KNbO₃ / Ag@WO₃ composite photocatalyst and its preparation method and application
By loading Ag@WO3 on the surface of KNbO3, a KNbO3/Ag@WO3 composite photocatalyst is formed, which solves the problems of narrow spectral response range and high recombination rate of existing photocatalysts, significantly improves the activity and efficiency of photocatalytic degradation of phenol, and has good application prospects.
Patent Information
- Application Number
- CN202410422394.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-09
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-04-09
AI Technical Summary
Existing photocatalysts such as KNbO3 and WO3 have problems such as large band gap, narrow spectral response range, high photogenerated electron hole recombination rate, and few surface active sites when photocatalytically degrading organic pollutants, which limits their photocatalytic activity and application potential.
Using KNbO3/Ag@WO3 composite photocatalyst, by loading narrow band gap Ag@WO3 on the surface of KNbO3, the spectral response range is expanded and the photogenerated carrier recombination rate is reduced, while the surface active sites of WO3 are increased to form KNbO3/Ag@WO3 Composite materials for photocatalytic degradation of phenol.
It significantly improves the activity of photocatalytic decomposition of phenol, reduces the electron-hole recombination rate, increases the light efficiency and light absorption range, overcomes the shortcomings of individual KNbO3 and WO3 photocatalysts, and has good prospects for environmental restoration and energy applications.
Smart Images

Figure CN118079910B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of photocatalytic materials, and in particular to a KNbO3 / Ag@WO3 composite photocatalyst and a preparation method and application thereof. Background Art
[0002] With the continuous development of industry, a large number of pollutants enter the water bodies and threaten human health; dye pollutants are one of the main sources of global environmental pollution. Dye pollutants accumulated in the environment can produce aromatic amine intermediates under the action of microorganisms, which have strong "three-cause" effects and potential environmental risks. Severe environmental pollution has prompted scientists to develop many methods to degrade organic compounds. In recent years, photocatalytic technology has become increasingly important because it plays a vital role in solving environmental pollution problems. Semiconductor materials can be used as photocatalysts to catalytically degrade organic pollutants. The catalyst degrades organic matter under light radiation and eventually completely mineralizes it into CO2, H2O and less toxic organic matter, inorganic ions, etc., showing its unique efficacy in energy and green chemistry.
[0003] Among all photocatalysts, potassium niobate (KNbO3) semiconductor is considered to be one of the most important photocatalysts due to its large nonlinear magnetic susceptibility and high photorefractive index. In addition, it has great application potential in photocatalytic degradation of organic pollutants due to its high stability, low cost, non-toxicity and strong oxidizing properties. However, due to its large band gap (~3.2eV) and the fact that it can only be excited under ultraviolet light, which only accounts for 4% of sunlight, and its photogenerated electron-hole pairs (e - -h + ) are easy to recombine, and the separation efficiency of photogenerated charges is low, which reduces its quantum efficiency. These factors greatly limit its photocatalytic activity.
[0004] At present, the main photocatalytic materials include titanium dioxide, graphene, carbon nitride, transition metal sulfides, transition metal oxides, etc. Among them, WO3, as a semiconductor photocatalyst, has a narrow band gap (~2.7 eV) and can effectively utilize part of the visible light. It shows good performance in degrading phenol pollutants. However, WO3 still has some shortcomings in photocatalysis, such as: (1) The conduction band position of WO3 photocatalyst is relatively low, and it is difficult for photogenerated electrons to reduce O2 adsorbed in the solution, resulting in a high recombination rate of photogenerated holes and electrons, thereby limiting its catalytic activity in the photodegradation reaction; (2) WO3 can only absorb part of the visible light, which limits its utilization rate of sunlight; (3) There are fewer active sites on the surface of WO3 photocatalyst. The above aspects will greatly affect the photocatalytic performance of WO3 and further affect its application in the field of photocatalysis. Summary of the invention
[0005] In view of the technical defects of the above-mentioned prior art, the purpose of the present invention is to provide a KNbO3 / Ag@WO3 composite photocatalyst and a preparation method and application thereof. The present invention uses Ag@WO3 and KNbO3 for compounding. On the one hand, by loading a band-matched narrow bandgap semiconductor on the surface of KNbO3, the spectral response range of KNbO3 is expanded and its photogenerated carrier recombination rate is reduced. On the other hand, Ag improves the surface active sites of WO3, so that the composite material simultaneously overcomes the technical defect of high recombination rate of photogenerated holes and electrons in KNbO3 and WO3, and the KNbO3 / Ag@WO3 composite photocatalyst is applied to the photodegradation of phenol.
[0006] In order to solve the above technical problems, the present invention adopts the following technical solutions:
[0007] The preparation method of KNbO3 / Ag@WO3 composite photocatalyst comprises the following steps:
[0008] The preparation methods of WO3 nanorods and KNbO3 microblocks are both existing technologies;
[0009] Using WO3 nanorods and KNbO3 microblocks as raw materials, WO3 nanorods, KNbO3 microblocks and soluble silver salt solution are mixed, and a photochemical reaction is first carried out under the irradiation of a xenon lamp. After the photochemical reaction, centrifugation and drying are carried out in sequence, and then annealing is carried out in an inert atmosphere to obtain a KNbO3 / Ag@WO3 composite photocatalyst; WO3 undergoes a photochemical reduction reaction with the soluble silver salt, and the silver ions are reduced and loaded on the WO3 nanorods. After annealing, a stable composite of KNbO3 and Ag@WO3 is achieved.
[0010] Preferably, the WO3 nanorods are prepared according to the following steps: Na2WO4·2H2O and citric acid are mixed in water, the pH of the solution is adjusted to 1.5-2.0, a hydrothermal reaction is performed, and then centrifugation and drying are performed to obtain WO3 nanorods;
[0011] The mass ratio of Na2WO4·2H2O to citric acid is 10-12:1, 1.0 mol / L hydrochloric acid solution is used to adjust the pH, and the conditions of the hydrothermal reaction are: hydrothermal reaction at 150-200°C for 8-16h.
[0012] Preferably, the KNbO3 microblock is prepared by a hydrothermal method, and the specific steps are: dispersing Nb2O5 in a KOH solution, stirring and mixing to obtain a suspension, subjecting the suspension to a hydrothermal reaction, and then centrifuging and drying to obtain a KNbO3 microblock;
[0013] The mass ratio of KOH to Nb2O5 is 55:2-7, and the conditions of the hydrothermal reaction are: hydrothermal reaction at 140-180°C for 10-16h.
[0014] Preferably, the soluble silver salt is selected from silver nitrate or silver chloride; the concentration of the soluble silver salt is 1 mg / mL, and the mass ratio of WO3 nanorods, KNbO3 microblocks, and silver nitrate is 1:0.1-0.2:10-30.
[0015] Preferably, the conditions for the photochemical reaction are: stirring the reaction for 8-10 hours under the irradiation of a xenon lamp, so that WO3 and the soluble silver salt undergo sufficient photochemical reduction reaction.
[0016] Preferably, the annealing conditions are: annealing at 400-500° C. for 2-3 h in an inert atmosphere.
[0017] Preferably, in the KNbO3 / Ag@WO3 composite photocatalyst, Ag@WO3 is loaded on KNbO3, and Ag@WO3 is coated on the surface of KNbO3 microblocks.
[0018] The present invention also protects the use of the above-mentioned KNbO3 / Ag@WO3 composite photocatalyst in the preparation of a photodegradation catalyst for phenol, and uses the KNbO3 / Ag@WO3 composite photocatalyst to photocatalytically degrade phenol under light conditions.
[0019] Preferably, the application method is: adding the KNbO3 / Ag@WO3 composite photocatalyst to the wastewater containing phenol, then stirring and catalytically degrading under light conditions, extracting the supernatant after a certain period of degradation, and using the photometric method to detect the change in the absorbance of phenol at 510nm over time;
[0020] In the process of photocatalytic degradation, H2O2 can also be used as a promoter.
[0021] Compared with the prior art, the present invention has the following beneficial effects:
[0022] 1. The present invention adopts a photochemical reaction method to prepare Ag@WO3 material, that is, a semiconductor-metal nanocomposite material. On the one hand, by using Ag to promote the photocatalytic performance of WO3 material, Ag@WO3 material has good charge separation ability. In addition, by introducing precious metal Ag to modify semiconductor WO3, charge separation is improved and the interfacial charge transfer process is promoted. This is because the charge accumulation in the Ag layer leads to Fermi level balance, making the quasi-Fermi level of the composite material close to the conduction band energy level of the oxidized semiconductor. On the other hand, due to the reduction of the electron-hole recombination rate, Ag@WO3 exhibits higher light efficiency, and due to the plasma effect generated by Ag nanoparticles, their absorption is expanded to the visible region of the solar spectrum.
[0023] In addition, Ag also provides more active sites for photocatalysis, which overcomes the technical defects of WO3 to a certain extent and improves the comprehensive performance of KNbO3 / Ag@WO3 composite photocatalyst.
[0024] 2. In the present invention, KNbO3 and Ag@WO3 are used for compounding, and during the annealing process, Ag@WO3 is tightly coated on the outer surface of KNbO3. The band gap of WO3 is more negative than the energy level of KNbO3. When WO3 is combined with KNbO3, a WO3 / KNbO3 heterojunction is formed at the interface of WO3 and KNbO3 materials. The heterojunction helps to promote the separation and migration of photogenerated electron-hole pairs; and WO3 loaded on the surface of KNbO3 will also broaden the light absorption range of KNbO3.
[0025] 3. The KNbO3 / Ag@WO3 composite photocatalytic material prepared by the present invention greatly improves the activity of photocatalytic decomposition of phenol, and solves the problem of poor photocatalytic activity of WO3 and KNbO3 in the prior art; the prepared KNbO3 / Ag@WO3 composite photocatalyst has good application prospects and industrialization prospects in the fields of environmental remediation and energy.
[0026] 4. The preparation method of the present invention is simple, and after a photochemical reaction, compounding is achieved in one step. The experimental conditions are easy to control, the cost is low, and it is safe and reliable, and suitable for large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 These are the X-ray diffraction patterns of KNbO3, WO3, the KNbO3 / Ag@WO3 composite photocatalyst of Example 1, and the Ag@WO3 photocatalyst of Comparative Example 1.
[0028] Figure 2 These are the UV-visible absorption graphs of KNbO3, WO3, the KNbO3 / Ag@WO3 composite photocatalyst of Example 1, and the Ag@WO3 photocatalyst of Comparative Example 1.
[0029] Figure 3 This is a comparison chart of the photodegradation efficiencies of KNbO3, WO3, the KNbO3 / Ag@WO3 composite photocatalyst of Example 1, and the Ag@WO3 photocatalyst of Comparative Example 1.
[0030] Figure 4 This is a comparison chart of the photodegradation kinetics of the KNbO3 / Ag@WO3 composite photocatalyst of Example 1. DETAILED DESCRIPTION
[0031] The specific embodiments of the present invention are described in detail below, but it should be understood that the protection scope of the present invention is not limited by the specific embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work belong to the protection scope of the present invention. The experimental methods described in the embodiments of the present invention are conventional methods unless otherwise specified.
[0032] Example 1
[0033] The preparation method of KNbO3 / Ag@WO3 composite photocatalyst comprises the following steps:
[0034] Preparation of S1. WO3 nanorods: 240 mg of Na2WO4·2H2O and 20 mg of citric acid were added to 9 mL of secondary water, stirred for 6 h, and then the pH value of the solution was adjusted to 1.5 with 1.0 mol / L HCl to obtain a mixed solution;
[0035] The mixed solution was transferred into a 25 mL stainless steel autoclave and subjected to a hydrothermal reaction at 170 °C for 12 h, followed by natural cooling. The prepared material was washed several times with secondary water and ethanol, and then dried at 60 °C for 5 h to obtain WO3 nanorods.
[0036] Preparation of S2 and KNbO3 microblocks:
[0037] 55 g of KOH was added to 50 mL of deionized water and stirred to dissolve, and then 5 g of Nb2O5 was dispersed in the KOH solution and magnetically stirred for 1 h to obtain a suspension;
[0038] The suspension was transferred to a polytetrafluoroethylene-lined reactor for reaction at a temperature of 160°C for 12 hours. After the reaction, the suspension was centrifuged, washed, and collected in a forced air drying oven and dried at 80°C for 12 hours to obtain KNbO3 microblocks.
[0039] Preparation of S3, KNbO3 / Ag@WO3 composite photocatalyst:
[0040] WO3 nanorods and KNbO3 microblocks were used as raw materials. The WO3 nanorods and KNbO3 microblocks were mixed with a silver nitrate solution, and a photochemical reaction was first carried out for 9 hours under the irradiation of a xenon lamp. After the photochemical reaction, centrifugation and drying were performed in sequence, and then annealing was performed at 400°C for 3 hours under an inert atmosphere to obtain a KNbO3 / Ag@WO3 composite photocatalyst.
[0041] The concentration of the silver nitrate solution is 1 mg / mL, and the mass ratio of WO3 nanorods, KNbO3 microblocks, and silver nitrate is 1:0.2:20.
[0042] Example 2
[0043] The preparation method of KNbO3 / Ag@WO3 composite photocatalyst comprises the following steps:
[0044] Preparation of S1. WO3 nanorods: 220 mg of Na2WO4·2H2O and 20 mg of citric acid were added to 9 mL of secondary water, stirred for 6 h, and then the pH value of the solution was adjusted to 2.0 with 1.0 mol / L HCl to obtain a mixed solution;
[0045] The obtained mixed solution was transferred into a 25 mL stainless steel autoclave and subjected to a hydrothermal reaction at 150 °C for 16 h, followed by natural cooling. The prepared material was washed several times with secondary water and ethanol, and then dried at 60 °C for 5 h to obtain WO3 nanorods.
[0046] Preparation of S2 and KNbO3 microblocks:
[0047] Add 55 g of KOH to 50 mL of deionized water and stir to dissolve. Then disperse 7 g of Nb2O5 in the KOH solution and stir magnetically for 1 h to obtain a suspension.
[0048] The suspension was transferred to a polytetrafluoroethylene-lined reactor for reaction at a temperature of 180°C for 10 hours. After the reaction, the suspension was centrifuged, washed, and collected in a forced air drying oven and dried at 80°C for 12 hours to obtain KNbO3 microblocks.
[0049] Preparation of S3, KNbO3 / Ag@WO3 composite photocatalyst:
[0050] WO3 nanorods and KNbO3 microblocks were used as raw materials. The WO3 nanorods and KNbO3 microblocks were mixed with a silver nitrate solution, and a photochemical reaction was first carried out for 8 hours under the irradiation of a xenon lamp. After the photochemical reaction, centrifugation and drying were performed in sequence, and then annealing was performed at 450°C for 2.5 hours under an inert atmosphere to obtain a KNbO3 / Ag@WO3 composite photocatalyst.
[0051] The concentration of the silver nitrate solution is 1 mg / mL, and the mass ratio of WO3 nanorods, KNbO3 microblocks, and silver nitrate is 1:0.1:10.
[0052] Example 3
[0053] The preparation method of KNbO3 / Ag@WO3 composite photocatalyst comprises the following steps:
[0054] Preparation of S1. WO3 nanorods: 200 mg of Na2WO4·2H2O and 20 mg of citric acid were added to 9 mL of secondary water, stirred for 6 h, and then the pH value of the solution was adjusted to 2.0 with 1.0 mol / L HCl to obtain a mixed solution;
[0055] The obtained mixed solution was transferred into a 25 mL stainless steel autoclave and subjected to a hydrothermal reaction at 200 °C for 8 h, followed by natural cooling. The prepared material was washed several times with secondary water and ethanol, and then dried at 60 °C for 5 h to obtain WO3 nanorods.
[0056] Preparation of S2 and KNbO3 microblocks:
[0057] Add 55 g of KOH to 50 mL of deionized water and stir to dissolve. Then disperse 2 g of Nb2O5 in the KOH solution and stir magnetically for 1 h to obtain a suspension.
[0058] The suspension was transferred to a polytetrafluoroethylene-lined reactor for reaction at a temperature of 140°C for 16 hours. After the reaction, the suspension was centrifuged, washed, and collected in a forced air drying oven and dried at 80°C for 12 hours to obtain KNbO3 microblocks.
[0059] Preparation of S3, KNbO3 / Ag@WO3 composite photocatalyst:
[0060] WO3 nanorods and KNbO3 microblocks were used as raw materials. The WO3 nanorods and KNbO3 microblocks were mixed with a silver nitrate solution, and a photochemical reaction was first carried out for 8 hours under the irradiation of a xenon lamp. After the photochemical reaction, centrifugation and drying were performed in sequence, and then annealing was performed at 500°C for 2 hours under an inert atmosphere to obtain a KNbO3 / Ag@WO3 composite photocatalyst.
[0061] The concentration of the silver nitrate solution is 1 mg / mL, and the mass ratio of WO3 nanorods, KNbO3 microblocks, and silver nitrate is 1:0.15:30.
[0062] Comparative Example 1
[0063] The preparation steps of this comparative example are the same as those of Example 1, except that the Ag@WO3 photocatalyst is prepared without compounding with KNbO3 microblocks. The preparation method includes the following steps:
[0064] Preparation of S1. WO3 nanorods: 240 mg of Na2WO4·2H2O and 20 mg of citric acid were added to 9 mL of secondary water, stirred for 6 h, and then the pH value of the solution was adjusted to 1.5 with 1.0 mol / L HCl to obtain a mixed solution;
[0065] The mixed solution was transferred into a 25 mL stainless steel autoclave and subjected to a hydrothermal reaction at 170 °C for 12 h, followed by natural cooling. The prepared material was washed several times with secondary water and ethanol, and then dried at 60 °C for 5 h to obtain WO3 nanorods.
[0066] Preparation of S2 and Ag@WO3 photocatalysts:
[0067] Using WO3 nanorods as raw materials, WO3 nanorods were mixed with silver nitrate solution, and stirred under xenon lamp for 9 hours of photochemical reaction. After the photochemical reaction, they were centrifuged and dried in sequence, and then annealed at 400°C for 3 hours under an inert atmosphere to obtain Ag@WO3 photocatalyst.
[0068] The concentration of the silver nitrate solution is 1 mg / mL, and the mass ratio of WO3 nanorods to silver nitrate is 1:20.
[0069] Examples 1-3 of the present invention all prepared KNbO3 / Ag@WO3 composite photocatalysts with excellent photocatalytic degradation performance of phenol. The material prepared in Example 1 is taken as an example, and compared with the WO3 nanorods, KNbO3 microblocks prepared in Example 1 and the Ag@WO3 photocatalyst prepared in Comparative Example 1. The specific research methods and results are as follows:
[0070] (1)Structure confirmation:
[0071] Figure 1 The X-ray diffraction patterns of KNbO3, WO3, KNbO3 / Ag@WO3 of Example 1, and Ag@WO3 of Comparative Example 1 are shown. XRD is used to characterize the phase and composition of the material. Figure 1 It can be seen that in the XRD spectrum of the KNbO3 / Ag@WO3 composite photocatalyst, the diffraction peaks of Ag@WO3 and KNbO3 both exist, indicating that the target product is obtained.
[0072] (2) Photodegradation performance test:
[0073] S1. Prepare phenol wastewater with a mass volume ratio of 10 mg / L, and add 50 mg of the KNbO3 / Ag@WO3 composite photocatalyst of Example 1 and 1 mL of hydrogen peroxide with a volume fraction of 30% (hydrogen peroxide is a promoter of photocatalytic degradation) to 100 mL of phenol wastewater, place it in a dark place and stir it for 30 minutes to reach adsorption-desorption equilibrium, then place it in a photochemical reaction device and use a 300W xenon lamp light source for illumination, the xenon lamp is located 12 cm above the liquid surface, and irradiate for 3 hours;
[0074] S2. During the degradation process, 4 mL of the reaction solution was taken every 10 minutes, and the catalyst was removed by high-speed centrifugation in a centrifuge. The supernatant was used to analyze the concentration of the pollutant phenol;
[0075] S3. Use the photometric method on a TU-1810 UV-visible spectrophotometer and use the colorimetric method to take 1 mL of the supernatant, then add the prepared 0.5 mL of NH4Cl-NH3·H2O buffer solution (measured in g / mL, with a mass fraction of 20%; the ammonia water is selected from concentrated ammonia water), 1 mL of 4-aminoantipyrine aqueous solution (measured in g / mL, with a mass fraction of 2%), and 1 mL of potassium ferrocyanide aqueous solution (measured in g / mL, with a mass fraction of 8%), then add water to make the volume to a 25 mL colorimetric tube, and then measure its absorbance, and the measured wavelength is 510 nm; according to the Lambert-Beer law, the concentration of the degradation product is proportional to its absorbance, and its corresponding concentration is calculated by the standard curve method.
[0076] Figure 2 It shows that pure KNbO3 has strong light absorption only in the ultraviolet region, while WO3, Ag@WO3 composite photocatalyst and KNbO3 / Ag@WO3 composite photocatalyst all have light absorption in the visible light range. It is worth noting that the KNbO3 / Ag@WO3 composite photocatalyst exhibits the strongest light absorption in the visible light range, so the composite of KNbO3 and Ag@WO3 helps to enhance the light absorption and photocatalytic activity of KNbO3.
[0077] Figure 3 is a comparison chart of the photodegradation activity of phenol. Figure 3 It can be seen that pure KNbO3 can hardly remove phenol, because pure KNbO3 has poor light absorption ability and can hardly generate photogenerated carriers; pure WO3 has a slightly higher degradation ability for phenol than pure KNbO3, and can decompose about 16.2% of phenol within 60 minutes, which is due to the wider light response of WO3 than KNbO3. Compared with pure KNbO3 catalyst, pure WO3 catalyst, Ag@WO3 composite photocatalyst and KNbO3 / Ag@WO3 composite photocatalyst, the prepared KNbO3 / Ag@WO3 composite photocatalyst has the highest removal rate for phenol. After 200 minutes of photocatalytic reaction, the removal rates of phenol by pure KNbO3 catalyst, pure WO3 catalyst, Ag@WO3 composite photocatalyst and KNbO3 / Ag@WO3 composite photocatalyst were 16.24%, 25.16%, 35.72% and 92.75%, respectively.
[0078] (3) Reaction kinetics study:
[0079] The photodegradation of phenol by KNbO3 / Ag@WO3 composite photocatalyst was studied using the Langmuire-Hinshelwood model. According to the LH model, the reaction rate can be expressed as:
[0080] Where Kr is the apparent rate constant, Ka is the adsorption equilibrium constant, Co is the initial concentration of the reactant,
[0081] r=K r K a C0
[0082] If KrCo<<1, the above formula is simplified to:
[0083] According to the equation, the first-order reaction kinetics of the photodegradation of phenol by KNbO3 / Ag@WO3 composite photocatalyst and H2O2 under visible light irradiation was considered. The results are as follows Figure 4 As shown, the results show that the photodegradation of phenol by KNbO3 / Ag@WO3 composite photocatalyst and H2O2 conforms to LH pseudo-first-order kinetics.
[0084] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations. The above-mentioned embodiments are only preferred embodiments for fully illustrating the present invention, and the protection scope thereof is not limited thereto.
Claims
1. Application of KNbO3 / Ag@WO3 composite photocatalyst in photocatalytic degradation of phenol, characterized in that: The preparation method of the KNbO3 / Ag@WO3 composite photocatalyst comprises the following steps: Preparation of WO3 nanorods and KNbO3 microblocks; Using WO3 nanorods and KNbO3 microblocks as raw materials, WO3 nanorods, KNbO3 microblocks and soluble silver salt solution were mixed, photochemical reaction was first carried out under xenon lamp irradiation, and then annealed in an inert atmosphere to obtain KNbO3 / Ag@WO3 composite photocatalyst.
2. The use of the KNbO3 / Ag@WO3 composite photocatalyst according to claim 1 in photocatalytic degradation of phenol, characterized in that: The concentration of the soluble silver salt solution is 1 mg / mL, and the mass ratio of WO3 nanorods, KNbO3 microblocks, and soluble silver salt is 1:0.1-0.2:10-30.
3. The use of the KNbO3 / Ag@WO3 composite photocatalyst according to claim 1 in photocatalytic degradation of phenol, characterized in that: The conditions for the photochemical reaction are: stirring the reaction for 8-10 hours under xenon lamp irradiation.
4. The use of the KNbO3 / Ag@WO3 composite photocatalyst according to claim 1 in photocatalytic degradation of phenol, characterized in that: The annealing conditions are: annealing at 400-500° C. for 2-3 h in an inert atmosphere.
5. The use of the KNbO3 / Ag@WO3 composite photocatalyst according to claim 1 in photocatalytic degradation of phenol, characterized in that: The WO3 nanorods are prepared according to the following steps: Na2WO4·2H2O and citric acid are mixed in water, the pH of the solution is adjusted to 1.5-2.0, and a hydrothermal reaction is performed to obtain the WO3 nanorods.
6. The use of the KNbO3 / Ag@WO3 composite photocatalyst according to claim 1 in photocatalytic degradation of phenol, characterized in that: The KNbO3 microblock is prepared by a hydrothermal method, and the specific steps are: dispersing Nb2O5 in a KOH solution, stirring and mixing to obtain a suspension, and subjecting the suspension to a hydrothermal reaction to obtain a KNbO3 microblock.
7. Use of the KNbO3 / Ag@WO3 composite photocatalyst according to any one of claims 1 to 6 in photocatalytic degradation of phenol, characterized in that: In the KNbO3 / Ag@WO3 composite photocatalyst, Ag@WO3 is loaded on KNbO3, and Ag@WO3 is coated on the surface of KNbO3 microblocks.
8. The use of the KNbO3 / Ag@WO3 composite photocatalyst according to claim 1 in photocatalytic degradation of phenol, characterized in that: The application method is: adding the KNbO3 / Ag@WO3 composite photocatalyst to the wastewater containing phenol, and then stirring and catalytically degrading it under light conditions.
9. The use of the KNbO3 / Ag@WO3 composite photocatalyst according to claim 8 in photocatalytic degradation of phenol, characterized in that: The lighting conditions are: 300-600W xenon lamp irradiation for 1-4h.