A method for preparing carbon nanotube-coated type II anhydrous gypsum by microwave calcination
By growing carbon nanotubes in situ on the surface of Type II anhydrite and using microwave synthesis, the problem of slow early hydration and high energy consumption of Type II anhydrite in the existing high-temperature calcination method has been solved, and the material performance has been improved and The reduction of energy consumption expands its application scope.
Patent Information
- Application Number
- CN202410106980.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-25
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2044-01-25
AI Technical Summary
The existing high-temperature calcination preparation method results in slow early hydration of type II anhydrite, low strength and high energy consumption. The calcination time is long and uneven, resulting in unstable quality.
The microwave calcination preparation method of carbon nanotube-coated type II anhydrite is adopted. By growing carbon nanotubes in situ on the surface of dihydrate gypsum, microwave synthesis is used to simultaneously achieve the in-situ growth of carbon nanotubes and the high temperature of type II anhydrite. Calcining reduces energy consumption and improves the material's compressive strength, flexural strength, thermal conductivity, and electrical conductivity.
It significantly improves the early hydration activity and comprehensive performance of Type II anhydrite, reduces production and preparation energy consumption, broadens its application fields, and improves product quality and production efficiency.
Smart Images

Figure CN118063114B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of building materials, and in particular relates to a microwave calcination preparation method of carbon nanotube-coated type II anhydrous gypsum. Background Art
[0002] Type II anhydrous gypsum, also known as hard gypsum, is a new type of gypsum cementitious material. The main component is calcium sulfate. Compared with ordinary building gypsum, type II anhydrous gypsum has better water resistance and higher hardness. In construction, it is often used as a decorative material for floors, walls, and ceilings; type II anhydrous gypsum generates less heat during the curing process and takes a longer time to cure, and usually requires the help of an activator for activation. Type II anhydrous gypsum is generally prepared by calcining natural dihydrate gypsum or industrial by-product gypsum at a high temperature of 500 to 900°C. Due to the use of high-temperature calcination, harmful impurities such as soluble phosphorus, fluorine and organic matter in industrial by-product gypsum can be effectively removed, thereby improving the quality of gypsum cementitious materials.
[0003] At present, the existing high-temperature calcination preparation method has defects. First, the early hydration of type II anhydrous gypsum is slow, the strength is low, and the functionality is single; and when type II anhydrous gypsum is calcined in an industrial kiln, the calcination time is long and it is easy to be heated unevenly, resulting in high energy consumption and unstable quality. Therefore, how to improve the early hydration activity and comprehensive performance of type II anhydrous gypsum, reduce the energy consumption of production and preparation, and expand its application range is a difficult problem that needs to be solved in this field. Summary of the invention
[0004] The invention provides a method for preparing carbon nanotube-coated type II anhydrous gypsum by microwave calcination.
[0005] The technical solution adopted by the present invention is as follows:
[0006] S1: adding hydrochloric acid to the original dihydrate gypsum and stirring and dispersing it, adding the conductive polymer monomer and continuing to stir it, adding the initiator, and then separating, drying and washing to obtain the conductive polymer-coated dihydrate gypsum particles;
[0007] S2: mixing the conductive polymer-coated dihydrate gypsum particles with the metal organic complex powder to obtain a blend;
[0008] S3: calcining the blended material with microwave to obtain carbon nanotube-coated type II anhydrous gypsum.
[0009] Furthermore, the mass ratio of the dihydrate gypsum to hydrochloric acid is 1:10, the mass ratio of the conductive polymer monomer to the dihydrate gypsum is 1:1-1:2, the initiator is ammonium persulfate, and the mass ratio of ammonium persulfate to the dihydrate gypsum is 1:100-3:100.
[0010] Furthermore, in S1, a magnetic stirrer is used to stir for 2 to 5 minutes, stirring is continued for 5 to 10 minutes after the conductive polymer monomer is added, stirring is continued for 2 to 4 hours after the ammonium persulfate is added, and the drying time is 12 to 24 hours.
[0011] Furthermore, the mass ratio of the conductive polymer coated dihydrate gypsum particles to the metal organic complex powder in S2 is 1:0.5 to 1:1.
[0012] Furthermore, the power of the microwave calcination in S3 is 500-900 W, and the microwave time is 10-30 s.
[0013] Furthermore, the type II anhydrous gypsum is one of natural dihydrate gypsum, desulfurized gypsum, phosphogypsum, titanium gypsum, citric acid gypsum and industrial by-product dihydrate gypsum.
[0014] Furthermore, the conductive polymer monomer is one of polyacetylene, polythiophene and polypyrrole.
[0015] Furthermore, the metal organic complex powder is one of ferrocene and nickelocene.
[0016] A carbon nanotube-coated type II anhydrous gypsum, wherein the carbon nanotube-coated type II anhydrous gypsum is a crown structure, the surface protrusions are nano-scale carbon nanotubes grown in situ, and the internal granular parts are micron-scale type II anhydrous gypsum.
[0017] The invention discloses an application of carbon nanotube-coated type II anhydrous gypsum, wherein the carbon nanotube-coated type II anhydrous gypsum is applied to floor heating backfill self-leveling materials and electricity storage functional materials.
[0018] Beneficial Effects
[0019] (1) By in situ growing a layer of carbon nanotubes on the surface of type II anhydrous gypsum, carbon nanotubes can act as nucleating agents to promote the hydration reaction process of type II anhydrous gypsum. At the same time, carbon nanotubes can improve the compressive and flexural strength of the material. Finally, carbon nanotubes give type II anhydrous gypsum good thermal and electrical conductivity, broadening the application field of type II anhydrous gypsum.
[0020] (2) By synchronously coupling the microwave synthesis process of carbon nanotubes and the calcination process of type II anhydrous gypsum, high-temperature calcination of type II anhydrous gypsum and in-situ growth modification of carbon nanotubes were achieved. At the same time, the use of microwave synthesis significantly reduced the calcination energy consumption of type II anhydrous gypsum, which is very beneficial to improving product quality and production efficiency. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 This is a flow chart for preparing carbon nanotube-coated type II anhydrous gypsum according to Example 1 of the present invention.
[0022] Figure 2 This is a SEM image of carbon nanotube-coated type II anhydrous gypsum according to Example 1 of the present invention.
[0023] Figure 3 This is a TEM image of carbon nanotube-coated type II anhydrous gypsum according to Example 1 of the present invention. DETAILED DESCRIPTION
[0024] In combination with embodiments 1-4 and the attached Figure 1-3 Table 1 also provides a clear and complete description of the technical solution of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0025] Combination Figure 1 It can be seen that the preparation method of the present invention includes solution polymerization and freeze drying, high-speed mixing, and microwave calcination; the specific steps are as follows: first, dihydrate gypsum is added to hydrochloric acid for stirring and dispersion, then a conductive polymer monomer is added and continued to be stirred and adsorbed, and finally an ammonium persulfate initiator is added to polymerize the monomer and uniformly coat the surface of the dihydrate gypsum; then the conductive polymer-coated dihydrate gypsum is separated from the solution by vacuum filtration and washing, and then placed in a freeze dryer for drying to obtain uniformly dispersed conductive polymer-coated dihydrate gypsum particles; then the conductive polymer-coated dihydrate gypsum particles and metal organic complex powder are uniformly mixed in a high-speed stirrer to obtain a blend; the blend is placed in a household microwave oven and heated to obtain carbon nanotube-coated type II anhydrous gypsum.
[0026] By adopting the above technical solution, by mixing dihydrate gypsum and hydrochloric acid in a fixed ratio, impurities on the surface of dihydrate gypsum can be dissolved in hydrochloric acid, providing active sites for subsequent adsorption of conductive polymer monomers. The purpose of adding a fixed ratio of conductive polymer monomers and ammonium persulfate initiator is to grow a conductive polymer film in situ on the surface of dihydrate gypsum, thereby improving the efficiency and uniformity of subsequent microwave heating.
[0027] The conductive polymer coated dihydrate gypsum particles are separated from the solution by vacuum filtration, and the hydrochloric acid and acetone washing is to remove impurities and incompletely polymerized monomers in the solution. The purpose of freeze drying is to evenly disperse the conductive polymer coated dihydrate gypsum particles to avoid decomposition and agglomeration of the sample during drying. The conductive polymer coated dihydrate gypsum particles are mixed with metal organic complex powders by a high-speed mixer to evenly disperse and adsorb the metal organic complex powders on the surface of the dihydrate gypsum particles, which is conducive to the subsequent in-situ growth of carbon nanotubes.
[0028] The metal organic complex powder is ferrocene and nickelocene, which are decomposed at high temperature on the surface of dihydrate gypsum to produce nano-iron and nano-nickel, which can be used as a catalyst for the in-situ synthesis of carbon nanotubes. At the same time, they are decomposed to produce hydrocarbons, which can be used as an organic carbon source for the in-situ synthesis of carbon nanotubes. In addition, the decomposition temperature of ferrocene and nickelocene is above 400°C, which is consistent with the calcination temperature of type II anhydrous gypsum of 500-900°C. Therefore, the in-situ synthesis of carbon nanotubes and the high-temperature calcination of type II anhydrous gypsum can be achieved simultaneously. By controlling the microwave heating power at 500-900W and the heating time at 10-30s, the internal temperature of the blend can be kept at 500-900°C, thereby avoiding the failure to generate carbon nanotubes due to too low temperature, or the transformation of type II anhydrous gypsum into dead-burned type I floor gypsum due to too high temperature.
[0029] Example 1
[0030] S1: Stir and disperse the phosphogypsum and hydrochloric acid solution in a mass ratio of 1:10 evenly, put them in a magnetic stirrer and stir for 2 minutes to mix evenly; then add polypyrrole in a mass ratio of 0.8:1 to phosphogypsum, and continue stirring for 5 minutes; finally, add ammonium persulfate initiator in a mass ratio of 2:100 to phosphogypsum; stir for 3 hours until the solution polymerization is completed; then put the obtained solution into a vacuum filter for separation, and then wash it with hydrochloric acid and acetone solutions, and finally place it in a freeze dryer for 12 hours to obtain evenly dispersed polypyrrole-coated phosphogypsum particles;
[0031] S2: Mix the dried polypyrrole-coated phosphogypsum particles and nickelocene in a mass ratio of 1:0.8, and then place them in a high-speed mixer and mix them evenly;
[0032] S3: The high-speed mixed blend is placed in a corundum crucible, and then placed in a household microwave oven for microwave heating at 800W for 20s.
[0033] Example 2
[0034] S1: Stir and disperse titanium gypsum and hydrochloric acid solution in a mass ratio of 1:10 evenly, put them in a magnetic stirrer and stir for 3 minutes to mix evenly; then add polythiophene in a mass ratio of 0.6:1 to titanium gypsum, and continue stirring for 7 minutes; finally, add ammonium persulfate initiator in a mass ratio of 1:100 to titanium gypsum; stir for 2 hours until the solution polymerization is completed; then put the obtained solution into a vacuum filter for separation, and then wash it with hydrochloric acid and acetone solution, and finally place it in a freeze dryer for 16 hours to obtain uniformly dispersed polythiophene-coated titanium gypsum particles;
[0035] S2: Mix the dried polythiophene-coated titanium gypsum particles and nickelocene in a mass ratio of 1:0.5, and then place them in a high-speed mixer and mix them evenly;
[0036] S3: The high-speed mixed blend is placed in a corundum crucible, and then placed in a household microwave oven for microwave heating, the microwave oven is 800W, and the heating time is 15s.
[0037] Example 3
[0038] S1: Stir and disperse the citric acid gypsum and hydrochloric acid solution in a mass ratio of 1:10 evenly, put them in a magnetic stirrer and stir for 4 minutes to mix evenly; then add polypyrrole in a mass ratio of 1:2 to citric acid gypsum, and continue stirring for 8 minutes; finally, add ammonium persulfate initiator in a mass ratio of 3:100 to citric acid gypsum; stir for 3 hours until the solution polymerization is completed; put the obtained solution into a vacuum filter for separation, then wash it with hydrochloric acid and acetone solutions, and finally place it in a freeze dryer for 20 hours to obtain evenly dispersed polypyrrole-coated citric acid gypsum particles;
[0039] S2: Mix the dried polypyrrole-coated citric acid gypsum particles and ferrocene in a mass ratio of 1:1, and then place them in a high-speed mixer and mix them evenly;
[0040] S3: The high-speed mixed blend is placed in a corundum crucible, and then placed in a household microwave oven for microwave heating at 700W for 30s.
[0041] Example 4
[0042] S1: Stir and disperse the desulfurized gypsum and hydrochloric acid solution in a mass ratio of 1:10 evenly, put them in a magnetic stirrer and stir for 5 minutes to mix evenly; then add polyacetylene in a mass ratio of 0.9:1 to desulfurized gypsum, and continue stirring for 10 minutes; finally, add ammonium persulfate initiator in a mass ratio of 3:100 to desulfurized gypsum; stir for 4 hours until the solution polymerization is completed; put the obtained solution into a vacuum filter for separation, then wash it with hydrochloric acid and acetone solution, and finally place it in a freeze dryer for 24 hours to obtain evenly dispersed polyacetylene-coated desulfurized gypsum particles;
[0043] S2: Mix the dried polyacetylene-coated desulfurized gypsum particles and nickelocene in a mass ratio of 1:0.9, and then place them in a high-speed mixer and mix them evenly;
[0044] S3: The high-speed mixed blend is placed in a corundum crucible, and then placed in a household microwave oven for microwave heating at 900 W for 10 s.
[0045] Combination Figure 2 and Figure 3 As shown, Figure 2It shows the prepared carbon nanotube-coated type II anhydrous gypsum sample particles, which is the position circled, and the raised part of the surface is growing with curled rod-like substances, which is the direction indicated by the arrow; these substances are mainly carbon nanotubes grown in situ. Figure 3 It shows that the prepared carbon nanotube-coated type II anhydrous gypsum sample presents a crown structure. The protruding parts on the surface are nanoscale carbon nanotubes grown in situ, and the internal granular parts are micron-scale type II anhydrous gypsum. This also verifies the SEM test results. The crown-structured carbon nanotubes promote the crystallization nucleation effect on the surface of the type II anhydrous gypsum sample and accelerate the early hydration. At the same time, they are distributed among the hydration products in the later stage, strengthen and toughen the hydration products, and improve the compressive and flexural strength of the samples.
[0046] 100 parts of carbon nanotube-coated type II anhydrous gypsum samples, 3 parts of potassium sulfate and 5 parts of CaO powder were mixed evenly, and then 42 parts of water were added to adjust the slurry fluidity to 180 mm. After casting and natural curing for 1d and 28d, the type II anhydrous gypsum without carbon nanotube coating was used as the reference group, and the compressive strength, flexural strength, thermal conductivity and resistivity of the samples were tested respectively. The data results are shown in Table 1. Compared with pure type II anhydrous gypsum, the 1d and 28d compressive strengths of type II anhydrous gypsum modified by carbon nanotubes coating are increased by 3.12 times and 1.86 times respectively, the flexural strength is increased by 3.84 and 2.15 times respectively, the thermal conductivity is increased by 2.34 times, and the resistivity is decreased by about 4 orders of magnitude. The above results show that in situ grown carbon nanotubes can significantly improve the strength, toughness, thermal conductivity and electrical conductivity of type II anhydrous gypsum, and at the same time can improve the hydration rate of type II anhydrous gypsum, especially the improvement of early 1d strength and toughness.
[0047] Table 1 is the test results of physical and mechanical properties of carbon nanotube-coated type II anhydrous gypsum
[0048]
[0049] The preparation method used in the present invention grows a layer of carbon nanotubes in situ on the surface of type II anhydrous gypsum, so that the carbon nanotubes can be used as a crystal nucleating agent to promote the hydration reaction process of type II anhydrous gypsum, and the carbon nanotubes can also improve the compressive and flexural strength of the material. Finally, the carbon nanotubes give the type II anhydrous gypsum good thermal and electrical conductivity, and expand the application field of type II anhydrous gypsum. And through the synchronous coupling of the microwave synthesis process of the carbon nanotubes and the calcination process of the type II anhydrous gypsum, the high-temperature calcination of the type II anhydrous gypsum and the in-situ growth modification of the carbon nanotubes are achieved, and the microwave synthesis also significantly reduces the calcination energy consumption of the type II anhydrous gypsum, which is very beneficial to improving product quality and production efficiency.
Claims
1. A method for preparing carbon nanotube-coated type II anhydrous gypsum by microwave calcination, characterized in that: The steps are as follows: S1: adding hydrochloric acid to the original dihydrate gypsum and stirring and dispersing it, adding the conductive polymer monomer and continuing to stir it, adding the initiator, and then separating, drying and washing to obtain the conductive polymer-coated dihydrate gypsum particles; S2: mixing the conductive polymer-coated dihydrate gypsum particles with the metal organic complex powder to obtain a blend; S3: calcining the blended material with microwave to obtain carbon nanotube-coated type II anhydrous gypsum; The conductive polymer in S1 is one of polyacetylene, polythiophene and polypyrrole; The metal organic complex powder in S2 is one of ferrocene and nickelocene; The power of the microwave calcination in S3 is 500-900W, and the microwave time is 10-30s.
2. The microwave calcination preparation method of carbon nanotube-coated type II anhydrous gypsum according to claim 1, characterized in that: The mass ratio of the dihydrate gypsum to hydrochloric acid is 1:10, the mass ratio of the conductive polymer monomer to the dihydrate gypsum is 1:1-1:2, the initiator is ammonium persulfate, and the mass ratio of ammonium persulfate to the dihydrate gypsum is 1:100-3:
100.
3. The microwave calcination preparation method of carbon nanotube-coated type II anhydrous gypsum according to claim 1, characterized in that: In the S1, magnetic stirring is used for 2 to 5 minutes, stirring is continued for 5 to 10 minutes after adding the conductive polymer monomer, and stirring is continued for 2 to 4 hours after adding ammonium persulfate; the drying time is 12 to 24 hours.
4. The microwave calcination preparation method of carbon nanotube-coated type II anhydrous gypsum according to claim 1, characterized in that: The mass ratio of the conductive polymer-coated dihydrate gypsum particles to the metal organic complex powder in S2 is 1:0.5 to 1:
1.
5. A carbon nanotube-coated type II anhydrous gypsum obtained by the preparation method according to any one of claims 1 to 4, characterized in that: The carbon nanotube-coated type II anhydrous gypsum is a crown-shaped structure, the raised portion on the surface is the nano-scale carbon nanotube grown in situ, and the granular portion inside is the micron-scale type II anhydrous gypsum.
6. The use of carbon nanotube-coated type II anhydrous gypsum as claimed in claim 5, characterized in that: The carbon nanotube-coated type II anhydrous gypsum is applied to floor heating backfill self-leveling materials and electricity storage functional materials.
Citation Information
Patent Citations
Method for processing non-autoclaved foam concrete building blocks in producing phosphogypsum through microwave high temperature
CN102218766A
Method for inserting carbon nanofillers into an inorganic curable system
CN103328407A
Preparation method for carbon nanometer pipe
CN106495130A
Ardealite pretreatment method and application thereof
CN111499237A
Cement-based material of conductive heating concrete and preparation method of cement-based material
CN114315297A
Cited By
Method for synchronously preparing type II anhydrite in semi-hydrated-dihydrated wet-process phosphoric acid process and type II anhydrite