lca1-Lca set) to (La1-La set), and sets the thickness control range of the thinned region to reduce the risk of lithium plating.

Benefits of technology

It achieves theoretical specifications for the thickness of the thinned area, reduces or avoids the risk of lithium plating, improves battery quality, and provides practical production guidance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118040012B_ABST
    Figure CN118040012B_ABST
Patent Text Reader

Abstract

This invention relates to the field of electrode technology, specifically to a battery and an electrical device. The provided battery includes a positive electrode and a negative electrode, both of which include a current collector and an active material layer disposed on at least one surface of the current collector along its thickness direction. The active material layer includes a main region and thinned regions located on both sides of the main region along a first direction; the thickness of the main region of the positive electrode is L. ca1 The thickness of the thinned region of the positive electrode sheet is L. ca2 The thickness of the current collector in the positive electrode is L. ca集 The thickness of the main body region of the negative electrode sheet is L. a1 The thickness of the thinned region of the negative electrode sheet is L. a2 The thickness of the current collector in the negative electrode is L. a集 Among them, L ca1 -L ca2 =ΔL ca L a1 -L a2 =ΔL a ΔL ca With ΔL a The ratio is greater than or equal to (L) ca1 -L ca集 ) and (L a1 -L a集 The ratio of ) to ). This application can theoretically control the thickness of the electrode thinning region, reduce or avoid the risk of lithium deposition in the thinning region, and can play a good guiding role in the control of the thinning region.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of electrode technology, and more specifically, to a battery and an electrical device. Background Technology

[0002] In batteries, such as lithium-ion batteries, the electrode plates typically consist of a current collector (e.g., foil) and a coating (active material layer). The coating is formed by applying a coating material onto the current collector. Since the slurry is a Newtonian fluid, material buildup easily occurs at the edges during coating, affecting the edge thickness and subsequent rolling. Thinning the edges of the electrode coating helps protect the battery during charging, and a uniform coating process has a certain impact on battery capacity, internal resistance, and cycle life. Generally, during the coating process, the thickness of the coating edge area is controlled by nozzle pads. The thickness at the edges is thinner than the larger surface area, thus dividing the electrode coating into a non-thinned area (also called the large surface area or main area) and thinned areas located on both sides of the non-thinned area.

[0003] In related technologies, the thinned area is inspected to check whether it meets the requirements for lithium battery production. Currently, in the coating process of lithium batteries, the thickness and width of the thinned area are measured using a micrometer or ten-thousand-finger caliper. Furthermore, the thinned area inspection can only be performed on the outermost side (tail side) after electrode coating is completed, and real-time coating control of the thinned area cannot be achieved. The reasonableness of the thickness difference in the thinned area is crucial, affecting not only the battery's cycle performance but also its safety performance. For example, if the thickness of the thinned area is unreasonable, it can easily lead to lithium plating risk, thus affecting battery performance. Currently, the industry's control standards for the thinned area are mostly based on empirical values. Typically, there is a thickness difference of several micrometers to tens of micrometers between the thinned area at the electrode edge and the large non-thinned area. The standard range is wide, lacking theoretical guidance.

[0004] In view of this, the present invention is hereby proposed. Summary of the Invention

[0005] In view of this, the present invention aims to at least partially solve one of the technical problems in the related art. To this end, the present invention provides a battery and electrical device that provides theoretical support for controlling the thickness of the thinned region, reducing or avoiding the risk of lithium plating in the thinned region.

[0006] To solve the above-mentioned technical problems, this application is implemented as follows:

[0007] According to one aspect of this application, an embodiment of this application provides a battery including a positive electrode and a negative electrode, each of the positive electrode and the negative electrode including a current collector and an active material layer disposed on at least one surface of the current collector along the thickness direction, the active material layer including a main region and thinned regions located on both sides of the main region along a first direction.

[0008] The thickness of the main body region of the positive electrode sheet is L. ca1 The thickness of the thinned region of the positive electrode sheet is L. ca2 The thickness of the positive electrode current collector is L. ca集 ;

[0009] The thickness of the main body region of the negative electrode sheet is L. a1 The thickness of the thinned region of the negative electrode sheet is L. a2 The thickness of the negative electrode current collector is L. a集 ;

[0010] The L ca1 L ca2 L ca集 L a1 L a2 L a集 Satisfy the following equation (1):

[0011]

[0012] Where, ΔL ca ΔL represents the thickness difference between the main region and the thinned region of the positive electrode sheet. ca =L ca1 -L ca2 ;

[0013] ΔL a ΔL represents the thickness difference between the main body region and the thinned region of the negative electrode sheet. a =L a1 -L a2 .

[0014] In addition, the battery according to this application may also have the following additional technical features:

[0015] In some of these implementations, the ΔL ca and the ΔL a Satisfy: ΔL ca ≥1.458ΔL a .

[0016] In some embodiments, the active material layer of the positive electrode is disposed on two surfaces of the current collector along the thickness direction, and the sum of the thicknesses of the thinned areas of the positive electrode on the two surfaces ranges from 0 to 25 μm; the active material layer of the negative electrode is disposed on two surfaces of the current collector along the thickness direction, and the sum of the thicknesses of the thinned areas of the negative electrode on the two surfaces ranges from 0 to 25 μm.

[0017] In some embodiments, the thickness of the thinned region of the positive electrode gradually decreases along the direction away from the main body region of the positive electrode; the thickness of the thinned region of the negative electrode gradually decreases along the direction away from the main body region of the negative electrode; the thickness L of the thinned region of the positive electrode... ca2 The average thickness of the thinned region of the positive electrode sheet; the thickness L of the thinned region of the negative electrode sheet. a2 The average thickness of the thinned region of the negative electrode sheet.

[0018] In some embodiments, the N / P values ​​of the thinned negative electrode region and the thinned positive electrode region satisfy the following equation (2) with the N / P values ​​of the main body regions of the negative electrode and the positive electrode:

[0019]

[0020] In some of these embodiments, the N / P value of the main body region is a known value, and the N / P value of the main body region ranges from 1.10 to 1.15.

[0021] In some of these embodiments, the thinned region N / P satisfies the following equation (3):

[0022]

[0023] The main region N / P satisfies the following equation (4):

[0024]

[0025] Where, q ca and q a These represent the specific capacity of the positive electrode and the specific capacity of the negative electrode, respectively, in mAh / g.

[0026] ρ ca and ρ a These represent the compacted density of the positive electrode and the compacted density of the negative electrode, respectively, in g / cm³. 3 ;

[0027] loading ca and loading a These represent the proportions of the positive electrode active material and the negative electrode active material, respectively.

[0028] By relating equations (3) and (4), we obtain the following formula (5):

[0029]

[0030] The N / P value of the thinned area is calculated using the formula (5).

[0031] In some of these embodiments, by modifying equation (5), the following equation (6) is obtained:

[0032]

[0033] Equation (1) is obtained based on equation (6) and equation (2).

[0034] In some of these embodiments, the N / P ratios of the negative and positive electrodes satisfy the following equation (7):

[0035]

[0036] S ca and S a These represent the surface density of the positive electrode and the surface density of the negative electrode, respectively, in g / cm³. 2 ;

[0037] The S ca and S a They satisfy the following equations (8) and (9) respectively.

[0038] ρ ca =S ca / L ca1 (8)

[0039] ρ a =S a / L a1 (9)

[0040] Equations (3) and (4) are derived from equations (7), (8) and (9).

[0041] According to another aspect of this application, an embodiment of this application provides an electrical device that includes the aforementioned battery.

[0042] Implementing the technical solution of the present invention has at least the following beneficial effects:

[0043] In this embodiment, the active material layer of both the positive and negative electrode sheets includes a main region and a thinned region. The thickness of the thinned region does not exceed the thickness of the main region. This is achieved by making ΔL... ca With ΔL a The ratio is greater than or equal to (L) ca1 -L ca集 ) and (L a1 -L a集The ratio of ) can effectively reduce or avoid the risk of lithium plating in the thinned area of ​​the battery. By ensuring that the thickness of the positive and negative electrode body area, the thinned area, and the current collector meets the above conditions, it is possible to determine whether the thickness of the thinned area is poorly designed, whether lithium plating is likely to occur, and to design an appropriate threshold for controlling the thickness of the thinned area, thereby helping to ensure the quality of the battery cell.

[0044] According to the present invention, given known cell design information such as the coating thickness of the positive and negative electrodes (i.e., the thickness of the main body area) and the current collector thickness of the positive and negative electrodes, the thickness control range of the thinning area for the non-lithium-deposited positive and negative electrodes can be determined. Thus, the thickness control range of the thinning area can be reasonably regulated from a theoretical perspective, which has practical production guidance significance.

[0045] Additional aspects and advantages of this application will be set forth in part in the description which follows, and in part will be obvious from the description, or may be learned by practice of the invention. Attached Figure Description

[0046] The above and other objects, features, and advantages of the present invention will become more apparent from the more detailed description of the embodiments of the invention in conjunction with the accompanying drawings. The drawings are provided to further illustrate the embodiments of the invention and form part of the specification. They are used together with the embodiments of the invention to explain the invention and do not constitute a limitation thereof. In the drawings, the same reference numerals generally represent the same parts or steps.

[0047] Figure 1 The diagram shown is a structural schematic of a battery provided in an embodiment of the present invention;

[0048] Figure 2 The diagram shown is a schematic diagram of lithium deposition in a thinning zone according to an embodiment of the present invention;

[0049] Figure 3 The figure shown is a correlation diagram between the N / P value and the thickness difference between the thinning areas of the positive and negative electrodes and the large surface area provided in the embodiment of the present invention.

[0050] Explanation of reference numerals in the attached figures:

[0051] 10-Positive electrode sheet;

[0052] 110 - Positive electrode current collector;

[0053] 120 - Positive electrode body region;

[0054] 130 - Positive electrode sheet thinning area;

[0055] 20-Negative electrode sheet;

[0056] 210 - Negative electrode current collector;

[0057] 220 negative electrode plate main body area;

[0058] 230 - Negative electrode thinning area;

[0059] 30 - Separating membrane. Detailed Implementation

[0060] The present application will be further described below with reference to specific embodiments. It should be understood that these embodiments are for illustrative purposes only and are not intended to limit the scope of the present application.

[0061] The endpoints and any values ​​of the ranges disclosed herein are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of the various ranges, the endpoint values ​​of the various ranges or individual point values, and individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed herein.

[0062] Unless otherwise specified, all embodiments and optional embodiments of this application can be combined to form new technical solutions. Unless otherwise specified, all technical features and optional technical features of this application can be combined to form new technical solutions.

[0063] Unless otherwise specified, the terms "comprising" and "including" as used in this application can be open-ended or closed-ended. For example, "comprising" and "including" can mean that other components or structures not listed may also be included, or that only the listed components or structures may be included.

[0064] In related technologies, the thickness control of the electrode thinning area is mostly based on empirical values. For example, the width of the thinning area is designed to be 8-15mm, the thickness difference between the thinning area and the main body area is ≤15μm (single-sided), and the thickness difference between the thinning area and the main body area is ≤25μm (double-sided). These are all based on past experience and the defined ranges are relatively broad. However, the N / P ratio of the thinning area can vary greatly due to the difference in the thickness of the thinning area. If the thinnest thinning area of ​​the negative electrode corresponds to the thickest thinning area of ​​the positive electrode, the battery will have a lithium plating problem. That is, if the thickness design of the thinning area is unreasonable, it is easy to cause lithium plating in the battery.

[0065] In view of this, the inventors of this application have theoretically standardized the thickness control range of the thinning zone, reducing or avoiding the risk of lithium plating in the thinning zone. This method is highly accurate and practical, providing theoretical support for the thickness control of the thinning zone. The invention will now be described in detail.

[0066] Please see Figures 1 to 3As shown, in some embodiments, a battery is provided, which includes a positive electrode 10 and a negative electrode 20. Both the positive electrode 10 and the negative electrode 20 include a current collector and an active material layer disposed on at least one surface of the current collector along the thickness direction. The active material layer includes a main region and thinned regions located on both sides of the main region along a first direction.

[0067] The aforementioned current collector has two surfaces in the thickness direction, such as a first surface and a second surface. The active material layer is disposed on at least one surface of the current collector in the thickness direction, that is, the active material layer can be disposed on both surfaces of the current collector in the thickness direction, i.e., the active material layer is disposed on both the first surface and the second surface; or, the active material layer can be disposed on one surface of the current collector in the thickness direction, such as on the first surface or the second surface.

[0068] As an example, this embodiment is mainly described with the active material layer disposed on two surfaces of the current collector along its thickness direction, namely the first surface and the second surface. It is understood that in other embodiments, the active material layer may be disposed on either the first surface or the second surface of the current collector.

[0069] Both the positive electrode 10 and the negative electrode 20 described above include a current collector and an active material layer. For example, the positive electrode 10 includes a positive electrode current collector 110 and a positive active material layer, and the negative electrode 20 includes a negative electrode current collector 210 and a negative active material layer. The active material layer includes a main region and thinned regions located on both sides of the main region along a first direction. For example, along the first direction, the active material layer includes a thinned region, a main region, and a thinned region connected in sequence. The first direction can be the width direction of the positive or negative electrode (or in some cases, the length direction). As an example, thinned regions are provided on both sides of the active material layer in the width direction, and the thinned regions extend along the length direction. A main region is provided between the thinned regions on both sides.

[0070] Along the first direction, the positive electrode active material layer includes a positive electrode thinning region 130, a positive electrode body region 120 and a positive electrode thinning region 130 connected in sequence, and the negative electrode active material layer includes a negative electrode thinning region 230, a negative electrode body region 220 and a negative electrode thinning region 210 connected in sequence.

[0071] In this embodiment, the thickness of the positive electrode body region 120 is L. ca1 The thickness of the thinned region 130 of the positive electrode sheet is L. ca2 The thickness of the positive electrode current collector 110 is L. ca集 The thickness of region 220 of the negative electrode body is L. a1 The thickness of the negative electrode thinning region 230 is L. a2 The thickness of the negative electrode current collector 210 is L.a集 .

[0072] It should be noted that the active material layer refers to the coated active material layer, not the rolled active material layer, i.e., the active material layer formed by coating the slurry onto the current collector. The coated active material layer includes a main area and a thinned area. The thickness of the main area and the thinned area refers to the thickness of the main area and the thickness of the thinned area after coating; however, the rolled electrode may not have a thinned area. Typically, in the electrode preparation process, the positive and negative electrode slurries are sprayed onto the current collector, resulting in a significant thickness difference between the thinned area and the main area of ​​the coated electrode. Further, rolling the coated electrode with a roll press can improve the compaction density and uniformity of the active material in the battery electrode, and improve the adhesion of the active material. After rolling, the material area is stretched with the foil, resulting in a uniform thickness of the entire electrode.

[0073] By creating a thinned zone on the electrode through coating, subsequent coating processes are facilitated, avoiding uneven coating and dripping, thus ensuring coating quality. Furthermore, it guarantees the uniformity and precision of the coating thickness. Additionally, the thinning and uniform distribution of the coating layer makes the surface of the coating roller smoother. This improves coating smoothness, reduces bubbles and defects on the coating surface, and results in a more aesthetically pleasing coating.

[0074] This embodiment defines the thickness relationship between the electrode body region, the thinned region, and the current collector, so that L ca1 L ca2 L ca集 L a1 L a2 L a集 Satisfy the following equation (1):

[0075]

[0076] Where, ΔL ca ΔL represents the thickness difference between the main region and the thinned region of the positive electrode sheet. ca =L ca1 -L ca2 ;

[0077] ΔL a ΔL represents the thickness difference between the main body region and the thinned region of the negative electrode sheet. a =L a1 -L a2 .

[0078] Therefore, by making ΔL ca With ΔL a The ratio is greater than or equal to (L) ca1 -L ca集 ) and (L a1 -La集 The ratio of ) can effectively reduce or avoid the risk of lithium plating in the thinned area of ​​the battery. By ensuring that the thickness of the positive and negative electrode body area, the thinned area, and the current collector meets the above conditions, it is possible to determine whether the thickness of the thinned area is poorly designed, whether lithium plating is likely to occur, and to design an appropriate threshold for controlling the thickness of the thinned area, thereby helping to ensure the quality of the battery cell.

[0079] According to the present invention, given known cell design information such as the coating thickness of the positive and negative electrodes (i.e., the thickness of the main body area) and the current collector thickness of the positive and negative electrodes, the thickness control range of the thinning area for the non-lithium-deposited positive and negative electrodes can be determined. Thus, the thickness control range of the thinning area can be reasonably regulated from a theoretical perspective, which has practical production guidance significance.

[0080] It should be explained that in batteries, N stands for negative and P stands for positive. The N / P value represents the ratio of the battery's negative electrode capacity to its positive electrode capacity, that is, N / P represents the negative electrode capacity / positive electrode capacity.

[0081] In this embodiment of the invention, the N / P of the thinning region can be calculated based on the design range of the N / P of the main region, and then the above formula (1) can be obtained. In this way, the thickness of the thinning region can be reasonably controlled or standardized from a theoretical point of view, reducing or avoiding the risk of lithium plating in the thinning region. This method is simple to operate, highly accurate, and highly applicable. It can play a good guiding role in controlling the thickness of the thinning region, and provides theoretical support for controlling the thickness of the thinning region.

[0082] According to this application, the thinning region N / P can be calculated based on the design range of the main region N / P, and the above formula (1) can be further obtained, which may specifically include:

[0083] Obtain the thickness L of the main body region 120 of the positive electrode sheet. ca1 The thickness L of the negative electrode body region 220 a1 The thickness L of the thinned region of the positive electrode sheet is 130. ca2 The thickness L of the negative electrode thinning region 230 a2 ;

[0084] Calculate the thickness difference between the main body region 120 and the thinned region 130 of the positive electrode sheet, that is, the thickness difference (both sides) of the thinned region 130 of the positive electrode sheet relative to the main body region 120 of the positive electrode sheet, ΔL. ca =L ca1 -L ca2 Calculate the thickness difference between the main body region 220 and the thinned region 230 of the negative electrode sheet, that is, the thickness difference (both sides) of the thinned region 230 of the negative electrode sheet relative to the main body region 220 of the negative electrode sheet, ΔL. a =L a1 -L a2 ;

[0085] Based on the specific capacity, areal density, and ratio of negative electrode active material of the negative electrode sheet, and the specific capacity, areal density, and ratio of positive electrode active material of the positive electrode sheet, the formula for calculating the N / P value of the electrode sheet is obtained. Here, the areal density of the negative electrode sheet is equal to the compacted density of the negative electrode sheet multiplied by L. a1 The product of L and L, the surface density of the positive electrode is equal to the compaction density of the positive electrode and L. ca1 The product;

[0086] Based on the calculation formula for the N / P value of the electrode, the N / P value of the main region of the electrode is compared with L. a1 L a集 L ca1 L ca集 Correlate the N / P value of the thinned region of the electrode with L. a1 ΔL a L a集 L ca1 ΔL ca L ca集 Related; based on the N / P value of the main region of the electrode, L a1 ΔL a L a集 L ca1 ΔL ca and L ca集 The N / P value of the thinned region of the electrode was calculated.

[0087] In some embodiments, the N / P value of the electrode satisfies the following equation (7):

[0088]

[0089] Where, q ca and q a These represent the specific capacity of the positive electrode and the specific capacity of the negative electrode, respectively, in mAh / g.

[0090] loading ca and loading a These represent the proportions of the positive electrode active material and the negative electrode active material, respectively.

[0091] S ca and S a These represent the surface density of the positive electrode and the surface density of the negative electrode, respectively, in g / cm³. 2 .

[0092] S ca and S a They satisfy the following equations (8) and (9) respectively.

[0093] ρ ca =S ca / L ca1 (8)

[0094] ρ a =S a / L a1 (9)

[0095] ρ ca and ρ a These represent the compacted density of the positive electrode and the compacted density of the negative electrode, respectively, in g / cm³. 3 .

[0096] According to this embodiment, the N / P ratio is calculated by the specific capacity, areal density and active material ratio of the positive and negative electrode sheets using the above formula (7). The above formulas (8) and (9) can be obtained by the relationship between compaction density, areal density and thickness. When the above formulas (8) and (9) are substituted into formula (7), the N / P ratio can be associated with the thickness of the electrode sheet.

[0097] Optionally, the thickness L of the main region of the positive electrode sheet is obtained as described above. ca1 Thickness L of the negative electrode body region a1 Thickness L of the thinned region of the positive electrode sheet ca2 The thickness L of the negative electrode thinning region a2 One method is to cut test specimens from the coating areas of the positive and negative electrodes, respectively, and use a micrometer to measure the thinned area of ​​the test specimen to obtain the thickness L of the thinned area of ​​the positive electrode. ca2 The thickness L of the negative electrode thinning region a2 Similarly, a micrometer is used to measure the main body area of ​​the test piece to obtain the thickness L of the main body area of ​​the positive electrode sheet. ca1 The thickness L of the negative electrode body region a1 Furthermore, this method can be used to test product quality on the production line.

[0098] Therefore, based on the above correlation between the N / P ratio and the electrode thickness, formulas for the N / P ratio of the thinned region and the N / P ratio of the main body region can be derived respectively. For example, in some embodiments, the N / P ratio of the thinned region satisfies the following formula (3), and the N / P ratio of the main body region satisfies the following formula (4):

[0099]

[0100]

[0101] Where, q ca and q a These represent the specific capacity of the positive electrode and the specific capacity of the negative electrode, respectively, in mAh / g.

[0102] ρ ca and ρ aThese represent the compacted density of the positive electrode and the compacted density of the negative electrode, respectively, in g / cm³. 3 ;

[0103] loading ca and loading a These represent the proportions of the positive electrode active material and the negative electrode active material, respectively.

[0104] By linking equations (3) and (4), we obtain the following formula (5):

[0105]

[0106] The N / P value of the thinned area is calculated using equation (5).

[0107] Furthermore, by transforming equation (5), we can obtain the following equation (6):

[0108]

[0109] Therefore, in equation (6), the ratio of N / P in the thinned region to N / P in the main region and the thickness of each electrode, such as ΔL, are used. ca ΔL a The thickness of the current collector and the main body area were correlated.

[0110] Optionally, the N / P ratio of the main region mentioned above is a known value, L. a1 L a集 L ca1 and L ca集 The actual measured value, ΔL a According to L a1 and L a2 The calculated value, ΔL ca According to L ca1 and L ca2 The calculated value obtained.

[0111] Optionally, the N / P value of the main region can be in the range of 1.10 to 1.15. Typically, the N / P ratio of the main region is a fixed value, such as 1.10 to 1.15, for example, 1.10, 1.11, 1.12, 1.13, 1.14, 1.15, etc.

[0112] Therefore, by using the above formula (6), the ratio of N / P in the thinned region to N / P in the main region can be used to determine whether the thickness of the thinned region is poorly designed, whether lithium plating is likely to occur, and to determine the appropriate threshold for controlling the thickness of the thinned region.

[0113] In this embodiment of the invention, the thickness parameter involved in equations (3) to (6) above can be a measured value or a calculated value, and other parameters can be a theoretical design value or a fixed value.

[0114] As shown in equation (6) above, in order to avoid lithium deposition in the thinned region, the ratio of the N / P ratio in the thinned region to the N / P ratio in the main region needs to be greater than or equal to 1, that is,

[0115]

[0116] Thus, we can obtain the following equation (2):

[0117]

[0118] In other words, to avoid lithium deposition in the thinned areas, the N / P values ​​of the thinned areas of the negative electrode and the positive electrode must satisfy the above equation (2) with the N / P values ​​of the main areas of the negative electrode and the positive electrode. Therefore, based on equations (6) and (2), by modifying them, equation (1) of this invention can be obtained.

[0119]

[0120] Therefore, based on the above, at least two determinations can be made according to the above relationship. For example, one determination is to calculate the N / P ratio of the thinned area based on known cell design information such as the thickness of the positive and negative electrode main body region, the thickness of the positive and negative electrode current collector, and the thickness difference between the positive and negative electrode main body region and the thinned area. Based on this, it can be determined whether there is a risk of lithium plating in the thinned area. Another determination is to determine the thickness control range of the positive and negative electrode thinned areas to prevent lithium plating in the thinned area based on known cell design information such as the thickness of the positive and negative electrode main body region and the thickness of the positive and negative electrode current collector. That is, in order to ensure that the thinned area does not plating lithium, the positive and negative electrode thinned areas need to meet the conditions shown in the above formula (1).

[0121] Optionally, the active material layer of the positive electrode is disposed on two surfaces of the current collector along the thickness direction, and the sum of the thicknesses of the thinned areas of the positive electrode on the two surfaces ranges from 0 to 25 μm; the active material layer of the negative electrode is disposed on two surfaces of the current collector along the thickness direction, and the sum of the thicknesses of the thinned areas of the negative electrode on the two surfaces ranges from 0 to 25 μm.

[0122] The sum of the thicknesses of the thinned regions on the two surfaces of the positive electrode current collector can range from 0 to 25 μm, excluding 0; the sum of the thicknesses of the thinned regions on the two surfaces of the negative electrode current collector can range from 0 to 25 μm, excluding 0. Under these thickness range conditions, and when the above formula (1) is satisfied, lithium deposition in the thinned regions can be prevented.

[0123] In some embodiments, the thickness of the thinned region of the positive electrode gradually decreases along the direction away from the main body region of the positive electrode; the thickness of the thinned region of the negative electrode gradually decreases along the direction away from the main body region of the negative electrode; the thickness L of the thinned region of the positive electrode... ca2 The average thickness of the thinned region of the positive electrode sheet; the thickness L of the thinned region of the negative electrode sheet. a2 This represents the average thickness of the thinned region of the negative electrode sheet.

[0124] The aforementioned current collector may include a coating area and a tab area. The coating area is used to deposit the active material layer, and the tab area is used to connect the tabs. The tab area may be located on both sides of the coating area. The thickness of the aforementioned positive electrode sheet thinning area gradually decreases along the direction away from the positive electrode sheet body area. For example, the thickness of the thinning area near the positive electrode sheet body area is the largest, while the thickness of the thinning area near the tab can be 0. Similarly, the thickness of the aforementioned negative electrode sheet thinning area gradually decreases along the direction away from the negative electrode sheet body area. For example, the thickness of the thinning area near the negative electrode sheet body area is the largest, while the thickness of the thinning area near the tab can be 0. Optionally, the width of the positive or negative electrode sheet thinning area can be 4mm to 6mm, for example, approximately 5mm.

[0125] Furthermore, such as Figure 3 As shown, multiple sets of experiments were conducted to verify the embodiments of the present invention. Figure 3 The "large area" in the middle refers to the main body area. After multiple experiments and processing of the experimental data, ΔL can be obtained. ca and ΔL a The relationship. In some embodiments, ΔL ca and ΔL a Satisfy: ΔL ca ≥1.458ΔL a When ΔL is satisfied ca ≥1.458ΔL a This can prevent lithium plating in the thinned area.

[0126] In some embodiments, the battery further includes a separator 30 disposed between the positive electrode 10 and the negative electrode 20. This application does not impose any particular limitations on the separator 30, as long as it achieves the purpose of this application.

[0127] Therefore, this invention calculates the N / P ratio of the thinned area based on the design range of the main electrode area, and then theoretically regulates the thickness control range of the thinned area to reduce or avoid the risk of lithium plating in the thinned area. Through the above formula derivation, at least two determinations can be made: First, given known cell design information such as the thickness of the positive and negative electrode main electrode areas, the thickness of the positive and negative electrode current collectors, and the thickness difference between the main electrode areas and the thinned area, the N / P ratio of the thinned area can be calculated to determine whether lithium plating occurs in the thinned area. Second, given known cell design information such as the thickness of the positive and negative electrode main electrode areas and the thickness of the positive and negative electrode current collectors, the thickness control range of the positive and negative electrode thinned areas without lithium plating can be determined. Based on the actual production capacity and the N / P ratio of the electrode main electrode area, designing the actual thickness control range of the thinned area has practical production guidance significance.

[0128] In some embodiments, this application also provides an electrical device that includes the aforementioned battery.

[0129] The battery in this application embodiment can be used as a power source for electrical devices or as an energy storage unit for electrical devices. Electrical devices can be, but are not limited to, mobile devices such as mobile phones, tablets, laptops, e-book players, electric toys, power tools, lighting fixtures, etc., electric vehicles such as electric bicycles, electric cars, electric bikes, electric trucks, etc., or they can also be electric trains, aircraft, energy storage systems, etc.

[0130] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the present invention will be further described below in conjunction with specific embodiments. The following embodiments describe the content disclosed in this application in more detail. These embodiments are merely illustrative, as various modifications and variations within the scope of the disclosure of this application will be apparent to those skilled in the art.

[0131] Example 1

[0132] Obtain the thickness L of the main body region of the positive electrode sheet ca1 Thickness L of the negative electrode body region a1 Thickness L of the thinned region of the positive electrode sheet ca2 The thickness L of the negative electrode thinning region a2 For example, test specimens can be cut from the coating areas of the positive and negative electrodes respectively, and a micrometer can be used to test the main body area and the thinned area of ​​the electrode. The thickness L of the main body area of ​​the positive electrode is... ca1 The thickness L of the negative electrode body region is 190 μm. a1 The thickness L of the thinned region of the positive electrode sheet is 125 μm. ca2 The thickness L of the thinned region of the negative electrode sheet is 179.35 μm. a2 The value is 116.47 μm. Relevant data for the electrode are shown in Table 1 below.

[0133] The thickness difference ΔL between the main region and the thinned region of the positive electrode sheet ca =L ca1 -L ca2 =10.65μm.

[0134] The thickness difference ΔL between the main body region and the thinned region of the negative electrode sheet a =L a1 -L a2 =8.53μm.

[0135] In this embodiment, the positive electrode current collector is made of Al, and the negative electrode current collector is made of Cu. The thickness of the positive electrode current collector is L. ca集 That is, L Al The thickness is 15 μm; the thickness of the current collector in the negative electrode is L. a集 That is, L Cu It is 5μm.

[0136] According to the above formula (7), the N / P ratio can be obtained as follows:

[0137]

[0138] Furthermore, according to the above formula (8)ρ ca =S ca / L ca1 Sum of formula (9)ρ a =S a / L a1 By analyzing the relationship between compaction density, surface density, and thickness, the N / P values ​​for the main region and the thinned region can be obtained, as shown below:

[0139]

[0140]

[0141] The above N / P ratio represents the main body N / P area, and the N / P thinning area represents the thinning area N / P; L Cu It represents L a集 That is, the thickness of the current collector in the negative electrode sheet; L Al It represents L ca集 That is, the thickness of the current collector in the positive electrode plate.

[0142] thus,

[0143] In addition, by substituting the above thickness values ​​into equation (6), the ratio of the thinned area N / P to the main body N / P can be obtained.

[0144]

[0145] This verifies the accuracy of the formula provided by the present invention.

[0146] The above calculations demonstrate the accuracy of the formula provided by this invention. Using the simplified formula, only the designed N / P ratio and the actual tested thickness of the thinned region are needed to determine whether the current thinned region is prone to lithium plating. The formula and data acquisition method provided by this invention are simple, quick, and yield highly accurate results. The ratio of the N / P ratio of the thinned region to the N / P ratio of the main region can indicate whether the thickness of the thinned region is poorly designed; when this ratio is less than 1, lithium plating is likely to occur.

[0147] Table 1

[0148]

[0149] like Figure 2 As shown, the ratio of N / P in the thinned region to N / P in the main region is 0.989, which is less than 1. Figure 2 It can be seen that when the ratio of N / P in the thinned region to N / P in the main region is less than 1, lithium plating is likely to occur.

[0150] Combining Table 1 and Figure 2 It can be seen that when the ratio of N / P in the thinned region to N / P in the main region is less than 1, lithium plating is likely to occur.

[0151] Furthermore, according to Substituting the thickness of the main body area and the current collector thickness into the above values, we can obtain...

[0152]

[0153] That is, when ΔL is satisfied ca ≥1.458ΔL a This can reduce or avoid lithium plating in the thinned area; see [reference needed]. Figure 3 As shown.

[0154] Example 2

[0155] To further verify the accuracy of the formula provided in this invention, multiple sets of experiments were conducted. These included actual measurements of the thickness of the main positive and negative electrode regions and the thickness of the thinned positive and negative electrode regions, calculations were performed using the provided formula, and the electrodes were disassembled to verify whether lithium plating occurred. See Table 2 below for details.

[0156] Table 2

[0157]

[0158]

[0159] From Table 2 or in combination Figure 2 and Figure 3 It can be seen that when ΔL is satisfied ca ≥1.458ΔL a When the thinning area is thinned, lithium deposition can be avoided. In addition, in combination with the above formula (2), that is, when the ratio of the N / P ratio of the thinned area to the N / P ratio of the main area is greater than or equal to 1, lithium deposition in the thinned area can be avoided.

[0160] According to the embodiments of the present invention, the thickness difference between the thinned area of ​​the negative electrode sheet and the main body area of ​​the negative electrode sheet is greater than the thickness difference between the thinned area of ​​the positive electrode sheet and the main body area of ​​the positive electrode sheet. As a result, there is less lithium deposition in the thinned area of ​​the cell, which is consistent with the calculation formula and logic of the N / P ratio.

[0161] Typically, the N / P ratio of the main body region of an electrode is a fixed value. Cell designers control the N / P ratio of the main body region of the electrode between 1.1 and 1.15. Due to the thickness difference in the thinned region, the contact between them relies more on the electrolyte to ensure lithium-ion transport. Therefore, it is necessary to reduce the N / P ratio of the thinned region to reduce the risk of lithium plating. As shown by the formula provided in this invention, the N / P ratio of the thinned region is strongly correlated with the thickness of the thinned region. By limiting the thickness of the thinned region, the N / P ratio of the thinned region can be controlled. Furthermore, this invention, through formula and linear R-squared, preferably uses a ratio of negative electrode thinned region thickness difference relative to the main body region / positive electrode thinned region thickness difference relative to the main body region > 1.42. In theoretical design, the design data should be tightened, and the ratio of negative electrode thinned region thickness difference relative to the main body region / positive electrode thinned region thickness difference relative to the main body region should be > 1.35 (tightening by ~5%).

[0162] In summary, in actual production, timely adjustments can be made based on the thickness difference of the thinned area to reduce lithium plating caused by abnormal N / P ratio in the thinned area.

[0163] The parts of this invention not described in detail are techniques known to those skilled in the art.

[0164] The basic principles of the present invention have been described above with reference to specific embodiments. However, it should be noted that the advantages, benefits, and effects mentioned in the present invention are merely examples and not limitations, and should not be considered as essential features of each embodiment of the present invention. Furthermore, the specific details disclosed above are for illustrative and facilitative purposes only, and are not limitations. These details do not limit the present invention to the necessity of employing the aforementioned specific details.

[0165] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them; although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some of the technical features; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A battery comprising a positive electrode and a negative electrode, characterized in that, Both the positive electrode and the negative electrode include a current collector and an active material layer disposed on at least one surface of the current collector along the thickness direction. The active material layer includes a main region and thinned regions located on both sides of the main region along a first direction. The thickness of the main body region of the positive electrode sheet is L. ca1 The thickness of the thinned region of the positive electrode sheet is L. ca2 The thickness of the positive electrode current collector is L. ca集 ; The thickness of the main body region of the negative electrode sheet is L. a1 The thickness of the thinned region of the negative electrode sheet is L. a2 The thickness of the negative electrode current collector is L. a集 ; The L ca1 L ca2 L ca集 L a1 L a2 L a集 Satisfy the following equation (1): (1) Where, ∆L ca ∆L represents the thickness difference between the main body region and the thinned region of the positive electrode sheet. ca =L ca1 -L ca2 ; ∆L a ∆L represents the thickness difference between the main body region and the thinned region of the negative electrode sheet. a =L a1 -L a2 ; ΔL ca =13~17μm; ∆L a =3~9μm; The ∆L ca and the ΔL a Satisfy: ∆L ca ≥1.458∆L a ; The N / P values ​​of the thinned negative electrode region and the thinned positive electrode region satisfy the following equation (2) with the N / P values ​​of the main body region of the negative electrode and the main body region of the positive electrode: (2); The thickness L of the thinned region of the positive electrode sheet ca2 The average thickness of the thinned region of the positive electrode sheet; The thickness L of the thinned region of the negative electrode sheet a2 The average thickness of the thinned region of the negative electrode sheet.

2. The battery according to claim 1, characterized in that, The active material layer of the positive electrode sheet is disposed on two surfaces of the current collector along the thickness direction, and the sum of the thicknesses of the thinned areas of the positive electrode sheet on the two surfaces ranges from 0 to 25 μm. The active material layer of the negative electrode sheet is disposed on two surfaces of the current collector along the thickness direction, and the sum of the thicknesses of the thinned areas of the negative electrode sheet on the two surfaces ranges from 0 to 25 μm.

3. The battery according to claim 2, characterized in that, Along the direction away from the main body region of the positive electrode sheet, the thickness of the thinned region of the positive electrode sheet gradually decreases; Along the direction away from the main body region of the negative electrode sheet, the thickness of the thinned region of the negative electrode sheet gradually decreases.

4. The battery according to claim 1, characterized in that, The N / P value of the main region is a known value, and the range of the N / P value of the main region is 1.10 to 1.

15.

5. The battery according to claim 1, characterized in that, The thinning region N / P satisfies the following equation (3): (3) The main region N / P satisfies the following equation (4): (4) Where, q ca and q a These represent the specific capacity of the positive electrode and the specific capacity of the negative electrode, respectively, in mAh / g. ρ ca and ρ a These represent the compacted density of the positive electrode and the compacted density of the negative electrode, respectively, in g / cm³. 3 ; loading ca and loading a These represent the proportions of the positive electrode active material and the negative electrode active material, respectively. By relating equations (3) and (4), we obtain the following formula (5): (5) The N / P value of the thinned area is calculated using the above formula (5).

6. The battery according to claim 5, characterized in that, By transforming equation (5), we obtain the following equation (6): (6) Equation (1) is obtained based on Equation (6) and Equation (2).

7. The battery according to claim 5, characterized in that, The N / P values ​​of the negative electrode and the positive electrode satisfy the following equation (7): (7) S ca and S a These represent the surface density of the positive electrode and the surface density of the negative electrode, respectively, in g / cm³. 2 ; The S ca and S a They satisfy the following equations (8) and (9) respectively. r ca =S ca / L ca1 (8) r a =S a / L a1 (9) Equations (3) and (4) are obtained based on equations (7), (8) and (9).

8. An electrical appliance, characterized in that, Includes the battery as described in any one of claims 1 to 7.

Citation Information

Patent Citations

  • Preparation method of battery pole piece, die head gasket and battery

    CN113130839A

  • Lithium ion battery

    CN117039117A

  • Electrode assembly and manufacturing method and manufacturing system therefor, battery cell and battery

    WO2022165689A1