A nanoparticle-reinforced Mg-Sn binary alloy and its preparation method

By refining Mg2Sn particles to the nanoscale through semi-solid isothermal treatment and hot extrusion, the problem of insufficient mechanical properties of magnesium alloys has been solved, and low-cost, high-performance Mg-Sn binary alloys have been prepared, expanding their application range.

CN118064739BActive Publication Date: 2026-11-10SOUTHWEST JIAOTONG UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410226838.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-02-29
Publication Date
2026-11-10
Estimated Expiration
2044-02-29

AI Technical Summary

Technical Problem

Existing magnesium alloys have poor corrosion resistance and high-temperature strength, and their room-temperature mechanical properties need to be further improved. Furthermore, existing methods are insufficient to refine Mg2Sn particles, leading to increased alloy costs and reduced elongation.

Method used

By employing semi-solid isothermal treatment and hot extrusion processes, nanoparticle-reinforced Mg-Sn binary alloys are prepared. Combining primary and secondary extrusion processes, Mg2Sn particles are refined to the nanoscale and dispersed on the α-Mg matrix, thereby improving the alloy's yield strength, tensile strength, and elongation.

Benefits of technology

It significantly improves the comprehensive mechanical properties of Mg-Sn binary alloys, reduces alloy costs, and expands their industrial application range, resulting in high-performance magnesium alloys with excellent yield strength, tensile strength, and elongation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118064739B_ABST
    Figure CN118064739B_ABST
Patent Text Reader

Abstract

A nanoparticle-reinforced Mg-Sn binary alloy and its preparation method are disclosed. The preparation method comprises the following steps: A. Preparing a cast Mg-Sn binary alloy according to the set mass percentage ratio of each constituent element; the set mass percentage ratio of each constituent element is: 1-14% Sn, unavoidable impurity element content ≤0.1%, and the remainder being Sn; B. Annealing the cast Mg-Sn binary alloy; C. Holding the annealed Mg-Sn binary alloy at 300-400℃ for 2-4 hours, followed by hot extrusion, with the extrusion temperature... The extrusion temperature is 300-400℃, the extrusion speed is 0.1-5 mm / s, and the extrusion ratio is 9-30:1; D. The hot-extruded Mg-Sn binary alloy is placed in a heat treatment furnace and heated to 550-640℃ for semi-solid isothermal treatment, held for 0.1-4 hours, and then water-quenched; E. The Mg-Sn binary alloy is held at 200-400℃ for 2-4 hours, and then subjected to a second extrusion to obtain the final product; the second extrusion temperature is 200-400℃, the extrusion speed is 0.1-5 mm / s, and the extrusion ratio is 9-60:1. The Mg-Sn binary alloy prepared by this method has excellent yield strength, tensile strength, and elongation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a nanoparticle-reinforced Mg-Sn binary alloy and its preparation method, belonging to the field of magnesium alloy manufacturing. Background Technology

[0002] Magnesium alloys, as a green metallic material, possess low density, high specific stiffness, excellent noise reduction and vibration resistance, and good casting properties, making them widely used in transportation, aerospace, and electronic communications. However, magnesium alloys have poor corrosion resistance and high-temperature strength, and their room-temperature mechanical properties still need further improvement to meet broader application requirements. Currently, alloying and hot deformation are the main methods to effectively improve the mechanical properties of magnesium alloys. While hot deformation can improve the properties of magnesium alloys to some extent, it is still not ideal. Alloying, as the simplest and most effective strengthening method, can effectively improve the microstructure of Mg-Sn binary alloys by adding alloying elements, thereby improving alloy performance. However, it also increases the cost of alloys and makes the manufacturing process more complex. Therefore, applying new processing technologies to achieve low-cost, high-performance magnesium alloys is of great significance.

[0003] The particle size and distribution of non-precipitated Mg2Sn particles have a significant impact on the mechanical properties of Mg-Sn binary alloys. Currently, Mg2Sn particles in deformed Mg-Sn alloys are mostly micrometer-sized, and existing deformation techniques make it difficult to further refine the particle size. To obtain particle-reinforced Mg-Sn alloys with excellent mechanical properties, existing methods can increase the volume fraction of the eutectic phase in the Mg-Sn alloy by increasing the Mg content. However, this leads to a decrease in the elongation of the alloy and a significant increase in alloy cost. In practical applications, magnesium alloys are required to have excellent comprehensive mechanical properties. Therefore, developing high-performance Mg-Sn alloys with excellent yield strength, tensile strength, and elongation is an urgent problem to be solved. Summary of the Invention

[0004] The purpose of this invention is to provide a nanoparticle-reinforced Mg-Sn binary alloy and its preparation method. This preparation method combines semi-solid isothermal treatment and hot extrusion process, and the prepared nanoparticle-reinforced Mg-Sn binary alloy has excellent yield strength, tensile strength and elongation.

[0005] The technical solution adopted by this invention to achieve its objective is: a nanoparticle-reinforced Mg-Sn binary alloy and its preparation method, the preparation method steps are as follows:

[0006] A. Prepare a cast Mg-Sn binary alloy according to the set mass percentage of each component element; the set mass percentage of each component element is: 1-14% Sn, unavoidable impurity element content ≤0.1%, and the remainder is Sn;

[0007] B. Anneal the as-cast Mg-Sn binary alloy prepared in step A;

[0008] C. After holding the annealed Mg-Sn binary alloy obtained in step B at 300-400℃ for 2-4 hours, hot extrusion is carried out. The extrusion temperature is 300-400℃, the extrusion speed is 0.1-5mm / s, and the extrusion ratio is 9-30:1.

[0009] D. Place the hot-extruded Mg-Sn binary alloy obtained in step C into a heat treatment furnace, heat it to 550-640℃ with the furnace for semi-solid isothermal treatment, hold it for 0.1-4h, and then water-quench it.

[0010] E. After holding the Mg-Sn binary alloy obtained in step D at 200-400℃ for 2-4 hours, it is then subjected to secondary extrusion to obtain nanoparticle-reinforced Mg-Sn binary alloy; the extrusion temperature of the secondary extrusion is 200-400℃, the extrusion speed is 0.1-5mm / s, and the extrusion ratio is 9-60:1.

[0011] The reaction principle of this invention is as follows: The as-cast Mg-Sn binary alloy obtained in step A has a eutectic phase morphology of micron-level lamellar spacing (α-Mg+Mg2Sn). After annealing in step B and hot extrusion in step C, the micron-level eutectic structure is broken into micron-level Mg2Sn particles. Then, through step D, the micron-level Mg2Sn particles are transformed into a nanon-level eutectic structure (α-Mg+Mg2Sn). Finally, after a second extrusion in step E, the nanon-level eutectic structure is broken into nanon-level Mg2Sn particles, which are dispersed on the α-Mg matrix and act as a reinforcing phase to improve the mechanical properties of the Mg-Sn binary alloy. This process produces a high-performance Mg-Sn alloy with excellent yield strength, tensile strength, and elongation.

[0012] Compared with the prior art, the beneficial effects of the present invention are:

[0013] First, the mass percentage of the constituent elements set in step A ensures that a Mg-Sn binary alloy with a eutectic (α-Mg+Mg2Sn) interlamellar spacing of nanometers can be obtained through subsequent processing steps B, C, and D.

[0014] 2. Homogenization annealing of the as-cast Mg-Sn binary alloy can remove the stress of the alloy and make it more deformable and workable; then hot extrusion treatment in step C can obtain a particle-reinforced Mg-Sn binary alloy with micron-sized Mg2Sn particles.

[0015] 3. Step D: The particle-reinforced Mg-Sn binary alloy with micron-sized Mg2Sn particles obtained in step C is subjected to semi-solid treatment. By controlling the temperature and time of the semi-solid treatment, a Mg-Sn binary alloy with nanometer-sized eutectic (α-Mg+Mg2Sn) interlamellar spacing is obtained in a short time.

[0016] IV. After obtaining a Mg-Sn binary alloy with a eutectic (α-Mg+Mg2Sn) interlamellar spacing of nanometers, the present invention selects a secondary extrusion method to break the nano-eutectic phase into nano-sized Mg2Sn particles, which are dispersed on the α-Mg matrix, thus obtaining a particle-reinforced Mg-Sn binary alloy with nano-sized Mg2Sn particles.

[0017] In summary, this invention, based on the Mg-Sn binary alloy prepared by traditional casting, combines primary extrusion, semi-solid treatment, and secondary extrusion processes to achieve the transformation of the second phase in the alloy from micron-scale lamellar to micron-scale particles, then to nano-scale lamellar, and finally to nano-scale particles. This results in a particle-reinforced Mg-Sn binary alloy with nano-scale Mg2Sn particles, significantly improving the comprehensive mechanical properties of the Mg-Sn binary alloy and greatly expanding the industrial application range of the Mg-Sn binary alloy.

[0018] Furthermore, in step A of the preparation method of the present invention, the mass percentage content of each constituent element in the preparation of the as-cast Mg-Sn binary alloy is set as follows: 2.5-7.5% Sn, unavoidable impurity element content ≤0.1%, and the remainder is Mg.

[0019] Experiments have verified that the mass percentage of the above elements can prepare stable eutectic (α-Mg+Mg2Sn) Mg-Sn binary alloys with a lamellar spacing of less than 100 nm. At the same time, the absence of other strengthening alloying elements greatly simplifies the preparation of the alloy and reduces the preparation cost.

[0020] Furthermore, the specific operation of step A in the preparation method of the present invention for preparing the as-cast Mg-Sn binary alloy is as follows: according to the set mass percentage ratio of each component element, pure Mg is placed in a crucible and heated to 300-400℃, and a mixed protective gas of CO2+SF6 is introduced. After the pure Mg has completely melted, pure Sn is placed in the pure Mg melt, and the temperature is continued to be heated to 720-760℃. After stirring for 2-5 minutes, the slag is removed, and the mixture is allowed to stand for 5-15 minutes. When the temperature drops to 700-750℃, the mixture is poured to obtain the as-cast Mg-Sn binary alloy.

[0021] Furthermore, in the preparation method of the present invention, the annealing temperature of step B, annealing treatment, is 390-460℃, and the annealing time is 10-24h.

[0022] Furthermore, in step C of the preparation method of the present invention, the extrusion ratio for hot extrusion of the annealed Mg-Sn binary alloy obtained in step B is 9-15:1.

[0023] Experiments have verified that the above extrusion ratio can make the thickness of the semi-solid Mg-Sn binary alloy layers more uniform, which is beneficial to the preparation of Mg-Sn binary alloys with stable nanoscale layer thickness. This is conducive to the preparation of particle-reinforced Mg-Sn binary alloys with nanoscale Mg2Sn particles that have excellent performance in all aspects.

[0024] Furthermore, in step D of the preparation method of the present invention, the Mg-Sn binary alloy obtained by hot extrusion in step C is placed in a heat treatment furnace and heated to 580-620℃ for semi-solid isothermal treatment, held for 0.1-1h, and then water-cooled and quenched.

[0025] Experiments have verified that the above temperature range and holding time are more conducive to the preparation of Mg-Sn binary alloys with stable nanoscale interlamellar spacing, which in turn is beneficial to the preparation of particle-reinforced Mg-Sn binary alloys with nanoscale Mg2Sn particles that have excellent performance in all aspects.

[0026] Furthermore, in step D of the preparation method of the present invention, the quenching medium for water-cooled quenching is water at 20-80°C.

[0027] Experiments have verified that quenching with water within the above temperature range results in a more uniform layer thickness in the semi-solid Mg-Sn binary alloy, which is beneficial for preparing Mg-Sn binary alloys with stable nanoscale layer thickness. This, in turn, facilitates the preparation of particle-reinforced Mg-Sn binary alloys with nanoscale Mg2Sn particles that exhibit excellent performance in all aspects.

[0028] Furthermore, the extrusion ratio of the secondary extrusion in step E of the preparation method of the present invention is 9-30:1.

[0029] Experiments have verified that the Mg-Sn binary alloy prepared by the above-mentioned secondary extrusion and pressing ratio has better comprehensive mechanical properties and can be used to prepare high-performance Mg alloys with excellent yield strength, tensile strength and elongation. Attached Figure Description

[0030] Figure 1 The image shows the tensile curve of the nanoparticle-reinforced Mg-Sn binary alloy prepared in Example 5 of this invention.

[0031] Figure 2 This is a SEM image of the semi-solid structure of the nanoparticle-reinforced Mg-Sn binary alloy prepared in step D of Example 5 of the present invention.

[0032] Figure 3This is a SEM image of the extruded microstructure of the nanoparticle-reinforced Mg-Sn binary alloy prepared in step E of Example 5 of the present invention. Detailed Implementation

[0033] Example 1

[0034] A nanoparticle-reinforced Mg-Sn binary alloy and its preparation method are described below:

[0035] A. Prepare a cast Mg-Sn binary alloy according to the set mass percentage of each component element; the set mass percentage of each component element is: 3.4% Sn, unavoidable impurity element content ≤0.1%, and the remainder is Mg; the specific operation for preparing the cast Mg-Sn binary alloy is as follows: pure Mg is placed in a crucible and heated to 300°C, and a CO2+SF6 mixed protective gas is introduced. After the pure Mg is completely melted, pure Sn is placed in the pure Mg melt, and the temperature is continued to rise to 730°C. After stirring for 5 minutes, the slag is removed, and the mixture is allowed to stand for 10 minutes. When the temperature drops to 720°C, the alloy is poured to obtain the cast Mg-Sn binary alloy.

[0036] B. Anneal the as-cast Mg-Sn binary alloy prepared in step A at 420℃ for 12h and then cool it in the furnace.

[0037] C. After the annealed Mg-Sn binary alloy obtained in step B is kept at 380℃ for 4 hours, it is hot extruded. The extrusion temperature is 380℃, the extrusion speed is 2mm / s, and the extrusion ratio is 9:1.

[0038] D. Place the hot-extruded Mg-Sn binary alloy obtained in step C into a heat treatment furnace, heat it to 600℃ with the furnace for semi-solid isothermal treatment, hold it for 20 minutes, and then water-quench it. The quenching medium for water-quenching is water at 75℃.

[0039] E. After holding the Mg-Sn binary alloy obtained in step D at 380℃ for 2 hours, it is then subjected to secondary extrusion to obtain nanoparticle-reinforced Mg-Sn binary alloy; the extrusion temperature of the secondary extrusion is 380℃, the extrusion speed is 2mm / s, and the extrusion ratio is 10:1.

[0040] The Mg-Sn binary alloy prepared in this example has a tensile strength of 299 MPa, a yield strength of 263 MPa, and an elongation of 16.41%.

[0041] Example 2

[0042] A nanoparticle-reinforced Mg-Sn binary alloy and its preparation method are described below:

[0043] A. Prepare a cast Mg-Sn binary alloy according to the set mass percentage of each component element; the set mass percentage of each component element is: 4.6% Sn, unavoidable impurity element content ≤0.1%, and the remainder is Mg; the specific operation for preparing the cast Mg-Sn binary alloy is as follows: place pure Mg in a crucible and heat to 320°C, then introduce a CO2+SF6 mixed protective gas. After the pure Mg has completely melted, place pure Sn in the pure Mg melt, continue heating to 720°C, stir for 5 minutes, remove slag, let stand for 15 minutes, and when the temperature drops to 725°C, pour to obtain the cast Mg-Sn binary alloy;

[0044] B. Anneal the as-cast Mg-Sn binary alloy prepared in step A at 410℃ for 24h, and then cool it in the furnace.

[0045] C. After the annealed Mg-Sn binary alloy obtained in step B is kept at 350℃ for 4 hours, it is hot extruded. The extrusion temperature is 350℃, the extrusion speed is 2mm / s, and the extrusion ratio is 10:1.

[0046] D. Place the hot-extruded Mg-Sn binary alloy obtained in step C into a heat treatment furnace, heat it to 625℃ with the furnace for semi-solid isothermal treatment, hold it for 10 minutes, and then water-quench it. The quenching medium for water-quenching is water at 60℃.

[0047] E. After holding the Mg-Sn binary alloy obtained in step D at 350℃ for 2 hours, it is then subjected to a second extrusion to obtain a nanoparticle-reinforced Mg-Sn binary alloy. The extrusion temperature of the second extrusion is 350℃, the extrusion speed is 2 mm / s, and the extrusion ratio is 10:1.

[0048] The Mg-Sn binary alloy prepared in this example has a tensile strength of 303 MPa, a yield strength of 264 MPa, and an elongation of 15.44%.

[0049] Example 3

[0050] A nanoparticle-reinforced Mg-Sn binary alloy and its preparation method are described below:

[0051] A. Prepare a cast Mg-Sn binary alloy according to the set mass percentage of each component element; the set mass percentage of each component element is: 7.9% Sn, unavoidable impurity element content ≤0.1%, and the remainder is Mg; the specific operation for preparing the cast Mg-Sn binary alloy is as follows: pure Mg is placed in a crucible and heated to 350°C, and a CO2+SF6 mixed protective gas is introduced. After the pure Mg is completely melted, pure Sn is placed in the pure Mg melt, and the temperature is continued to rise to 730°C. After stirring for 3 minutes, the slag is removed, and the mixture is allowed to stand for 12 minutes. When the temperature drops to 715°C, the alloy is poured to obtain the cast Mg-Sn binary alloy.

[0052] B. Anneal the as-cast Mg-Sn binary alloy prepared in step A at 430℃ for 16h and then cool it in the furnace.

[0053] C. After the annealed Mg-Sn binary alloy obtained in step B is kept at 330℃ for 3 hours, it is hot extruded. The extrusion temperature is 330℃, the extrusion speed is 1mm / s, and the extrusion ratio is 20:1.

[0054] D. Place the hot-extruded Mg-Sn binary alloy obtained in step C into a heat treatment furnace, heat it to 600℃ with the furnace for semi-solid isothermal treatment, hold it for 30 minutes, and then water-quench it. The quenching medium for water-quenching is water at 45℃.

[0055] E. After holding the Mg-Sn binary alloy obtained in step D at 330℃ for 3 hours, it is then subjected to secondary extrusion to obtain nanoparticle-reinforced Mg-Sn binary alloy; the extrusion temperature of the secondary extrusion is 309℃, the extrusion speed is 2mm / s, and the extrusion ratio is 10:1.

[0056] The Mg-Sn binary alloy prepared in this example has a tensile strength of 329 MPa, a yield strength of 288 MPa, and an elongation of 10.5%.

[0057] Example 4

[0058] A nanoparticle-reinforced Mg-Sn binary alloy and its preparation method are described below:

[0059] A. Prepare a cast Mg-Sn binary alloy according to the set mass percentage of each component element; the set mass percentage of each component element is: 10.5% Sn, unavoidable impurity element content ≤0.1%, and the remainder is Mg; the specific operation for preparing the cast Mg-Sn binary alloy is as follows: place pure Mg in a crucible and heat to 390°C, then introduce a CO2+SF6 mixed protective gas. After the pure Mg has completely melted, place pure Sn in the pure Mg melt, continue heating to 740°C, stir for 4 minutes, remove slag, let stand for 9 minutes, and when the temperature drops to 720°C, pour to obtain the cast Mg-Sn binary alloy;

[0060] B. Anneal the as-cast Mg-Sn binary alloy prepared in step A at 426℃ for 16h and then cool it in the furnace.

[0061] C. After the annealed Mg-Sn binary alloy obtained in step B is kept at 365℃ for 4 hours, it is hot extruded. The extrusion temperature is 365℃, the extrusion speed is 3mm / s, and the extrusion ratio is 25:1.

[0062] D. Place the hot-extruded Mg-Sn binary alloy obtained in step C into a heat treatment furnace, heat it to 590℃ with the furnace for semi-solid isothermal treatment, hold it for 40 minutes, and then water-quench it. The quenching medium for water-quenching is water at 40℃.

[0063] E. After holding the Mg-Sn binary alloy obtained in step D at 300℃ for 2.5h, it is then subjected to secondary extrusion to obtain nanoparticle-reinforced Mg-Sn binary alloy; the extrusion temperature of the secondary extrusion is 300℃, the extrusion speed is 2.5mm / s, and the extrusion ratio is 15:1.

[0064] The Mg-Sn binary alloy prepared in this example has a tensile strength of 342 MPa, a yield strength of 300 MPa, and an elongation of 6.4%.

[0065] Example 5

[0066] A nanoparticle-reinforced Mg-Sn binary alloy and its preparation method are described below:

[0067] A. Prepare a cast Mg-Sn binary alloy according to the set mass percentage of each component element; the set mass percentage of each component element is: 12.1% Sn, unavoidable impurity element content ≤0.1%, and the remainder is Mg; the specific operation for preparing the cast Mg-Sn binary alloy is as follows: pure Mg is placed in a crucible and heated to 360°C, and a CO2+SF6 mixed protective gas is introduced. After the pure Mg is completely melted, pure Sn is placed in the pure Mg melt, and the temperature is continued to rise to 732°C. After stirring for 4 minutes, the slag is removed, and the mixture is allowed to stand for 8 minutes. When the temperature drops to 728°C, the alloy is poured to obtain the cast Mg-Sn binary alloy.

[0068] B. Anneal the as-cast Mg-Sn binary alloy prepared in step A at 435℃ for 11 hours and then cool it in the furnace.

[0069] C. After the annealed Mg-Sn binary alloy obtained in step B is kept at 370℃ for 4 hours, it is hot extruded. The extrusion temperature is 370℃, the extrusion speed is 2.4 mm / s, and the extrusion ratio is 20:1.

[0070] D. Place the hot-extruded Mg-Sn binary alloy obtained in step C into a heat treatment furnace, heat it to 615℃ with the furnace for semi-solid isothermal treatment, hold it for 25 minutes, and then water-quench it. The quenching medium for water-quenching is water at 20℃.

[0071] E. After holding the Mg-Sn binary alloy obtained in step D at 305℃ for 3.5h, it is then subjected to secondary extrusion to obtain nanoparticle-reinforced Mg-Sn binary alloy; the extrusion temperature of the secondary extrusion is 305℃, the extrusion speed is 2mm / s, and the extrusion ratio is 15:1.

[0072] The Mg-Sn binary alloy prepared in this example has a tensile strength of 356 MPa, a yield strength of 311 MPa, and an elongation of 4.95%.

[0073] Figure 1 The tensile curve of the nanoparticle-reinforced Mg-Sn binary alloy prepared in this embodiment is shown. Figure 2 This is a SEM image of the semi-solid microstructure of the nanoparticle-reinforced Mg-Sn binary alloy prepared in step D of this embodiment. Figure 2 Image (a) shows the SEM image of the semi-solid microstructure of the Mg-Sn binary alloy after semi-solid isothermal treatment in Example 5. After the semi-solid isothermal treatment, solute atoms rapidly diffuse to the grain boundaries and remelt at high temperature. After rapid quenching, a continuous network eutectic microstructure is formed. At the same time, small liquid pools also exist within the grains due to solute atom segregation, local defects, or local stress concentration, which are formed during remelting and solidification. Figure 2In the middle (b), which is a magnified view of (a), it can be seen that the Mg2Sn eutectic phase has been refined to the nanoscale. Figure 3 This is a SEM image of the extruded microstructure of the nanoparticle-reinforced Mg-Sn binary alloy prepared in step E of this embodiment. Figure 3 In the middle (a), there is a SEM image of the nanoparticle-reinforced Mg-Sn binary alloy after hot extrusion. The nano-Mg-Sn layers at the grain boundaries are completely broken into nano-Mg-Sn particles and distributed in a band-like pattern along the extrusion direction. Figure 3 In the middle (b), which is a magnified view of (a), it can be seen that the nano Mg2Sn sheets are refined into nano Mg2Sn particles and some short nano Mg2Sn sheets that are not completely broken during the extrusion process. In addition, some dynamically precipitated nano Mg2Sn particles were found in the matrix.

[0074] Example 6

[0075] A nanoparticle-reinforced Mg-Sn binary alloy and its preparation method are described below:

[0076] A. Prepare a cast Mg-Sn binary alloy according to the set mass percentage of each component element; the set mass percentage of each component element is: 1% Sn, unavoidable impurity element content ≤0.1%, and the remainder is Mg; the specific operation for preparing the cast Mg-Sn binary alloy is as follows: place pure Mg in a crucible and heat to 400℃, then introduce a CO2+SF6 mixed protective gas. After the pure Mg has completely melted, place pure Sn in the pure Mg melt, continue heating to 760℃, stir for 2 minutes, remove slag, let stand for 5 minutes, and when the temperature drops to 700℃, pour to obtain the cast Mg-Sn binary alloy;

[0077] B. Anneal the as-cast Mg-Sn binary alloy prepared in step A at 390℃ for 24 hours, and then cool it in the furnace.

[0078] C. After the annealed Mg-Sn binary alloy obtained in step B is kept at 300℃ for 4 hours, it is hot extruded. The extrusion temperature is 300℃, the extrusion speed is 0.1mm / s, and the extrusion ratio is 15:1.

[0079] D. Place the hot-extruded Mg-Sn binary alloy obtained in step C into a heat treatment furnace, heat it to 550℃ with the furnace for semi-solid isothermal treatment, hold it for 4 hours, and then water-quench it. The quenching medium for water-quenching is water at 20℃.

[0080] E. After holding the Mg-Sn binary alloy obtained in step D at 380℃ for 2 hours, it is then subjected to secondary extrusion to obtain nanoparticle-reinforced Mg-Sn binary alloy; the extrusion temperature of the secondary extrusion is 380℃, the extrusion speed is 2mm / s, and the extrusion ratio is 10:1.

[0081] Example 7

[0082] A nanoparticle-reinforced Mg-Sn binary alloy and its preparation method are described below:

[0083] A. Prepare a cast Mg-Sn binary alloy according to the set mass percentage of each component element; the set mass percentage of each component element is: 3.4% Sn, unavoidable impurity element content ≤0.1%, and the remainder is Mg; the specific operation for preparing the cast Mg-Sn binary alloy is as follows: pure Mg is placed in a crucible and heated to 300°C, and a CO2+SF6 mixed protective gas is introduced. After the pure Mg is completely melted, pure Sn is placed in the pure Mg melt, and the temperature is continued to rise to 730°C. After stirring for 5 minutes, the slag is removed, and the mixture is allowed to stand for 10 minutes. When the temperature drops to 720°C, the alloy is poured to obtain the cast Mg-Sn binary alloy.

[0084] B. Anneal the as-cast Mg-Sn binary alloy prepared in step A at 460℃ for 10h and then cool it in the furnace.

[0085] C. After the annealed Mg-Sn binary alloy obtained in step B is kept at 400℃ for 2 hours, it is hot extruded. The extrusion temperature is 400℃, the extrusion speed is 5mm / s, and the extrusion ratio is 30:1.

[0086] D. Place the hot-extruded Mg-Sn binary alloy obtained in step C into a heat treatment furnace, heat it to 640℃ with the furnace for semi-solid isothermal treatment, hold it for 6 minutes, and then water-quench it. The quenching medium for water-quenching is water at 80℃.

[0087] E. After holding the Mg-Sn binary alloy obtained in step D at 380℃ for 2 hours, it is then subjected to secondary extrusion to obtain nanoparticle-reinforced Mg-Sn binary alloy; the extrusion temperature of the secondary extrusion is 380℃, the extrusion speed is 2mm / s, and the extrusion ratio is 10:1.

[0088] Example 8

[0089] A nanoparticle-reinforced Mg-Sn binary alloy and its preparation method are described below:

[0090] A. Prepare a cast Mg-Sn binary alloy according to the set mass percentage of each component element; the set mass percentage of each component element is: 2.5% Sn, unavoidable impurity element content ≤0.1%, and the remainder is Mg; the specific operation for preparing the cast Mg-Sn binary alloy is as follows: place pure Mg in a crucible and heat to 300°C, then introduce a CO2+SF6 mixed protective gas. After the pure Mg has completely melted, place pure Sn in the pure Mg melt, continue heating to 730°C, stir for 5 minutes, remove slag, let stand for 10 minutes, and when the temperature drops to 750°C, pour to obtain the cast Mg-Sn binary alloy;

[0091] B. Anneal the as-cast Mg-Sn binary alloy prepared in step A at 420℃ for 12h and then cool it in the furnace.

[0092] C. After the annealed Mg-Sn binary alloy obtained in step B is kept at 380℃ for 4 hours, it is hot extruded. The extrusion temperature is 380℃, the extrusion speed is 2mm / s, and the extrusion ratio is 9:1.

[0093] D. Place the hot-extruded Mg-Sn binary alloy obtained in step C into a heat treatment furnace, heat it to 580℃ with the furnace for semi-solid isothermal treatment, hold it for 60 minutes, and then water-quench it. The quenching medium for water-quenching is water at 40℃.

[0094] E. After holding the Mg-Sn binary alloy obtained in step D at 380℃ for 2 hours, it is then subjected to secondary extrusion to obtain nanoparticle-reinforced Mg-Sn binary alloy; the extrusion temperature of the secondary extrusion is 380℃, the extrusion speed is 2mm / s, and the extrusion ratio is 10:1.

[0095] Example 9

[0096] A nanoparticle-reinforced Mg-Sn binary alloy and its preparation method are described below:

[0097] A. Prepare a cast Mg-Sn binary alloy according to the set mass percentage of each component element; the set mass percentage of each component element is: 7.5% Sn, unavoidable impurity element content ≤0.1%, and the remainder is Mg; the specific operation for preparing the cast Mg-Sn binary alloy is as follows: place pure Mg in a crucible and heat to 300℃, then introduce a CO2+SF6 mixed protective gas. After the pure Mg has completely melted, place pure Sn in the pure Mg melt, continue heating to 730℃, stir for 5 minutes, remove slag, let stand for 10 minutes, and when the temperature drops to 720℃, pour to obtain the cast Mg-Sn binary alloy;

[0098] B. Anneal the as-cast Mg-Sn binary alloy prepared in step A at 420℃ for 12 hours, and then cool it in the furnace.

[0099] C. After the annealed Mg-Sn binary alloy obtained in step B is kept at 380℃ for 4 hours, it is hot extruded. The extrusion temperature is 380℃, the extrusion speed is 2mm / s, and the extrusion ratio is 9:1.

[0100] D. Place the hot-extruded Mg-Sn binary alloy obtained in step C into a heat treatment furnace, heat it to 620℃ with the furnace for semi-solid isothermal treatment, hold it for 6 minutes, and then water-quench it. The quenching medium for water-quenching is water at 30℃.

[0101] E. After holding the Mg-Sn binary alloy obtained in step D at 380℃ for 2 hours, it is then subjected to secondary extrusion to obtain nanoparticle-reinforced Mg-Sn binary alloy; the extrusion temperature of the secondary extrusion is 380℃, the extrusion speed is 2mm / s, and the extrusion ratio is 10:1.

Claims

1. A method for preparing a nanoparticle-reinforced Mg-Sn binary alloy, comprising the following steps: A. Prepare a cast Mg-Sn binary alloy according to the set mass percentage of each component element; the set mass percentage of each component element is: 2.5-7.5% Sn, unavoidable impurity element content ≤0.1%, and the remainder is Mg; B. Anneal the as-cast Mg-Sn binary alloy prepared in step A; C. After holding the annealed Mg-Sn binary alloy obtained in step B at 300-400℃ for 2-4 hours, hot extrusion is carried out. The extrusion temperature is 300-400℃, the extrusion speed is 0.1-5mm / s, and the extrusion ratio is 9-30:

1. D. Place the hot-extruded Mg-Sn binary alloy obtained in step C into a heat treatment furnace and heat it to 580-620℃ for semi-solid isothermal treatment. Hold it for 0.1-1h to transform the micron-sized Mg2Sn particles in the Mg-Sn binary alloy into a eutectic (α-Mg+Mg2Sn) structure with a lamellar spacing of nanometers. Then, water-quench it. E. After holding the Mg-Sn binary alloy obtained in step D at 200-400℃ for 2-4 hours, a second extrusion is performed to break the eutectic (α-Mg+Mg2Sn) structure with nanoscale interlamellar spacing in the Mg-Sn binary alloy into nanoscale Mg2Sn particles, which are dispersed on the α-Mg matrix, thus obtaining a nanoparticle-reinforced Mg-Sn binary alloy. The extrusion temperature of the second extrusion is 200-400℃, the extrusion speed is 0.1-5mm / s, and the extrusion ratio is 9-30:

1.

2. The method for preparing a nanoparticle-reinforced Mg-Sn binary alloy according to claim 1, characterized in that: The specific operation for preparing the as-cast Mg-Sn binary alloy in step A is as follows: According to the set mass percentage ratio of each component element, pure Mg is placed in a crucible and heated to 300-400℃. A mixed protective gas of CO2 and SF6 is introduced. After the pure Mg has completely melted, pure Sn is placed in the pure Mg melt and heated to 720-760℃. After stirring for 2-5 minutes, the slag is removed, and the mixture is allowed to stand for 5-15 minutes. When the temperature drops to 700-750℃, the mixture is poured to obtain the as-cast Mg-Sn binary alloy.

3. The method for preparing a nanoparticle-reinforced Mg-Sn binary alloy according to claim 1, characterized in that: The annealing temperature for step B is 390-460℃, and the annealing time is 10-24h.

4. The method for preparing a nanoparticle-reinforced Mg-Sn binary alloy according to claim 1, characterized in that: In step C, the hot extrusion ratio of the annealed Mg-Sn binary alloy obtained in step B is 9-15:

1.

5. The method for preparing a nanoparticle-reinforced Mg-Sn binary alloy according to claim 1, characterized in that: In step D, the quenching medium for water-cooled quenching is water at 20-80℃.

6. A nanoparticle-reinforced Mg-Sn binary alloy, characterized in that: The nanoparticle-reinforced Mg-Sn binary alloy is prepared by any one of the preparation methods according to claims 1-5.

Citation Information

Patent Citations

  • Method of preparing nano quasi-crystal reinforced Mg-Zn-Y alloy by two times of extrusion

    CN107815578A

  • Magnesium based alloy extension material and method for producing the same

    JP2018012888A