Production methods of low-temperature steel plates for ship storage

By coating the surface of steel billets with a specific coating and combining it with high-pressure water descaling technology during the production of low-temperature steel plates, the problem of surface quality defects caused by oxide scale has been solved, the low-temperature toughness and mechanical properties have been improved, and the efficient production of high-quality low-temperature steel plates has been achieved.

CN118064691BActive Publication Date: 2026-11-17INST OF RES OF IRON & STEEL JIANGSU PROVINCE +1
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202410263792.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-08
Publication Date
2026-11-17
Estimated Expiration
2044-03-08

AI Technical Summary

Technical Problem

In the production of low-temperature steel plates, the oxide scale on the surface of the billet leads to surface quality defects, affects low-temperature toughness and mechanical properties, and increases production costs.

Method used

Before heating, a coating with specific components is applied to the surface of the steel billet, and high-pressure water descaling technology is used to prevent the formation of oxide scale. At the same time, the surface quality and low-temperature toughness of the steel plate are improved by optimizing the heating, rolling and heat treatment processes.

Benefits of technology

It effectively prevents the formation of oxide scale, improves the surface quality and low-temperature toughness of steel plates, reduces production costs, increases production efficiency, and meets the performance requirements of low-temperature steel plates used in ship storage.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004731855400000141
    Figure BDA0004731855400000141
  • Figure BDA0004731855400000142
    Figure BDA0004731855400000142
  • Figure BDA0004731855400000161
    Figure BDA0004731855400000161
Patent Text Reader

Abstract

This invention discloses a method for producing low-temperature steel plates for ship storage. The thickness H of the steel plate is 8-50 mm. The production method includes: refining molten steel and casting it into steel billets; applying a coating to the ground surface; heating to a soaking temperature of 1160-1200℃; after exiting the heating furnace, high-pressure water descaling is performed before the first and third rolling passes; the initial rolling temperature is 1050-1100℃; and when H < 12 mm, the final rolling temperature T... fr +100~120℃, final rolling temperature T when 12mm≤H fr ±20℃; after cooling, heat treatment is performed, including tempering, with a tempering temperature of Ac1-50~80℃ and a holding time of [(2.0~3.0)H]min / mm and more than 30min, to obtain the finished steel plate. This invention comprehensively improves surface quality and low-temperature performance, and also increases production efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of steel materials technology, and relates to a method for producing low-temperature steel plates, especially a method for producing low-temperature steel plates for ship storage. Background Technology

[0002] For clean energy sources and chemical raw materials such as liquefied petroleum gas (LPG), liquefied ethane (LEC), and liquefied ethylene gas (LEG), cryogenic steel plates are required as the basic material for storage and transportation containers during long-distance ocean transport and storage. Because they operate in low-temperature environments, such as -110℃ to -135℃, cryogenic steel plates need to possess excellent mechanical properties at room temperature as well as excellent low-temperature toughness. In terms of composition, cryogenic steel plates require low levels of impurities such as phosphorus (P), sulfur (S), and nitrogen (N), and a high nickel content.

[0003] However, during the production process, when low-temperature steel billets are heated to high temperatures in a furnace, the surface of the billets comes into contact with oxygen in the environment, forming oxide scale. Once this oxide scale enters the subsequent rolling process, it will be pressed deep into the steel, causing surface defects in the final steel product. Furthermore, the formation of oxide scale also leads to increased steel microstructure loss and adds the processing steps required to remove the oxide scale, seriously affecting the economic efficiency of steel production.

[0004] In conclusion, improving surface quality and low-temperature toughness is a problem that needs to be solved in the production of low-temperature steel plates. Summary of the Invention

[0005] In order to solve the problems of improving the surface quality and low-temperature toughness of steel billets, the present invention aims to provide a method for producing low-temperature steel plates, especially a method for producing low-temperature steel plates for ship storage.

[0006] To achieve the above-mentioned objective, one embodiment of the present invention provides a method for producing low-temperature steel plates for ship storage. The finished thickness H of the steel plate is 8-50 mm, and the production method includes:

[0007] The steel is smelted and cast into billets with a thickness of 220-250 mm. The chemical composition of the billets, by mass percentage, includes: C: 0.05-0.07%, Si: 0.15-0.25%, Mn: 0.5-0.7%, P≤0.008%, S≤0.003%, Cr≤0.05%, Ni: 4.85-5.3%, Cu≤0.015%, Nb≤0.002%, Ti≤0.002%, Alt: 0.02-0.05%, N≤0.004%, with the balance being iron and unavoidable impurities.

[0008] The steel billet is heated in a heating furnace at a soaking temperature of 1160–1200℃; the steel billet is ground before entering the heating furnace, and then a coating is applied to the ground surface.

[0009] After exiting the heating furnace, the rolling mill is kept free of roller table water between the heating furnace and the rough descaling machine for hot rolling. High-pressure water descaling is performed before the first and third rolling passes, with a descaling water pressure ≥22MPa. The initial rolling temperature is 1050–1100℃, and the final rolling temperature is adjusted according to the finished product thickness H. When 8mm ≤ H < 12mm, the final rolling temperature T is [not specified]. fr The final rolling temperature T is +100~120℃, when 12mm≤H≤50mm. fr ±20℃; among which,

[0010] T fr =902-98C+47Si-10Mn-9.7Ni+95Cr-24Cu-115Ti+223Nb-202Al, where the element symbols in this formula represent 100 times the mass percentage of each element in the steel billet;

[0011] After the hot-rolled steel sheet is cooled, it undergoes heat treatment to obtain the finished steel sheet; the heat treatment includes tempering, with a tempering temperature of Ac1-50~80℃, Ac1=T fc The tempering holding time is [(2.0~3.0)H]min / mm and more than 30min, at -200~220℃.

[0012] T fc =784+117C+28Si-10Mn+11Ni-126Cr-34Cu-131Ti+357Nb-173Al, where the element symbols represent 100 times the mass percentage of each element in the billet.

[0013] Preferably, when 8mm≤H<12mm, the production method further includes, before the “surface grinding” step in the “the billet is heated in a heating furnace at a soaking temperature of 1160~1200℃; the billet is surface ground before entering the heating furnace, and then a coating is applied to the ground surface” step: the cast billet is surface ground, then a coating is applied to the ground surface, and then it is put into a heating furnace for heating at a soaking temperature of 1200~1240℃, and then it is cut into billets with a thickness of 80~120mm.

[0014] Preferably, when H≥12mm, the "hot rolling" is a two-stage rolling process, with the total reduction in the first stage being 53-79%; and the starting temperature of the second stage rolling after warming is 820-860℃, corresponding to the finished steel plate of 40mm<H≤50mm, or 890-940℃, corresponding to the finished steel plate of 12mm≤H≤40mm.

[0015] Preferably, in the phrase "after the hot-rolled steel plate has cooled":

[0016] When 12mm≤H≤40mm, air cooling is used; otherwise, water cooling is used with an accelerated cooling control system, and the final cooling temperature is ≤200℃ and the reddening temperature is ≤300℃.

[0017] Preferably, if H < 12 mm, the inlet water temperature T is controlled in the accelerated cooling control system. fc +90~115℃, cooling rate (25+1.5H / mm)±1.5℃ / s; if H>40mm, control the inlet water temperature T in the accelerated cooling control system. fc ±10℃, cooling rate (25+0.5H / mm)±1.5℃ / s.

[0018] Preferably, when H ≥ 12 mm, the heat treatment further includes quenching before tempering, with a quenching holding time of [(2.0~3.0)H] min / mm and a quenching temperature of Ac3 + 30~50℃ corresponding to finished steel plates with a diameter of 40 mm < H ≤ 50 mm, or Ac3 - 50~90℃ corresponding to finished steel plates with a diameter of 12 mm ≤ H ≤ 40 mm, wherein Ac3 = T fr -60~90℃.

[0019] Preferably, the coating is prepared from 60-70 parts by weight of SiO2, 15-20 parts by weight of Al2O3, 0.5-1.5 parts by weight of ZrO2, 1-3 parts by weight of SiC, 1-2 parts by weight of B4C, 4.5-22 parts by weight of binder and solvent.

[0020] Preferably, the coating also satisfies the following composition by weight: ZrO2 + (0.10 ~ 0.20) = (SiC / 2) 0.5 SiO2 / Al2O3 = (2.5~4.5) and SiC+B4C = 2.5~5.

[0021] Preferably, the coating is prepared from 30-60 parts by weight of SiO2, 3-20 parts by weight of Al2O3, 5-18 parts by weight of ZrO2, 1-12 parts by weight of SiC, 1-8 parts by weight of C, 1-3 parts by weight of B4C, 2-16 parts by weight of binder and solvent.

[0022] Preferably, the coating also satisfies the following by weight: Al2O3 = (0.1~0.4)SiO2, ZrO2 = (1~1.5)SiC and SiC+C+B4C = 3~23.

[0023] Preferably, when applying the coating:

[0024] A full coat is applied in multiple passes.

[0025] The time T after the steel billet is coated in the heating furnace is obtained. When T≤400min, the coating is stopped after one full spraying of the steel billet surface; when T>400min, the coating is stopped after n=ceil((t-400min) / 30min) full sprayings of the steel billet surface.

[0026] Each full-coverage spray coating is 0.2 to 0.3 mm thick.

[0027] Preferably, the chemical composition of the steel billet, by mass percentage, is: Mn = 2Si + 0.05~0.22%, Mn + Si: 0.65~0.95%.

[0028] Compared with existing technologies, the beneficial effects of this embodiment are as follows: Before heating the steel billet, a coating is applied to the surface of the billet to protect it. Combined with descaling control, this solves the problem of surface quality defects in the finished steel plate caused by high-temperature oxide scale on the billet. It avoids compromising mechanical properties and low-temperature toughness by prioritizing surface quality. Furthermore, through comprehensive design of heating, rolling, and heat treatment, the mechanical properties and low-temperature toughness of the final steel plate are improved, resulting in a comprehensive improvement in surface quality and low-temperature performance. This increases production efficiency while ensuring stable and excellent product performance, and the resulting product meets the quality requirements for low-temperature steel plates used in ship storage. Detailed Implementation

[0029] The following detailed embodiments will further illustrate the technical solution of the present invention.

[0030] One embodiment of the present invention provides a method for producing steel plates, which is particularly suitable for the preparation of low-temperature steel plates with a thickness H of 8-50 mm used in ship storage. The production method includes processes such as billet casting, pre-hot rolling treatment, hot rolling, cooling, and heat treatment. Each process is described in detail below.

[0031] casting process

[0032] In this process, molten steel is refined according to a predetermined chemical composition and poured into steel billets with a thickness of 220-250 mm.

[0033] The predetermined chemical composition is the chemical composition that the obtained steel billet needs to meet, and it is also the chemical composition that the final steel plate product needs to meet.

[0034] In one embodiment, the predetermined chemical composition comprises, by mass percentage: C: 0.05–0.07%, Si: 0.15–0.25%, Mn: 0.5–0.7%, P ≤ 0.008%, S ≤ 0.003%, Cr ≤ 0.05%, Ni: 4.85–5.3%, Cu ≤ 0.015%, Nb ≤ 0.002%, Ti ≤ 0.002%, Alt: 0.02–0.05%, N ≤ 0.004%, with the balance being iron and unavoidable impurities.

[0035] The following explains the role and dosage of each chemical component in the low-temperature steel billet described in this embodiment.

[0036] Carbon (C) is a strengthening element and also a stabilizing element for austenite. If the C content is too low, the strength of the steel plate is difficult to guarantee; if the C content is too high, it will increase the ductile-brittle transition temperature and affect the low-temperature toughness of the steel plate. Therefore, while ensuring strength, the C content should be as low as possible. In this invention, the C content is controlled between 0.05% and 0.07%.

[0037] Si is a deoxidizing element and can also inhibit the grain boundary segregation of P. However, a high Si content affects the low-temperature toughness of the steel plate. In this invention, the Si content is controlled at 0.15-0.25% to ensure the deoxidation effect and reduce oxide inclusions in the steel without affecting the low-temperature toughness.

[0038] Mn is a solid solution strengthening and grain refinement element, as well as an austenite stabilizing element. Adding Mn can significantly improve the hardenability of materials. However, it is also an element that easily segregates and forms inclusions; excessive addition can affect the fracture toughness and low-temperature impact toughness of steel plates. In this invention, the Mn content is controlled at 0.5% to 0.7%.

[0039] Ni (Ni): It can improve the hardenability of steel plates and is an effective element for improving fracture toughness and low-temperature toughness. However, the alloy cost is relatively high, and it is prone to forming a sticky iron oxide scale on the surface at high temperatures, which is difficult to remove. In this invention, the Ni content is 4.85%–5.3%.

[0040] Al: is a deoxidizing element. Excessive aluminum can increase the Al2O3 inclusions in steel, affecting the low-temperature toughness of the steel. In this invention, Al is controlled at 0.02-0.05%.

[0041] Cr, Cu, Nb, and Ti: These are derived from scrap steel added during smelting and are non-additive elements. Their content should be controlled to meet the following requirements: Cr ≤ 0.05%, Cu ≤ 0.015%, Nb ≤ 0.002%, and Ti ≤ 0.002%.

[0042] P, S, N: Impurity elements, which should be controlled within a low range as much as possible. In this invention, P ≤ 0.008%, S ≤ 0.003%, and N ≤ 0.005%.

[0043] More preferably, the chemical composition of the steel billet, by mass percentage, is: Mn = 2Si + 0.05~0.22%, Mn + Si: 0.65~0.95%.

[0044] Furthermore, the "steel refining" process in this step can be implemented using any feasible technology in the field. For example, in one embodiment, molten steel is refined by a process of molten iron pretreatment-converter smelting-LF refining-RH refining, and then cast into steel billets using continuous casting technology.

[0045] Hot rolling pretreatment process

[0046] In one embodiment, the steel billet is subjected to a series of processes including grinding, coating, and heating before proceeding to the next process, the hot rolling process.

[0047] Specifically, in the grinding process, the steel billet undergoes surface grinding to ensure a clean surface. Preferably, the grinding depth is 3mm to ensure that the coating in the subsequent coating process can be well adhered to the substrate of the steel billet.

[0048] In the coating process, a coating is applied to the surface of the ground steel billet. The coating is a suspension that can be applied to the surface of the steel billet to protect it, thereby preventing the oxide scale generated during the subsequent high-temperature heating of the billet in the furnace from adversely affecting the final steel plate product, improving surface quality, and reducing production costs caused by oxide scale removal.

[0049] In a first preferred embodiment of the coating, the coating is prepared from 60 to 70 parts by weight of SiO2, 15 to 20 parts by weight of Al2O3, 0.5 to 1.5 parts by weight of ZrO2, 1 to 3 parts by weight of SiC, 1 to 2 parts by weight of B4C, 4.5 to 22 parts by weight of binder and solvent.

[0050] The following explains the function and content of each component of the coating:

[0051] SiO2: The main substance providing melt shielding in the coating formed by the coating; hard, which can improve the strength of the coating at room temperature on the surface of the steel billet; high melting point, which is the key to the high temperature resistance of the coating; moderate viscosity, which is the main component of the viscous dense film layer at high temperature; low coefficient of linear expansion, which provides the coating with self-detachment; in this embodiment, SiO2 accounts for 60 to 70 parts by weight in the remaining components except for the solvent;

[0052] Al2O3 has good chemical stability and a high melting point, which can increase the high-temperature softening temperature of the coating. At high temperatures, it can combine with SiO2 to form ceramic mullite, which fills the cracks and voids in the coating during the film formation process, making the coating more dense. In this embodiment, Al2O3 accounts for 15 to 20 parts by weight in the components other than the solvent.

[0053] ZrO2: It has a high melting point and will transform from a monoclinic crystal system to a tetragonal crystal system at high temperatures, causing the coating formed by the coating material to expand in volume; it has poor thermal conductivity, which causes huge stress between the coating formed by the coating material and the steel billet substrate after the steel billet leaves the heating furnace, and it is easy to fall off during the high-pressure water descaling process; In this embodiment, ZrO2 accounts for 0.5 to 1.5 parts by weight of the components other than the solvent.

[0054] SiC: The coating formed by the coating provides the main redox properties; during the heating process, it reacts with oxygen before Fe to generate SiO2 and C, which can effectively prevent the surface oxidation of the steel billet; the product SiO2 is an effective component that provides the shielding properties of the melt film; the product C, as a reducing substance, can also prevent the oxidation of the steel billet; in this embodiment, SiC accounts for 1 to 3 parts by weight in the remaining components except for the solvent.

[0055] B4C: The coating formed by the coating provides a substance with redox and intermelting reactivity; at temperatures above 600°C, it reacts with oxygen to generate B2O3, which can effectively dissolve the iron oxide scale generated on the surface of the slab; in this embodiment, B4C accounts for 1 to 2 parts by weight of the components other than the solvent.

[0056] Binder: It is easily soluble in solvent and can be used as a dispersant when a solvent is used to prepare a suspension of coating. It can bond with the metal matrix at room temperature. It can also assist in film formation during the heating process of steel billet. In this embodiment, the binder accounts for 4.5 to 22 parts by weight of the components other than the solvent, and the weight of the solvent is 7.4 to 12 times the weight of the binder.

[0057] The coating described in this embodiment uses the aforementioned chemical composition and content. Compared with existing coatings, it can significantly improve the high-temperature oxidation protection effect on steel billets, greatly reduce the probability of oxide scale formation during the heating process, thereby reducing surface defects in finished steel products caused by oxide scale, and reducing the production difficulty and cost caused by oxide scale removal. Furthermore, the coating is safe in composition, has no risk of secondary pollution, is low in cost, and is easy to prepare. In summary, this low-cost, easy-to-prepare, and highly safe coating improves the surface quality of finished steel products, reduces production costs and difficulty, and has significant comprehensive economic and environmental benefits.

[0058] The binder may be K2SiO3 or Na5P3O 10 K2SiO3 is preferred. K2SiO3 is readily soluble in water and can form stable hydrates. It can be used as a high-quality dispersant when preparing suspension-like coatings. It can bond firmly with the steel billet matrix at room temperature. Furthermore, K2SiO3 has a low melting point and good fluidity. As a low-melting-point component during the heating process of the steel billet, it can quickly fill the loose and porous structure formed during the coating film formation process, and encapsulate the surrounding powder to form a molten glass film.

[0059] The weight of the flux is 7.4 to 12 times the weight of the binder.

[0060] Preferably, the solvent is water, which is abundant, inexpensive, easy to obtain, and safe.

[0061] Furthermore, the coating contains no other components besides SiO2, Al2O3, ZrO2, SiC, B4C, binder, and solvent.

[0062] More preferably, the coating also satisfies the following condition by weight: ZrO2 + (0.10 ~ 0.20) = (SiC / 2) 0.5 The SiO2 / Al2O3 ratio is (2.5–4.5) and the SiC+B4C ratio is 2.5–5. Thus, when these components satisfy the relevant relationships, the high-temperature oxidation protection effect on the steel billet can be further improved, and the probability of oxide scale formation during the heating process can be significantly reduced.

[0063] In this embodiment, the preparation process of the coating is as follows: the powders of each component of component A are dried and dehydrated at a temperature of 80-100°C for 30-45 minutes; each component is weighed according to the target weight parts and ball-milled to obtain powder; the sieved powder is added to a solvent and stirred at a speed of 100-150 r / min for 15-25 minutes, and then allowed to stand for 15-30 minutes to obtain the coating.

[0064] The "target weight parts" refers to the weight parts of each component in the coating as described above. Furthermore, ball milling grinds each component to a particle size below 250 mesh, resulting in a powder with a particle size below 250 mesh. After ball milling, the powder can be sieved through a 250-mesh sieve to obtain the final powder.

[0065] In addition, 5mm SiC grinding balls are used in the ball mill, the ball-to-powder ratio (i.e., the mass ratio of grinding balls to powder) is 3:1, the ball mill speed is 150r / min and the running time is 1.5h.

[0066] In a second preferred embodiment of the coating, the coating is prepared from 30 to 60 parts by weight of SiO2, 3 to 20 parts by weight of Al2O3, 5 to 18 parts by weight of ZrO2, 1 to 12 parts by weight of SiC, 1 to 8 parts by weight of C, 1 to 3 parts by weight of B4C, 2 to 16 parts by weight of binder and solvent.

[0067] The following explains the function and content of each component of the coating:

[0068] SiO2: The main substance providing melt shielding in the coating formed by the coating; hard, which can improve the strength of the coating at room temperature on the surface of the steel billet; high melting point, which is the key to the high temperature resistance of the coating; moderate viscosity, which is the main component of the viscous dense film layer at high temperature; low coefficient of linear expansion, which provides the coating with self-detachment; in this embodiment, SiO2 accounts for 30 to 60 parts by weight in the total components except for the solvent;

[0069] Al2O3 has good chemical stability and a high melting point, which can increase the high-temperature softening temperature of the coating. At high temperatures, it can combine with SiO2 to form ceramic mullite, which fills the cracks and voids in the coating during the film formation process, making the coating more dense. In this embodiment, Al2O3 accounts for 3 to 20 parts by weight in the total components except for the solvent.

[0070] ZrO2: It has a high melting point and will transform from a monoclinic crystal system to a tetragonal crystal system at high temperatures, causing the coating formed by the coating material to expand in volume; it has poor thermal conductivity, which causes huge stress between the coating formed by the coating material and the steel billet substrate after the steel billet leaves the heating furnace, and it is easy to fall off during the high-pressure water descaling process; in this embodiment, ZrO2 accounts for 5 to 18 parts by weight of the total components except for the solvent.

[0071] SiC: The coating formed by the coating provides the main redox properties; during the heating process, it reacts with oxygen before Fe to generate SiO2 and C, which can effectively prevent the surface oxidation of the steel billet; the product SiO2 is an effective component that provides the shielding properties of the melt film; the product C, as a reducing substance, can also prevent the oxidation of the steel billet; in this embodiment, SiC accounts for 1 to 12 parts by weight in the total components except for the solvent.

[0072] C: Provides redox properties to the coating and alleviates decarburization on the surface of the steel billet; in this embodiment, C accounts for 1 to 8 parts by weight of the total components except for the solvent.

[0073] B4C: The coating formed by the coating provides redox and intermetallic reactivity; at temperatures above 600°C, it reacts with oxygen to generate B2O3, which can effectively dissolve the iron oxide scale generated on the surface of the slab; in this embodiment, B4C accounts for 1 to 3 parts by weight of the total components except the solvent.

[0074] Binder: It is easily soluble in solvents and can be used as a dispersant when solvents are used to prepare suspension-like coatings. It can bond with the metal matrix at room temperature. It can also assist in film formation during the heating process of steel billets. In this embodiment, the binder accounts for 2 to 16 parts by weight of the total components other than the solvent.

[0075] The coating described in this embodiment uses the above-mentioned chemical composition and content. Compared with the coatings of the prior art, it can greatly improve the high-temperature anti-oxidation protection effect on steel billets and greatly reduce the probability of oxide scale formation during the heating process of steel billets. Compared with the coating of the first preferred embodiment, the coating of this embodiment can reduce the stickiness of the oxide scale generated by the steel billet due to high-temperature heating, making the oxide scale easier to remove in the subsequent descaling process, i.e., the removal rate is high. As a result, it reduces the surface defects of finished steel products caused by oxide scale on steel billets, reduces the cost of oxide scale removal of steel products, and has great comprehensive economic and environmental benefits.

[0076] The binder may be K2SiO3 or Na5P3O 10 Na5P3O is preferred. 10 Na5P3O 10 It is readily soluble in water and can form stable hydrates. It serves as an excellent dispersant when preparing suspensions of coatings and can bond firmly to the steel billet matrix at room temperature. Furthermore, Na5P3O 10 With a low melting point and good fluidity, it can be used as a low-melting-point component during the heating process of steel billets. It can quickly fill the loose and porous structure formed during the coating film formation process, and wrap the surrounding powder to form a molten glass film.

[0077] In this embodiment, the weight of the flux is 0.25 to 0.4 times the weight of the remaining components of the coating (i.e., the sum of SiO2, Al2O3, ZrO2, SiC, C, B4C and binder).

[0078] Preferably, the solvent is water, which is abundant, inexpensive, easy to obtain, and safe.

[0079] More preferably, the coating, by weight, also satisfies: Al2O3 = (0.1–0.4)SiO2, ZrO2 = (1–1.5)SiC, and SiC + C + B4C = 3–23. Thus, with these components satisfying the relevant relationships, the removal efficiency of oxide scale generated on steel billets during descaling can be further improved.

[0080] In this embodiment, the preparation process of the coating is as follows: weigh each component according to the target weight parts, mix the powders other than SiC and B4C and put them into a ball mill container made of SiC material for ball milling; after ball milling is completed, mix SiC and B4C with the ball milled powder, and then add solvent; stir at a speed of 200-500 r / min for 30-60 min to obtain a mixture with a viscosity of 3-15 mPa.s, and then let it stand for 30 min to obtain the coating.

[0081] Preferably, the particle size of the powder obtained from ball milling is between 200 and 400 mesh.

[0082] During the ball milling process, SiC grinding balls are used, with a ball-to-powder ratio (mass ratio of grinding balls to powder) of 3.5:1 to 5:1. The ball mill speed is (0.2 to 1.3)R r / s / mm, and the running time is 2 to 4 hours. Furthermore, when the maximum particle diameter R of the original powder is greater than 15mm, 20mm large grinding balls and 5mm medium grinding balls are used, with a mass ratio of 4.5:1 to 6:1; when the maximum particle diameter R of the original powder is between 5 and 15mm, 5mm medium grinding balls and 3mm small grinding balls are used, with a mass ratio of 2:1 to 4:1; when the maximum particle diameter R of the original powder is less than 5mm, 3mm small grinding balls are used, with a mass ratio of 4.5:1 to 6:1.

[0083] Furthermore, the coating process specifically includes:

[0084] A full coating is achieved through multiple passes. For the surface of the steel billet, multiple coats are required to ensure that the entire surface is covered with paint, thus completing a full coating. The thickness of the paint in each full coating is 0.2 to 0.3 mm.

[0085] The time T after the steel billet is coated in the heating furnace is obtained. When T≤400min, the coating is stopped after one full spraying of the steel billet surface; when T>400min, the coating is stopped after n=ceil((t-400min) / 30min) full sprayings of the steel billet surface.

[0086] Where ceil(x) represents the floor function of x, that is, the smallest integer not less than x. For example, when x takes the value 1.2, then ceil(x) takes the value 2. More specifically, when t = 440 min, (t-400 min) / 30 min = 1.33, then n = ceil(1.33) = 2. Accordingly, the coating is completed after two full sprayings on the surface of the steel billet.

[0087] Thus, by adjusting the number of full-scale sprayings based on the time T the steel billet spends in the heating furnace after coating, the thickness and quality of the coating on the surface of the steel billet can be guaranteed, which can further greatly improve the surface protection effect of the steel billet.

[0088] Furthermore, when T > 400 min, the time interval between any two full-coverage sprays should not be less than 15 min. This ensures that the coating formed by each full-coverage spray has good density, thereby improving the density of the final complete coating.

[0089] In the heating process, the coated steel billet obtained in the previous coating process is heated in a heating furnace at a temperature of 1160-1200°C in the soaking zone, in preparation for subsequent rolling, which in this embodiment is the subsequent <hot rolling process>; while in another embodiment, the number of times the full coating is applied in the previous coating process is adjusted according to the furnace time T in the heating process.

[0090] As mentioned earlier, the finished thickness H of the steel plate is 8–50 mm. Among them, when the finished thickness H of the steel plate is ≥12 mm, the soaking temperature is 1170–1200℃, and the furnace time T is 380–420 min.

[0091] However, when the thickness H of the finished steel plate is less than 12 mm, in addition to the above-described process of grinding, coating, and heating the steel billet, a more preferred embodiment may include an additional billet-opening process. Specifically, before the aforementioned grinding process, an additional process of first grinding, first coating, first heating, and billet-opening is added. That is, for a finished product thickness H ≥ 12 mm, the complete preparation process for the finished steel plate is steelmaking - continuous casting - grinding - coating - heating - hot rolling - cooling - heat treatment; while for a finished product thickness < 12 mm, the complete preparation process for the finished steel plate is steelmaking - continuous casting - first grinding - first coating - first heating - billet-grinding - coating - heating - hot rolling - cooling - heat treatment.

[0092] Specifically, for finished product thickness <12mm: the first grinding process is the same as the grinding process, and the first coating process is basically the same as the coating process; in the first heating process, the temperature of the soaking zone is 1200-1240℃, and the furnace time T1 of the first heating is 240-380min, while in the first coating process, the number of full-coverage sprayings is adjusted according to the furnace time T1 of the first heating; in the billet-making process, the steel billet obtained in the first coating process is rolled to a thickness of 80-120mm; in the heating process, the temperature of the soaking zone is 1160-1180℃, the soaking zone holding time is 60-80min, and the furnace time T is 80-120min, while in the coating process, the number of full-coverage sprayings is adjusted according to the furnace time T.

[0093] Hot rolling process

[0094] In this process, the steel billet that has left the heating furnace in the previous hot rolling pretreatment process is taken into the rolling mill for hot rolling in a state where there is no water in the roller table between the heating furnace and the rough descaling machine, and is rolled into a hot rolled steel plate with a thickness H of 8 to 50 mm.

[0095] High-pressure water descaling is performed before the first and third rolling passes, with a descaling water pressure ≥22MPa. Of course, intermittent fine descaling can also be performed depending on the oxide scale condition on the steel plate surface. For example, if necessary, high-pressure water descaling can also be performed before the fifth rolling pass.

[0096] In the specific hot rolling process, the initial rolling temperature is 1050~1100℃, and the final rolling temperature is adjusted according to the finished product thickness H. When 8mm≤H<12mm, the final rolling temperature T is... fr The final rolling temperature T is +100~120℃, when 12mm≤H≤50mm. fr ±20℃; among which,

[0097] T fr =902-98C+47Si-10Mn-9.7Ni+95Cr-24Cu-115Ti+223Nb-202Al, where the element symbols in this formula represent 100 times the mass percentage of each element in the steel billet.

[0098] Regarding the final rolling temperature when 12mm ≤ H ≤ 50mm, if H ≥ 40mm, the final rolling temperature T can be further optimized. fr ±10℃.

[0099] In a further preferred embodiment, when H < 12 mm, the rolling process adopts single-stage rolling, and in the first 5 passes, at least 3 passes have a reduction of more than 16 mm, and the single-pass reduction rate is 10-35%.

[0100] When H ≥ 12 mm, the rolling process adopts a two-stage rolling process. The first-pass reduction in the first stage is ≥ 15%, and the total reduction in the first stage is 53-79%. Furthermore: if H ≤ 40 mm, the preferred total reduction in the first stage is 55-79%, the initial thickness after heating is (3.5-4.0) H, the initial rolling temperature in the second stage after heating is 890-940℃, and the total reduction in the second stage is ≥ 52%. If H > 40 mm, the initial thickness after heating is (2.0-3.0) H, the initial rolling temperature in the second stage after heating is 820-860℃, and the total reduction in the second stage is ≥ 49%.

[0101] Cooling process

[0102] In this cooling process, the hot-rolled steel plate is cooled after exiting the rolling mill.

[0103] Preferably, air cooling is used when 12mm≤H≤40mm; otherwise, water cooling is used with an accelerated-cooling control system (ACC), and the final cooling temperature is ≤200℃ and the reddening temperature is ≤300℃.

[0104] For example, when H < 12 mm, an accelerated cooling control system is used for water cooling to control the inlet water temperature T. fc +90~115℃, cooling rate (25+1.5H / mm)±1.5℃ / s; when H>40mm, an accelerated cooling control system is used for water cooling, controlling the inlet water temperature T. fc ±10℃, cooling rate (25+0.5H / mm)±1.5℃ / s.

[0105] Where T fc =784+117C+28Si-10Mn+11Ni-126Cr-34Cu-131Ti+357Nb-173Al, where the element symbols represent 100 times the mass percentage of each element in the billet.

[0106] Heat treatment process

[0107] In this process, the steel plate after the cooling process is heat-treated to obtain the final steel plate product.

[0108] Of course, shot blasting can be performed before heat treatment, for example at a speed of 0.06 to 0.1 m / s.

[0109] Specific geothermal treatment includes tempering, with a tempering temperature of Ac1-50~80℃, where Ac1=T. fcThe tempering temperature is -200~220℃, and the holding time is [(2.0~3.0)H]min / mm and more than 30min. After tempering, the steel plate is air-cooled to obtain the finished product.

[0110] In the preferred embodiment, for steel plate products with H < 12mm, the heat treatment in this process only requires tempering, that is, the steel plate after shot blasting can be directly tempered; while for steel plate products with H ≥ 12mm, the heat treatment in this process can also include quenching, followed by tempering.

[0111] For example, when 12mm≤H≤40mm, the steel plate after shot blasting is first quenched at a temperature of Ac3+30~50℃, where Ac3=T fr The quenching temperature is -60~90℃, and the holding time is [(2.0~3.0)H]min / mm. After quenching, tempering is performed. When H>40mm, the steel plate after shot blasting is first quenched at a temperature Ac3-50~90℃, where Ac3=T fr The quenching temperature is -60~90℃, and the holding time is [(2.0~3.0)H]min / mm. This process can also be called sub-temperature quenching, followed by tempering.

[0112] The preferred embodiments of the present invention have been described above. In the basic embodiment, the steel plate production method, compared with the prior art, involves applying a coating to the surface of the steel billet before heating it to protect the surface. Combined with descaling control, this solves the problem of surface quality defects in the finished steel plate caused by high-temperature oxide scale on the billet. It avoids compromising mechanical properties and low-temperature toughness by prioritizing surface quality. Furthermore, through comprehensive design of heating, rolling, and heat treatment, the mechanical properties and low-temperature toughness of the final steel plate are improved, resulting in a comprehensive improvement in surface quality and low-temperature performance. This improves production efficiency while ensuring stable and excellent product performance, and the resulting product meets the quality requirements for low-temperature steel plates used in ship storage.

[0113] The low-temperature steel plate produced by the production method described in this embodiment has a tensile strength of 600-710 MPa, a yield strength of 400-590 MPa, an elongation of ≥25%, an impact strength of ≥230 J at -135℃, and excellent surface quality.

[0114] The above describes a method for producing steel plates according to one embodiment. Several specific embodiments are provided below.

[0115] First, steel billets with a thickness of 220 mm were obtained by following the process of hot metal pretreatment-converter smelting-LF refining-RH refining-continuous casting. The chemical composition of each steel billet is shown in Table 1.

[0116] [Table 1]

[0117]

[0118] Six steel billets from Example A1 were taken and ground. Five of the billets were coated with paint according to the coating process described above, while the remaining billet was left uncoated, resulting in Examples B1 to B5 and Comparative Example B6 as shown in Table 2. The paints listed in Table 2 were prepared using the corresponding preparation methods of the paints of this invention.

[0119] [Table 2]

[0120]

[0121] Subsequently, the steel billets of each embodiment in Table 2 were heated in a heating furnace at a homogenization temperature of 1200℃ for 420 minutes. After exiting the heating furnace, the steel billets of each embodiment underwent surface quality metallographic analysis, for example, using GB / T 15125-2009 "Metallic Materials - Metallographic Examination Test Specimens and Test Methods" standard. The specific test results for each test example are shown in Table 3. High-pressure water descaling was then performed using the same descaling water pressure (specifically 18MPa). After descaling, the surface quality of the steel billets was then tested using metallographic analysis, for example, using GB / T 15125-2009 "Metallic Materials - Metallographic Examination Test Specimens and Test Methods" standard. The oxide scale removal rate is shown in Table 3.

[0122] [Table 3]

[0123] Surface oxide scale coverage (%) Average depth of surface oxide layer (mm) Oxide scale removal rate (%) Example B1 2.7 0.218 99.0 Example B2 2.8 0.237 99.1 Example B3 2.8 0.261 98.8 Example B4 4.6 0.331 100.0 Example B5 5.2 0.354 100.0 Comparative Example B6 100.0 0.477 37.5

[0124] As can be seen from Table 3, in Examples B1 to B3 using the coating of the first preferred embodiment of the present invention, the amount of oxide scale generated during high-temperature heating is greatly reduced, and the coating has excellent anti-oxidation effect on the steel billet during high-temperature heating. In Examples B4 to B5 using the coating of the second preferred embodiment of the present invention, the amount of oxide scale generated during high-temperature heating is greatly reduced (compared to Comparative Example B6), and the oxide scale has low viscosity, resulting in excellent oxide scale removal during descaling. That is, Examples B1 to B5 can all ensure that there is less oxide scale on the surface of the steel billet after descaling, thereby preventing the oxide scale from being pressed deep into the steel plate matrix during rolling, thus ensuring the surface quality of the final steel plate product.

[0125] It should be noted that in this application, "surface oxide scale coverage" refers to the proportion of the steel surface covered by oxide scale, which is characterized by the ratio of the oxide scale area of ​​the sample to the total area of ​​the sample; "average surface oxide scale depth" is characterized by the average oxide scale depth of the n samples; "oxide scale removal rate" refers to the ratio of the oxide scale area removed after descaling to the oxide scale area before descaling, which is characterized by the formula (100% - S1 / (surface oxide scale coverage × S)) based on the oxide scale area S1 of the sample (after descaling) and the total area S of the sample (after descaling).

[0126] Furthermore, the steel billets in each embodiment of Table 1 are processed into finished steel plates using the hot-rolling pretreatment-hot rolling-cooling-heat treatment technique described in this invention. The coating used in each embodiment is coating 2 from Table 2, and the key parameters for the heating, hot rolling, cooling, and heat treatment processes are shown in Table 4. In Table 4, the "soaking zone" and "furnace time" for embodiments A1, A4, and A7 refer to the soaking zone temperature and furnace time T after billet opening; the "second opening temperature" for embodiments A2-A3, A5-A6, and A8-A9 refers to the opening temperature of the second stage of rolling.

[0127] [Table 4]

[0128]

[0129] [Table 4 continued]

[0130]

[0131] For the finished steel plates of Examples A1 to A9, samples were taken according to GB / T 15125-2009 "Metallic Materials - Test Specimens and Test Methods for Metallographic Examination". Mechanical properties were tested according to GB / T 228.1-2021 "Metallic Materials - Tensile Testing - Part 1: Test Method at Room Temperature" and low-temperature toughness was tested according to GB / T 229-2007 "Metallic Materials - Charpy Pendulum Impact Test Method". The test results are shown in Table 5. Surface quality and metallographic structure were also tested. All examples showed excellent surface quality, with a surface oxide scale coverage of 2.5%, an average oxide scale indentation depth of 0.225 mm, and an oxide scale removal rate of over 98.5%.

[0132] [Table 5]

[0133] Yield strength, MPa Tensile strength, MPa The ratio of yield strength -135 impact, J Elongation, % Example A1 419 697 0.60 268,354,264 25 Example A2 562 702 0.80 282,319,294 26 Example A3 436 710 0.61 349,339,337 26 Example A4 544 659 0.83 304,302,303 27 Example A5 492 646 0.76 243,265,251 26 Example A6 511 606 0.84 250,354,344 25 Example A7 512 624 0.82 242,288,360 27 Example A8 558 668 0.84 277,360,308 26 Example A9 543 673 0.81 263,322,244 27

Claims

1. A method for producing low-temperature steel plates for ship storage, characterized in that, The finished thickness H of the steel plate is 8~50mm, and the production method includes: The steel is smelted and cast into steel billets with a thickness of 220-250 mm. The chemical composition of the steel billet, by mass percentage, includes: C: 0.05-0.07%, Si: 0.15-0.25%, Mn: 0.5-0.7%, P≤0.008%, S≤0.003%, Cr≤0.05%, Ni: 4.85-5.3%, Cu≤0.015%, Nb≤0.002%, Ti≤0.002%, Alt: 0.02-0.05%, N≤0.004%, with the balance being iron and unavoidable impurities. The steel billet is heated in a heating furnace at a soaking temperature of 1160~1200℃. Before entering the heating furnace, the steel billet undergoes surface grinding, and then a coating is applied to the ground surface. The coating is prepared from 60~70 parts by weight of SiO2, 15~20 parts by weight of Al2O3, 0.5~1.5 parts by weight of ZrO2, 1~3 parts by weight of SiC, 1~2 parts by weight of B4C, 4.5~22 parts by weight of binder and solvent. After exiting the heating furnace, the rolling mill is kept free of roller table water between the heating furnace and the rough descaling machine for hot rolling. High-pressure water descaling is performed before the first and third rolling passes, with a descaling water pressure ≥22MPa. The initial rolling temperature is 1050~1100℃, and the final rolling temperature is adjusted according to the finished product thickness H. When 8mm ≤ H < 12mm, the final rolling temperature T... fr +(100~120)℃, when 12mm≤H≤50mm, the final rolling temperature T fr ±20℃; where T fr =902-98C+47Si-10Mn-9.7Ni+95Cr-24Cu-115Ti+223Nb-202Al, where the element symbols in this formula represent 100 times the mass percentage of each element in the billet; The hot-rolled steel sheet is cooled and then heat-treated to obtain the finished steel sheet; the heat treatment includes tempering at a temperature of Ac1-50~80℃, where Ac1=T fc The holding time for tempering is [(2.0~3.0)H]min / mm and more than 30min, where T fc =784+117C+28Si-10Mn+11Ni-126Cr-34Cu-131Ti+357Nb-173Al, where the element symbols represent 100 times the mass percentage of each element in the billet.

2. The method for producing low-temperature steel plates for ship storage according to claim 1, characterized in that, When 8mm≤H<12mm, the production method further includes: firstly grinding the surface of the cast steel billet, then applying a coating to the ground surface for the first time, then heating it in a heating furnace at a soaking temperature of 1200~1240℃, and then cutting it into billets with a thickness of 80~120mm; then, heating the billet in a heating furnace at a soaking temperature of 1160~1200℃; before entering the heating furnace, the billet is ground, and then a coating is applied to the ground surface.

3. The method for producing low-temperature steel plates for ship storage according to claim 1, characterized in that, When H≥12mm, the "hot rolling" is a two-stage rolling process. The total reduction in the first stage of rolling is 53~79%. When 40mm<H≤50mm, the starting rolling temperature of the second stage of rolling after the initial heating period is 820~860℃. When 12mm≤H≤40mm, the starting rolling temperature of the second stage of rolling after the initial heating period is 890~940℃.

4. The method for producing low-temperature steel plates for ship storage according to claim 1, characterized in that, In the phrase "cooling the hot-rolled steel plate": When 12mm≤H≤40mm, air cooling is used; When H < 12 mm or H > 40 mm, an accelerated cooling control system is used for water cooling, with a final cooling temperature ≤ 200℃ and a reddening temperature ≤ 300℃.

5. The method for producing low-temperature steel plates for ship storage according to claim 4, characterized in that, If H < 12 mm, control the inlet water temperature T in the accelerated cooling control system. fc +90~115℃, cooling rate (25+1.5H / mm)±1.5℃ / s; if H>40mm, control the inlet water temperature T in the accelerated cooling control system. fc ±10℃, cooling rate (25+0.5H / mm)±1.5℃ / s.

6. The method for producing low-temperature steel plates for ship storage according to claim 1, characterized in that, When H ≥ 12 mm, the heat treatment further includes quenching before tempering, with a quenching holding time of [(2.0~3.0)H] min / mm. When 12 mm ≤ H ≤ 40 mm, the quenching temperature is Ac3 + 30~50℃, and when 40 mm < H ≤ 50 mm, the quenching temperature is Ac3 - 50~90℃, where Ac3 = T. fr -60~90℃.

7. The method for producing low-temperature steel plates for ship storage according to claim 1, characterized in that, The coating also satisfies the following condition by weight: ZrO2 + (0.10~0.20) = (SiC / 2) 0.5 SiO2 / Al2O3 = (2.5~4.5) and SiC + B4C = 2.5~5.

8. A method for producing low-temperature steel plates for ship storage, characterized in that, The finished thickness H of the steel plate is 8~50mm, and the production method includes: The steel is smelted and cast into steel billets with a thickness of 220-250 mm. The chemical composition of the steel billet, by mass percentage, includes: C: 0.05-0.07%, Si: 0.15-0.25%, Mn: 0.5-0.7%, P≤0.008%, S≤0.003%, Cr≤0.05%, Ni: 4.85-5.3%, Cu≤0.015%, Nb≤0.002%, Ti≤0.002%, Alt: 0.02-0.05%, N≤0.004%, with the balance being iron and unavoidable impurities. The steel billet is heated in a heating furnace at a soaking temperature of 1160~1200℃. Before entering the heating furnace, the steel billet undergoes surface grinding, and then a coating is applied to the ground surface. The coating is prepared from 30~60 parts by weight of SiO2, 3~20 parts by weight of Al2O3, 5~18 parts by weight of ZrO2, 1~12 parts by weight of SiC, 1~8 parts by weight of C, 1~3 parts by weight of B4C, 2~16 parts by weight of binder and solvent. After exiting the heating furnace, the rolling mill is kept free of roller table water between the heating furnace and the rough descaling machine for hot rolling. High-pressure water descaling is performed before the first and third rolling passes, with a descaling water pressure ≥22MPa. The initial rolling temperature is 1050~1100℃, and the final rolling temperature is adjusted according to the finished product thickness H. When 8mm ≤ H < 12mm, the final rolling temperature T... fr +(100~120)℃, when 12mm≤H≤50mm, the final rolling temperature T fr ±20℃; where T fr =902-98C+47Si-10Mn-9.7Ni+95Cr-24Cu-115Ti+223Nb-202Al, where the element symbols in this formula represent 100 times the mass percentage of each element in the billet; The hot-rolled steel sheet is cooled and then heat-treated to obtain the finished steel sheet; the heat treatment includes tempering at a temperature of Ac1-50~80℃, where Ac1=T fc The holding time for tempering is [(2.0~3.0)H]min / mm and more than 30min, where T fc =784+117C+28Si-10Mn+11Ni-126Cr-34Cu-131Ti+357Nb-173Al, where the element symbols represent 100 times the mass percentage of each element in the billet.

9. The method for producing low-temperature steel plates for ship storage according to claim 8, characterized in that, The coating, by weight, also satisfies the following: Al2O3=(0.1~0.4)SiO2, ZrO2=(1~1.5)SiC and SiC+C+B4C=3~23.

10. The method for producing low-temperature steel plates for ship storage according to claim 1, characterized in that, When applying paint: A full coat is applied in multiple passes. The time T after the steel billet is coated in the heating furnace is obtained. When T≤400min, the coating is stopped after one full spraying of the steel billet surface; when T>400min, the coating is stopped after n=ceil((t-400min) / 30min) full sprayings of the steel billet surface. Each full-coverage spray coating is 0.2~0.3mm thick.

11. The method for producing low-temperature steel plates for ship storage according to claim 1, characterized in that, The chemical composition of the steel billet, expressed as a percentage by mass, is: Mn = 2Si + 0.05~0.22%, Mn + Si: 0.65~0.95%.

Citation Information

Patent Citations

  • Marine 5Ni steel plate with excellent brittle failure resistance and manufacturing method thereof

    CN114892105A