Preparation method of sulfide electrolyte powder sintered in nitrogen-containing atmosphere and negative electrode-free solid-state lithium battery

By sintering sulfide electrolyte powder in a nitrogen-containing atmosphere and designing without anode, the stability and energy density problems of all-solid-state sulfide batteries are solved, and battery performance with high air stability and high energy density is achieved.

CN118040073BActive Publication Date: 2024-10-18ANAI NEW ENERGY TECHNOLOGY (YANCHENG) CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410368249.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-28
Publication Date
2024-10-18
Estimated Expiration
2044-03-28

AI Technical Summary

Technical Problem

All-solid-state sulfide batteries have problems such as poor stability, narrow electrochemical windows, and violent interface reactions, which limit their application. Moreover, the problem of lithium consumption during the charge and discharge process of negative electrode-free batteries needs to be solved urgently.

Method used

A preparation method for sintered sulfide electrolyte powder in a nitrogen-containing atmosphere and a negative-electrode solid-state lithium battery is adopted. The air stability and ion conductivity of the sulfide electrolyte are improved through ball milling and sintering processes, and lithium sulfide and lithium nitride are used in the battery as The cathode material forms the final oxidation product of nitrogen to avoid side reactions.

Benefits of technology

It significantly improves the air stability of the sulfide electrolyte and the energy density of the battery, inhibits the formation of lithium dendrites, reduces the lithium consumption of the negative SEI layer, and improves the safety and energy density of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118040073B_ABST
    Figure CN118040073B_ABST
Patent Text Reader

Abstract

A method for preparing a sulfide electrolyte powder sintered in a nitrogen-containing atmosphere and a negative electrode-free solid-state lithium battery belongs to the technical field of all-solid-state lithium batteries. The method comprises: (1) weighing a certain mass of precursors and mixing them evenly by a ball mill; placing the mixture in a closed container and evacuating it; then introducing a certain amount of nitrogen-containing gas and sealing the container; heating the sealed container, sintering it at a constant temperature, and cooling it to obtain a sulfide electrolyte powder sintered in a nitrogen-containing atmosphere. (2) The negative electrode-free solid-state lithium battery is formed by using a sulfide electrolyte powder sintered in a nitrogen-containing atmosphere as an electrolyte, lithium sulfide powder as a positive electrode, and lithium nitride as a lithium supplement, and assembling it with a current collector.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of all-solid-state lithium batteries, and in particular relates to a method for preparing a sulfide electrolyte powder sintered in a nitrogen-containing atmosphere and a negative-electrode-free solid-state lithium battery. Background Art

[0002] High-energy lithium-ion batteries have dominated the electronics market over the past few decades and are now expanding to electric vehicles and grid-scale stationary storage. All-solid-state batteries are considered one of the next-generation energy storage technologies that can compete with or even surpass the most advanced liquid lithium-ion batteries. By replacing organic liquid electrolytes with non-flammable solid electrolytes, all-solid-state batteries are expected to solve the safety issues associated with flammable organic electrolytes and enable applications over a wide temperature range.

[0003] With the in-depth study of solid electrolytes in solid-state batteries, the ionic conductivity of sulfide solid electrolytes is almost comparable to that of organic liquid electrolytes, but the stability of all-solid-state sulfide batteries is still not ideal, mainly limited by the poor air stability of the electrolyte, narrow electrochemical window, and violent interfacial reactions. It is urgent to develop an electrolyte system with high air resistance and interface stability, and optimize the preparation method of electrolyte materials, which will help promote the large-scale and mass production of solid electrolyte materials and realize their commercial application. In addition, the anode-free battery that has emerged in recent years has further improved the energy density of the battery by eliminating the use of the anode, and is considered to be the ultimate goal of lithium batteries. Therefore, combining the concept of solid-state batteries with the concept of no anode to construct a stable anode-free solid-state battery is expected to achieve both high battery safety and high energy density. Summary of the invention

[0004] The purpose of the present invention is to improve the wet air stability of sulfide electrolyte and the energy density of all-solid-state sulfide battery, and provide a simple preparation method of sulfide electrolyte powder sintered in nitrogen-containing atmosphere and anode-free solid lithium battery, which is used to improve the air stability and ionic conductivity of sulfide solid electrolyte material. By sintering sulfide precursor in nitrogen-containing gas atmosphere, the sulfide electrolyte material obtained after sintering contains nitrogen, has a certain ability to resist water vapor and inhibit lithium dendrites. At the same time, lithium sulfide positive electrode and lithium nitride lithium supplement agent are used as cathode-free solid battery positive electrode, which can further improve battery energy density on the one hand, and can also be used to compensate for lithium consumption for the formation of negative electrode SEI layer during charging and discharging. In addition, the final oxidation product of lithium nitride as lithium supplement agent in the first cycle is nitrogen, which will not participate in the subsequent electrochemical reaction of solid battery and will not affect battery performance.

[0005] To achieve the above purpose, the technical solution adopted by the present invention is as follows:

[0006] A method for preparing sulfide electrolyte powder sintered in a nitrogen-containing atmosphere, the method comprising the following steps:

[0007] Step 1: Weigh the electrolyte precursor, put the precursor mixture into a ball mill, and ball mill at a speed of 50-600 r / min for 0.5-6 h to obtain a uniform mixture;

[0008] Step 2: Place the homogeneous mixture in step 1 in a sealed container and evacuate the container;

[0009] Step 3: introducing nitrogen-containing gas into the vacuumed sealed container and sealing the container;

[0010] Step 4: After heating the sealed container, sintering at a heat preservation temperature, and cooling the container, sulfide electrolyte powder is obtained.

[0011] Furthermore, in step one, the electrolyte precursor is A:B=n:m; wherein; A is an alkali metal sulfide; preferably A is one or more of lithium sulfide, sodium sulfide, and potassium sulfide; B is a metal or non-metal sulfide; preferably B is one or more of phosphorus pentasulfide, tin disulfide, silicon disulfide, arsenic trisulfide, and germanium sulfide; and the molar ratio of n:m is 0.2 to 5:1.

[0012] Furthermore, in step three, the nitrogen-containing gas is one or more of ammonia, nitric oxide, nitrogen dioxide, and nitrogen tetroxide.

[0013] Furthermore, in step three, the volume of nitrogen-containing gas introduced into each gram of electrolyte precursor is 0.1-100 ml.

[0014] Furthermore, in step 4, the sintering temperature is 100-700° C., and the sintering time is 0.1-25 h.

[0015] A sulfide electrolyte powder sintered in a nitrogen-containing atmosphere prepared by the above preparation method.

[0016] An application of the nitrogen-containing atmosphere sintered sulfide electrolyte powder material prepared by the above preparation method, the application is: for preparing a negative electrode-free solid-state lithium battery.

[0017] Furthermore, the application is:

[0018] Step 1: uniformly mix lithium sulfide powder and carbon nanotube material in a mass ratio of 1:0.05-1, and then ball-mill the mixture with lithium nitride and nitrogen-containing atmosphere sintered sulfide electrolyte powder in a mass ratio of 1:0.05-0.2:0.2-1 to obtain a composite positive electrode powder containing a lithium supplement;

[0019] Step 2: 50-100 mg of nitrogen-containing atmosphere sintered sulfide electrolyte powder is placed in a 16 mm tableting mold and pressed at a pressure of 200 MPa for 10 minutes, then 1-15 mg of composite positive electrode powder containing a lithium supplement is weighed and evenly dispersed on one side of the sulfide electrolyte sheet sintered in a nitrogen-containing atmosphere, and pressed at a pressure of 360 MPa for 10 minutes to obtain a nitrogen-containing atmosphere sintered sulfide electrolyte sheet containing a composite positive electrode;

[0020] Step 3: Place the current collector on the other side of the obtained sulfide electrolyte sheet sintered in a nitrogen atmosphere containing a composite positive electrode, place the above multilayer structure in a battery shell and seal it, and finally obtain a negative electrode-free solid-state battery. There is no active material on the negative electrode side of the negative electrode battery before cycling. During the charging process, lithium is directly deposited on the current collector to form lithium metal, and then the lithium metal is deposited back to the positive electrode during the discharge stage. Therefore, the negative electrode-free battery reduces the overall mass of the battery and helps to improve the battery energy density.

[0021] Furthermore, in step three, the current collector is one of copper foil, aluminum foil, stainless steel foil and titanium foil.

[0022] The negative electrode-free solid-state lithium battery is obtained by the above-mentioned preparation method.

[0023] Compared with the prior art, the present invention has the following advantages:

[0024] (1) In the present invention, the sulfide electrolyte is prepared by directly sintering by adjusting the sintering atmosphere, so that uniform doping of nitrogen can be achieved. Compared with the traditional solid-phase mixing method for nitrogen doping, the defect of uneven distribution of doping elements is avoided.

[0025] (2) The sulfide electrolyte sintered in a nitrogen atmosphere prepared by the present invention has good air stability and can avoid the generation of toxic hydrogen sulfide gas when the electrolyte directly contacts the air.

[0026] (3) The SEI formed at the negative electrode interface of the sulfide electrolyte sintered in a nitrogen atmosphere prepared by the present invention contains lithium nitride, which can promote the uniform deposition of lithium metal and inhibit the formation of lithium dendrites.

[0027] (4) The cathode-free solid-state battery prepared by the present invention uses lithium sulfide as the cathode, and lithium nitride as the lithium supplement further improves the energy density of the sulfide solid-state battery. At the same time, the final oxidation product of lithium nitride is nitrogen gas, which will not react with the battery components and affect the battery performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 is a scanning electron microscope photograph of the sulfide electrolyte powder sintered in a nitrogen-containing atmosphere obtained in Example 1;

[0029] Figure 2This is a graph of the first cycle discharge capacity of a negative electrode-free solid-state battery assembled with sulfide electrolyte powder sintered in a nitrogen-containing atmosphere obtained in Examples 1, 2, and 3. DETAILED DESCRIPTION

[0030] The technical solution of the present invention is further described below in conjunction with the accompanying drawings and embodiments, but is not limited thereto. Any modification or equivalent replacement of the technical solution of the present invention that does not depart from the spirit and scope of the technical solution of the present invention should be included in the protection scope of the present invention.

[0031] Embodiment 1:

[0032] Preparation of sulfide electrolyte powder sintered in nitrogen-containing atmosphere:

[0033] Step 1: Weigh the electrolyte precursor, weigh 2 g of lithium sulfide (Li2S) and phosphorus pentasulfide (P2S5) in a mass ratio of 3:1, put the precursor mixture into a ball mill, and ball mill at a speed of 100 r / min for 2 h to obtain a uniform mixture;

[0034] Step 2: Place the homogeneous mixture in step 1 in a sealed container and evacuate the container;

[0035] Step 3: Pass 50 ml of ammonia gas into the vacuumed sealed container and seal the container;

[0036] Step 4: Heat the sealed container at a rate of 2°C / min to 260°C, sinter for 5 hours, and then cool it down to room temperature at a rate of 2°C / min to obtain sulfide electrolyte powder sintered in a nitrogen-containing atmosphere. Figure 1 As shown, the particle size of the sulfide electrolyte powder obtained by sintering in a nitrogen-containing atmosphere is about 2 to 3 microns and is evenly distributed. Its room temperature ion conductivity is 1.01 mS / cm. After being exposed to air with a relative humidity of 20% for one hour, the ion conductivity is 0.92 mS / cm, proving that the prepared electrolyte has a certain wet air stability.

[0037] Preparation of negative electrode-free solid-state lithium battery:

[0038] Step 1: uniformly mix lithium sulfide powder and carbon nanotube material in a mass ratio of 1:1, and ball-mill the lithium sulfide carbon mixed material with lithium nitride and sulfide electrolyte powder sintered in a nitrogen-containing atmosphere in a mass ratio of 1:0.05:1 to obtain a composite positive electrode powder containing a lithium supplement;

[0039] Step 2: 60 mg of sulfide electrolyte powder sintered in a nitrogen-containing atmosphere was placed in a 16 mm tablet pressing mold and pressed at a pressure of 200 MPa for 10 minutes. Subsequently, 10 mg of composite positive electrode powder containing a lithium supplement was weighed and evenly dispersed on one side of the sulfide electrolyte sheet sintered in a nitrogen-containing atmosphere, and pressed at a pressure of 360 MPa for 10 minutes to obtain a sulfide electrolyte sheet sintered in a nitrogen-containing atmosphere containing a composite positive electrode;

[0040] Step 3: placing a copper foil current collector on the other side of the obtained sulfide electrolyte sheet sintered in a nitrogen atmosphere containing a composite positive electrode, placing the multilayer structure in a battery shell and sealing it, and finally obtaining a negative electrode-free solid-state battery;

[0041] like Figure 2 As shown, the all-solid-state negative electrode-free battery assembled in Example 1 has a high discharge specific capacity of 1368 mAh / g in the first cycle, proving that the composite positive electrode powder containing a lithium supplement and the negative electrode-free design concept can comprehensively improve the energy density of the all-solid-state battery.

[0042] Embodiment 2:

[0043] Preparation of sulfide electrolyte powder sintered in nitrogen-containing atmosphere:

[0044] Step 1: Weigh the electrolyte precursor, weigh 100 g of lithium sulfide (Li2S) and tin disulfide (SnS2) in a mass ratio of 3:2, put the precursor mixture into a ball mill, and ball mill at a speed of 100 r / min for 2 h to obtain a uniform mixture;

[0045] Step 2: Place the homogeneous mixture in step 1 in a sealed container and evacuate the container;

[0046] Step 3: Introduce 200 ml of nitric oxide into the vacuum sealed container and seal the container;

[0047] Step 4: Heat the sealed container at a rate of 5°C / min to 500°C, sinter at this temperature for 10 hours, and then cool it down to room temperature at a rate of 1°C / min to obtain a sulfide electrolyte powder sintered in a nitrogen-containing atmosphere.

[0048] The room temperature ionic conductivity of the sulfide electrolyte powder sintered in the nitrogen-containing atmosphere obtained in Example 2 is 0.85 mS / cm. After being exposed to air with a relative humidity of 40% for one hour, the ionic conductivity is 0.80 mS / cm, which proves that the prepared electrolyte has high wet air stability.

[0049] Preparation of negative electrode-free solid-state lithium battery:

[0050] Step 1: uniformly mix lithium sulfide powder and carbon nanotube material in a mass ratio of 1:0.5, and ball-mill the lithium sulfide carbon mixed material with lithium nitride and sulfide electrolyte powder sintered in a nitrogen-containing atmosphere in a mass ratio of 1:0.1:1 to obtain a composite positive electrode powder containing a lithium supplement;

[0051] Step 2: 70 mg of sulfide electrolyte powder sintered in a nitrogen-containing atmosphere was placed in a 16 mm tablet pressing mold and pressed at a pressure of 200 MPa for 10 minutes. Subsequently, 8 mg of composite positive electrode powder containing a lithium supplement was weighed and evenly dispersed on one side of the sulfide electrolyte sheet sintered in a nitrogen-containing atmosphere, and pressed at a pressure of 360 MPa for 10 minutes to obtain a sulfide electrolyte sheet sintered in a nitrogen-containing atmosphere containing a composite positive electrode;

[0052] Step 3: placing a stainless steel foil current collector on the other side of the obtained sulfide electrolyte sheet sintered in a nitrogen atmosphere containing a composite positive electrode, placing the above multilayer structure in a battery shell and sealing it, and finally obtaining a negative electrode-free solid-state battery;

[0053] like Figure 2 As shown, the all-solid-state negative electrode-free battery assembled in Example 2 has a high discharge specific capacity of 1451 mAh / g in the first cycle, proving that the composite positive electrode powder containing a lithium supplement and the negative electrode-free design concept can comprehensively improve the energy density of the all-solid-state battery.

[0054] Embodiment 3:

[0055] Preparation of sulfide electrolyte powder sintered in nitrogen-containing atmosphere:

[0056] Step 1: Weigh the electrolyte precursor, weigh 50 g of lithium sulfide (Li2S) and germanium sulfide (GeS2) in a mass ratio of 2:1, put the precursor mixture into a ball mill, and ball mill at a speed of 200 r / min for 1 h to obtain a uniform mixture;

[0057] Step 2: Place the homogeneous mixture in step 1 in a sealed container and evacuate the container;

[0058] Step 3: Pass 500 ml of nitrogen dioxide into the vacuumed sealed container and seal the container;

[0059] Step 4: Heat the sealed container at a rate of 10°C / min to 550°C, then sinter at this temperature for 10 hours, and then cool it down to room temperature at a rate of 10°C / min to obtain sulfide electrolyte powder sintered in a nitrogen-containing atmosphere.

[0060] The room temperature ionic conductivity of the sulfide electrolyte powder sintered in the nitrogen-containing atmosphere obtained in Example 3 is 0.61 mS / cm. After being exposed to air with a relative humidity of 18% for one hour, the ionic conductivity is 0.51 mS / cm, which proves that the prepared electrolyte has good wet air stability.

[0061] Preparation of negative electrode-free solid-state lithium battery:

[0062] Step 1: uniformly mix lithium sulfide powder and carbon nanotube material in a mass ratio of 1:0.5, and ball-mill the lithium sulfide carbon mixed material with lithium nitride and sulfide electrolyte powder sintered in a nitrogen-containing atmosphere in a mass ratio of 1:0.1:1 to obtain a composite positive electrode powder containing a lithium supplement;

[0063] Step 2: 80 mg of sulfide electrolyte powder sintered in a nitrogen-containing atmosphere was placed in a 16 mm tablet pressing mold and pressed at a pressure of 200 MPa for 10 minutes. Subsequently, 9 mg of composite positive electrode powder containing a lithium supplement was weighed and evenly dispersed on one side of the sulfide electrolyte sheet sintered in a nitrogen-containing atmosphere, and pressed at a pressure of 360 MPa for 10 minutes to obtain a sulfide electrolyte sheet sintered in a nitrogen-containing atmosphere containing a composite positive electrode;

[0064] Step 3: placing an aluminum foil current collector on the other side of the obtained sulfide electrolyte sheet sintered in a nitrogen atmosphere containing a composite positive electrode, placing the multilayer structure in a battery shell and sealing it, and finally obtaining a negative electrode-free solid-state battery;

[0065] like Figure 2 As shown, the all-solid-state negative electrode-free battery assembled in Example 3 has a high discharge specific capacity of 1392 mAh / g in the first cycle, proving that the composite positive electrode powder containing a lithium supplement and the negative electrode-free design concept can comprehensively improve the energy density of the all-solid-state battery.

Claims

1. Application of a sulfide electrolyte powder material sintered in a nitrogen-containing atmosphere in the preparation of a negative electrode-free solid-state lithium battery, characterized in that: The application is: Step 1: uniformly mix lithium sulfide powder and carbon nanotube material in a mass ratio of 1:0.05-1, and then ball-mill the mixture with lithium nitride and nitrogen-containing atmosphere sintered sulfide electrolyte powder in a mass ratio of 1:0.05-0.2:0.2-1 to obtain a composite positive electrode powder containing a lithium supplement; Step 2: Take 50-100 mg of nitrogen-containing atmosphere sintered sulfide electrolyte powder and place it in a 16 mm tablet pressing mold, press it at a pressure of 200 MPa for 10 minutes, then weigh 1-15 mg of composite positive electrode powder containing lithium supplement and evenly disperse it on one side of the sulfide electrolyte sheet sintered in nitrogen-containing atmosphere, and press it at a pressure of 360 MPa for 10 minutes to obtain a nitrogen-containing atmosphere sintered sulfide electrolyte sheet containing a composite positive electrode; Step 3: placing a current collector on the other side of the obtained sulfide electrolyte sheet sintered in a nitrogen atmosphere containing a composite positive electrode, placing the above multilayer structure in a battery shell and sealing it, and finally obtaining a negative electrode-free solid-state battery; The preparation steps of the sulfide electrolyte powder sintered in a nitrogen-containing atmosphere are as follows: Step 1: Weigh the electrolyte precursor, put the precursor mixture into a ball mill, and mill it at a speed of 50-600 r / min for 0.5-6 hours to obtain a uniform mixture; the electrolyte precursor is A: B = n: m; in; A is an alkali metal sulfide; B is a metal or non-metal sulfide; the molar ratio of n:m is 0.2~5:1; Step 2: Place the homogeneous mixture in step 1 in a sealed container and evacuate the container; Step 3: introducing nitrogen-containing gas into the vacuumed sealed container and sealing the container; the nitrogen-containing gas is one or more of ammonia, nitric oxide, nitrogen dioxide, and nitrogen tetroxide; the volume of the nitrogen-containing gas introduced per gram of electrolyte precursor is 0.1-100 ml; Step 4: After heating the sealed container, sintering at a high temperature, and cooling it, sulfide electrolyte powder is obtained.

2. The use of a nitrogen-containing atmosphere sintered sulfide electrolyte powder material according to claim 1, characterized in that: The sintering temperature is 100-700°C and the sintering time is 0.1-25 h.

3. The use of a nitrogen-containing atmosphere sintered sulfide electrolyte powder material according to claim 1, characterized in that: The current collector is one of copper foil, aluminum foil, stainless steel foil and titanium foil.

4. A negative electrode-free solid-state lithium battery, characterized in that: Obtained by the application described in any one of claims 1 to 3.

Citation Information

Patent Citations

  • Method for preparing sulfide solid electrolyte with low cost and high efficiency

    CN114361579A

  • Electrolyte sheet with SSE surface modified by metal oxide and solid-state lithium battery without negative electrode

    CN115911524A

  • Negative-electrode-free lithium ion battery and preparation method thereof

    CN117219879A