A nucleating agent for improving the cell density of supercritical physical foaming PET and a preparation method thereof

By preparing a core agent consisting of polymer base material, functional additives, etc., the problems of cell density and temperature resistance in PET foam material were solved, and the cell density and temperature resistance were improved.

CN118085511BActive Publication Date: 2024-11-05WEISAI (JIANGSU) COMPOSITE MATERIALS TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410128185.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-30
Publication Date
2024-11-05
Estimated Expiration
2044-01-30

AI Technical Summary

Technical Problem

Existing nucleating agents used in PET foam materials suffer from problems such as large cell size, low and uneven density, and limited functionality.

Method used

A core agent is used, which is composed of polymer base material, functional additives, sodium bicarbonate, synergistic additives, lubricants and dispersants, etc., and is prepared through steps such as ultrasonic dispersion, stirring and vacuum drying to improve the cell density and temperature resistance.

Benefits of technology

It significantly improves the cell density of PET and enhances the temperature resistance of PET foam materials, thus offering broader market prospects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118085511B_ABST
    Figure CN118085511B_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of nucleating agent production, in particular to a nucleating agent for improving the cell density of supercritical physical foaming PET and a preparation method thereof; the nucleating agent is prepared from the following raw materials in parts by weight: 20 to 30 parts of polymer base material, 10 to 12 parts of functional additives, 10 to 14 parts of sodium bicarbonate, 6 to 10 parts of synergistic additives, 5 to 7 parts of lubricants, 3 to 5 parts of dispersants and 30 to 40 parts of ethyl acetate; the nucleating agent prepared by the invention is prepared by ultrasonically dispersing the polymer base material in ethyl acetate, adding sodium bicarbonate and stirring, then heating, sampling, filtering, and washing with deionized water, vacuum drying the obtained product to obtain a pre-product, pre-dispersing the pre-product, the functional additive, the lubricant and the dispersant, and banburying and granulating the obtained product to obtain the nucleating agent; the prepared nucleating agent for improving the cell density of supercritical physical foaming PET can not only effectively improve the cell density, but also has the effect of improving the temperature resistance of PET foaming materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of nucleating agent production, in particular to a nucleating agent for improving the cell density of supercritical physical foaming PET and a preparation method thereof. Background Art

[0002] PET is a thermoplastic with excellent performance. It has high melting temperature (Tm) and glass transition temperature (Tg). It has good heat resistance, fatigue resistance, friction and wear resistance, creep resistance, electrical insulation and chemical resistance. It is cheaper than other engineering plastics and is widely used in synthetic fibers, films, engineering plastics, medicines and daily necessities.

[0003] Adding nucleating agents to PET foaming materials can introduce a large number of evenly distributed low potential energy hot spots, and then to stable bubble nuclei. Therefore, adding nucleating agents can effectively increase the cell density. However, existing nucleating agents, such as nano-silica, aminosilica, talcum powder and other nucleating agents, have problems such as large cell size, low cell density, uneven bubble size, and single function. Therefore, how to effectively improve the performance of existing nucleating agents has become an important issue that the PET foaming industry cannot avoid.

[0004] Therefore, the present invention provides a nucleating agent for improving the cell density of supercritical physical foaming PET and a preparation method thereof, which are used to solve the above-mentioned related technical problems. Summary of the invention

[0005] The object of the present invention is to provide a nucleating agent for improving the cell density of supercritical physical foaming PET and a preparation method thereof. The nucleating agent for improving the cell density of supercritical physical foaming PET prepared by the present invention can not only effectively improve the cell density, but also has the effect of improving the temperature resistance of PET foaming materials.

[0006] To achieve the above object, the present invention provides the following technical solutions:

[0007] The first aspect of the present invention provides a core agent for improving the cell density of supercritical physical foaming PET, wherein the core agent is made of the following raw materials in parts by weight: 20 to 30 parts of a polymer base material, 10 to 12 parts of a functional additive, 10 to 14 parts of sodium bicarbonate, 6 to 10 parts of a synergistic additive, 5 to 7 parts of a lubricant, 3 to 5 parts of a dispersant and 30 to 40 parts of ethyl acetate.

[0008] The present invention is further configured as follows: the preparation process of the polymer base material is as follows:

[0009] Ultrasonic dispersion of an appropriate amount of the composite material in an appropriate amount of N,N-dimethylformamide at a solid-liquid ratio of 0.02 to 0.05 g / mL for 20 to 30 minutes to obtain a dispersion;

[0010] After the polyethylene terephthalate is melted, the dispersion is added dropwise to the melted polyethylene terephthalate at a solid-liquid ratio of 0.012 to 0.022 g / mL, and the mixture is reacted at this temperature for 8 to 10 minutes;

[0011] After the reaction is completed, the obtained product is vacuum dried at a temperature of 60 to 70° C. for 12 to 14 minutes to obtain a dry product;

[0012] An appropriate amount of aminosilicone oil is placed in an appropriate amount of ethylene glycol at a volume ratio of 0.2 to 0.4:1 and mixed thoroughly to obtain an aminosilicone oil mixture. An appropriate amount of dry product is placed in the aminosilicone oil mixture at a solid-liquid ratio of 0.024 to 0.036 g / mL, and treated at 120 to 130°C for 3 to 4 hours. After cooling to 60°C, it is precipitated and filtered in an appropriate amount of 6°C acetone, and then washed with 6°C acetone for 4 to 6 times. After washing, it is vacuum dried at 60 to 70°C for 12 to 14 minutes to obtain a polymer base material.

[0013] The present invention is further configured as follows: the composite material is prepared by mixing crotonic acid, styrene and dicumyl peroxide in a mass ratio of 0.3-0.6:0.5-0.8:1.

[0014] The present invention is further configured as follows: the preparation process of the functional additive is as follows:

[0015] Place an appropriate amount of silane coupling agent KH560 in an appropriate amount of 10% ethanol aqueous solution at a volume ratio of 0.12 to 0.22:1, mix thoroughly, adjust the pH value to 4, seal and let stand for 60 to 70 minutes to obtain a standing solution;

[0016] Place an appropriate amount of functional material in an appropriate amount of static liquid at a solid-liquid ratio of 0.045-0.055:1, heat it to 70-72°C, stir it at 80-100r / min for 20-24h, filter it, rinse it with deionized water 2-4 times, and dry it in a drying oven at 70°C for 26h to obtain a functional additive.

[0017] The present invention is further configured as follows: the functional material is prepared by mixing hydrotalcite and montmorillonite in a mass ratio of 0.4 to 0.6:1.

[0018] The present invention is further configured as follows: the synergistic aid is prepared by mixing triethylenetetramine, sodium dodecylbenzenesulfonate and 2,4,6-tris(dimethylaminomethyl)phenol in a mass ratio of 0.2-0.4:0.3-0.7:1.

[0019] The present invention is further configured as follows: the lubricant is selected from any one of zinc stearate and calcium stearate.

[0020] The present invention is further configured as follows: the dispersant is selected from any one of stearamide and hexenyl bisstearamide.

[0021] The second aspect of the present invention: also provides a method for preparing the above-mentioned nucleating agent for improving the cell density of supercritical physical foaming PET, comprising the following steps:

[0022] Step 1, accurately weigh the polymer base material, functional additive, sodium bicarbonate, synergist, lubricant, dispersant and ethyl acetate respectively, then ultrasonically disperse the polymer base material in ethyl acetate for 20 to 30 minutes, then add sodium bicarbonate, and stir at 450 to 550 r / min and room temperature for 20 to 30 minutes, then add the synergist, continue stirring for 15 to 17 minutes, then heat to 60°C for 300 to 320 minutes, take samples, filter, rinse with deionized water for 3 to 7 times, and place the obtained product in a vacuum drying oven at 60°C for 24 hours to obtain a pre-product;

[0023] Step 2: pre-disperse the pre-product, functional additives, lubricants and dispersants, and obtain the core agent by mixing and granulating the obtained product.

[0024] Compared with the prior art, the present invention has the following beneficial effects:

[0025] The core agent for improving the cell density of supercritical physical foaming PET prepared by the present invention is made of polymer base material, functional additive, sodium bicarbonate, synergistic additive, lubricant, dispersant and ethyl acetate as raw materials, and the polymer base material is ultrasonically dispersed in ethyl acetate, and sodium bicarbonate is added for stirring, and then the temperature is raised, and after sampling and suction filtration, it is rinsed with deionized water, and the obtained product is vacuum dried to obtain a pre-product, and the pre-product, functional additive, lubricant and dispersant are pre-dispersed, and the obtained product is subjected to banburying and granulation to obtain a core agent; the prepared core agent for improving the cell density of supercritical physical foaming PET can not only effectively improve the cell density; but also has the function of improving the temperature resistance of PET foaming materials. The core agent for improving the cell density of supercritical physical foaming PET prepared by the present invention has a broader market prospect and is more suitable for promotion. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0027] Figure 1 It is a statistical diagram of the cell density of the present invention;

[0028] Figure 2 It is a statistical diagram of the highest temperature resistance of the present invention. DETAILED DESCRIPTION

[0029] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0030] Example 1

[0031] The present embodiment provides a core agent for improving the cell density of supercritical physical foaming PET, wherein the core agent is made of the following raw materials in parts by weight: 20 parts of a polymer base material, 10 parts of a functional additive, 10 parts of sodium bicarbonate, 6 parts of a synergistic additive, 5 parts of a lubricant, 3 parts of a dispersant and 30 parts of ethyl acetate.

[0032] The preparation process of the polymer base material is as follows:

[0033] An appropriate amount of the composite material was ultrasonically dispersed in an appropriate amount of N,N-dimethylformamide at a solid-liquid ratio of 0.02 g / mL for 20 min to obtain a dispersion;

[0034] After the polyethylene terephthalate is melted, the dispersion is added dropwise to the melted polyethylene terephthalate at a solid-liquid ratio of 0.012 g / mL, and the mixture is reacted at this temperature for 8 minutes;

[0035] After the reaction is completed, the obtained product is vacuum dried at 60°C for 12 min to obtain a dry product;

[0036] An appropriate amount of aminosilicone oil is placed in an appropriate amount of ethylene glycol at a volume ratio of 0.2:1 and mixed thoroughly to obtain an aminosilicone oil mixture. An appropriate amount of dry product is placed in the aminosilicone oil mixture at a solid-liquid ratio of 0.024 g / mL, and treated at 120°C for 3 h. After cooling to 60°C, it is precipitated and filtered in an appropriate amount of 6°C acetone, and then washed with 6°C acetone for 4 times. After washing, it is vacuum dried at 60°C for 12 min to obtain a polymer base material.

[0037] Furthermore, the composite material is prepared by mixing crotonic acid, styrene and dicumyl peroxide in a mass ratio of 0.3:0.5:1.

[0038] It should be noted that the amino silicone oil was purchased from Shandong Xinrunjin Chemical Co., Ltd.

[0039] In addition, the preparation process of the functional additive is as follows:

[0040] Place an appropriate amount of silane coupling agent KH560 in an appropriate amount of 10% ethanol aqueous solution at a volume ratio of 0.12:1 and mix thoroughly, adjust the pH value to 4, seal and let stand for 60 minutes to obtain a standing solution;

[0041] An appropriate amount of functional material was placed in an appropriate amount of static liquid at a solid-liquid ratio of 0.045:1, and the temperature was raised to 70°C. Stirring was carried out at 80 r / min for 20 hours. After filtration, the mixture was rinsed with deionized water twice and dried in a drying oven at 70°C for 26 hours to obtain a functional additive.

[0042] Furthermore, the functional material is prepared by mixing hydrotalcite and montmorillonite in a mass ratio of 0.4:1.

[0043] It should be noted that hydrotalcite was purchased from Wuhan Lanabai Pharmaceutical Chemical Co., Ltd., and montmorillonite was purchased from Zhejiang Huate New Materials Co., Ltd.

[0044] In addition, the synergistic aid is prepared by mixing triethylenetetramine, sodium dodecylbenzene sulfonate and 2,4,6-tris(dimethylaminomethyl)phenol in a mass ratio of 0.2:0.3:1.

[0045] Zinc stearate is used as lubricant.

[0046] The dispersant is stearamide.

[0047] In addition, this embodiment also provides a method for preparing the above-mentioned nucleating agent for improving the cell density of supercritical physical foaming PET, comprising the following steps:

[0048] Step 1, accurately weigh the polymer base material, functional additive, sodium bicarbonate, synergist, lubricant, dispersant and ethyl acetate respectively, then ultrasonically disperse the polymer base material in ethyl acetate for 20 minutes, then add sodium bicarbonate, and stir at 450r / min and room temperature for 20 minutes, then add the synergist, continue stirring for 15 minutes, then heat to 60°C for 300 minutes, take samples, filter, rinse with deionized water 3 times, and place the obtained product in a vacuum drying oven at 60°C for 24 hours to obtain a pre-product;

[0049] Step 2: pre-disperse the pre-product, functional additives, lubricants and dispersants, and obtain the core agent by mixing and granulating the obtained product.

[0050] Example 2

[0051] The present embodiment provides a core agent for improving the cell density of supercritical physical foaming PET, wherein the core agent is made of the following raw materials in parts by weight: 25 parts of a polymer base material, 11 parts of a functional additive, 12 parts of sodium bicarbonate, 8 parts of a synergistic additive, 6 parts of a lubricant, 4 parts of a dispersant and 35 parts of ethyl acetate.

[0052] The preparation process of the polymer base material is as follows:

[0053] An appropriate amount of the composite material was ultrasonically dispersed in an appropriate amount of N,N-dimethylformamide at a solid-liquid ratio of 0.03 g / mL for 25 min to obtain a dispersion;

[0054] After the polyethylene terephthalate is melted, the dispersion is added dropwise to the melted polyethylene terephthalate at a solid-liquid ratio of 0.017 g / mL, and the mixture is reacted at this temperature for 9 minutes;

[0055] After the reaction was completed, the obtained product was vacuum dried at 65°C for 13 min to obtain a dry product;

[0056] An appropriate amount of aminosilicone oil is placed in an appropriate amount of ethylene glycol at a volume ratio of 0.3:1 and mixed thoroughly to obtain an aminosilicone oil mixture. An appropriate amount of dry product is placed in the aminosilicone oil mixture at a solid-liquid ratio of 0.03 g / mL, and treated at 125°C for 4 hours. After cooling to 60°C, it is precipitated and filtered in an appropriate amount of 6°C acetone, and then washed with 6°C acetone for 5 times. After washing, it is vacuum dried at 65°C for 13 minutes to obtain a polymer base material.

[0057] Furthermore, the composite material is prepared by mixing crotonic acid, styrene and dicumyl peroxide in a mass ratio of 0.4:0.6:1.

[0058] It should be noted that the amino silicone oil was purchased from Shandong Xinrunjin Chemical Co., Ltd.

[0059] In addition, the preparation process of the functional additive is as follows:

[0060] Place an appropriate amount of silane coupling agent KH560 in an appropriate amount of 10% ethanol aqueous solution at a volume ratio of 0.17:1 and mix thoroughly, adjust the pH value to 4, seal and let stand for 65 minutes to obtain a standing solution;

[0061] An appropriate amount of functional material was placed in an appropriate amount of static liquid at a solid-liquid ratio of 0.05:1, and the temperature was raised to 71°C. The mixture was stirred at 90 r / min for 22 hours. After filtration, the mixture was rinsed with deionized water for 3 times and dried in a drying oven at 70°C for 26 hours to obtain a functional additive.

[0062] Furthermore, the functional material is prepared by mixing hydrotalcite and montmorillonite in a mass ratio of 0.5:1.

[0063] It should be noted that hydrotalcite was purchased from Wuhan Lanabai Pharmaceutical Chemical Co., Ltd., and montmorillonite was purchased from Zhejiang Huate New Materials Co., Ltd.

[0064] In addition, the synergistic additive is prepared by mixing triethylenetetramine, sodium dodecylbenzenesulfonate and 2,4,6-tris(dimethylaminomethyl)phenol in a mass ratio of 0.3:0.5:1.

[0065] Calcium stearate is used as lubricant.

[0066] The dispersant is hexenyl bis stearamide.

[0067] In addition, this embodiment also provides a method for preparing the above-mentioned nucleating agent for improving the cell density of supercritical physical foaming PET, comprising the following steps:

[0068] Step 1, accurately weigh the polymer base material, functional additive, sodium bicarbonate, synergist, lubricant, dispersant and ethyl acetate respectively, then ultrasonically disperse the polymer base material in ethyl acetate for 25 minutes, then add sodium bicarbonate, and stir at 500r / min and room temperature for 25 minutes, then add the synergist, continue stirring for 16 minutes, then heat to 60°C for 310 minutes, take samples, filter, rinse with deionized water 5 times, and place the obtained product in a vacuum drying oven at 60°C for 24 hours to obtain a pre-product;

[0069] Step 2: pre-disperse the pre-product, functional additives, lubricants and dispersants, and obtain the core agent by mixing and granulating the obtained product.

[0070] Example 3

[0071] The present embodiment provides a core agent for improving the cell density of supercritical physical foaming PET, wherein the core agent is made of the following raw materials in parts by weight: 30 parts of a polymer base material, 12 parts of a functional additive, 14 parts of sodium bicarbonate, 10 parts of a synergistic additive, 7 parts of a lubricant, 5 parts of a dispersant and 40 parts of ethyl acetate.

[0072] The preparation process of the polymer base material is as follows:

[0073] An appropriate amount of the composite material was ultrasonically dispersed in an appropriate amount of N,N-dimethylformamide at a solid-liquid ratio of 0.05 g / mL for 30 min to obtain a dispersion;

[0074] After the polyethylene terephthalate is melted, the dispersion is added dropwise to the melted polyethylene terephthalate at a solid-liquid ratio of 0.022 g / mL, and the mixture is reacted at this temperature for 10 minutes;

[0075] After the reaction was completed, the obtained product was vacuum dried at 70°C for 14 min to obtain a dry product;

[0076] An appropriate amount of aminosilicone oil is placed in an appropriate amount of ethylene glycol at a volume ratio of 0.4:1 and mixed thoroughly to obtain an aminosilicone oil mixture. An appropriate amount of dry product is placed in the aminosilicone oil mixture at a solid-liquid ratio of 0.036 g / mL, and treated at 130°C for 4 hours. After cooling to 60°C, it is precipitated and filtered in an appropriate amount of 6°C acetone, and then washed with 6°C acetone for 6 times. After washing, it is vacuum dried at 70°C for 14 minutes to obtain a polymer base material.

[0077] Furthermore, the composite material is prepared by mixing crotonic acid, styrene and dicumyl peroxide in a mass ratio of 0.6:0.8:1.

[0078] It should be noted that the amino silicone oil was purchased from Shandong Xinrunjin Chemical Co., Ltd.

[0079] In addition, the preparation process of the functional additive is as follows:

[0080] Place an appropriate amount of silane coupling agent KH560 in an appropriate amount of 10% ethanol aqueous solution at a volume ratio of 0.22:1 and mix thoroughly, adjust the pH value to 4, seal and let stand for 70 minutes to obtain a standing solution;

[0081] Place an appropriate amount of functional material in an appropriate amount of static liquid at a solid-liquid ratio of 0.055:1, heat it to 72°C, stir it at 80-100r / min for 24 hours, filter it, rinse it with deionized water for 4 times, and then dry it in a drying oven at 70°C for 26 hours to obtain a functional additive.

[0082] Furthermore, the functional material is prepared by mixing hydrotalcite and montmorillonite in a mass ratio of 0.6:1.

[0083] It should be noted that hydrotalcite was purchased from Wuhan Lanabai Pharmaceutical Chemical Co., Ltd., and montmorillonite was purchased from Zhejiang Huate New Materials Co., Ltd.

[0084] In addition, the synergistic aid is prepared by mixing triethylenetetramine, sodium dodecylbenzenesulfonate and 2,4,6-tris(dimethylaminomethyl)phenol in a mass ratio of 0.4:0.7:1.

[0085] Zinc stearate is used as lubricant.

[0086] The dispersant is stearamide.

[0087] In addition, this embodiment also provides a method for preparing the above-mentioned nucleating agent for improving the cell density of supercritical physical foaming PET, comprising the following steps:

[0088] Step 1, accurately weigh the polymer base material, functional additive, sodium bicarbonate, synergist, lubricant, dispersant and ethyl acetate respectively, then ultrasonically disperse the polymer base material in ethyl acetate for 30 minutes, then add sodium bicarbonate, and stir at 550r / min and room temperature for 30 minutes, then add the synergist, continue stirring for 17 minutes, then heat to 60°C for 320 minutes, take samples, filter, rinse with deionized water 7 times, and place the obtained product in a vacuum drying oven at 60°C for 24 hours to obtain a pre-product;

[0089] Step 2: pre-disperse the pre-product, functional additives, lubricants and dispersants, and obtain the core agent by mixing and granulating the obtained product.

[0090] Comparative Example 1: The preparation method of the core agent and the specific ratio of the raw materials provided in this example are substantially the same as those in Example 1, with the main difference being that polyethylene terephthalate is used instead of the polymer base material in this example.

[0091] Comparative Example 2: The preparation method of the core agent and the specific ratio of the raw materials provided in this example are substantially the same as those in Example 1, with the main difference being that this example does not contain a functional auxiliary agent.

[0092] Comparative Example 3: The preparation method of the core agent and the specific ratio of the raw materials provided in this example are substantially the same as those in Example 1, the main difference being that this example does not contain sodium bicarbonate.

[0093] Effect test

[0094] The core agents prepared by Examples 1 to 3 of the present invention are respectively recorded as Experimental Examples 1 to 3; the core agents prepared by Comparative Examples 1 to 3 are recorded as Comparative Examples 1 to 3; and then the performance of each group of core agent samples of equal amount is tested respectively.

[0095] Test 1. Cell density test and result analysis:

[0096] Each group of core agents was used to foam PET, and the process was as follows: the core agent, the auxiliary agent (glyceryl monostearate, the addition amount was 0.12% of the mass of the PET raw material) and the PET raw material were mixed evenly, and then supercritical carbon dioxide was directly extruded and foamed in an extruder. The process conditions were as follows: the temperature of each section from the feed port to the extruder outlet was set at 160°C in zone I, 160°C in zone II, and 180°C in zone III, the melt pump temperature was 180°C, the screw speed was 40r / min, and the CO2 flow injection rate was 20-40ml / min; the mass ratio of the core agent to the PET raw material was 3:100, and the foamed specimens were taken for scanning electron microscopy analysis, and the relevant data were recorded in Table 1.

[0097] Table 1: Test data record table

[0098] Group <![CDATA[Cell density (×10 8 Cell / cm 3 )]]> Example 1 Group 3.5 Example 2 Group 3.6 Example 3 Group 3.5 Comparison group 1 1.5 Comparison of 2 groups 3.0 Comparison of 3 groups 2.6

[0099] From Table 1 and Figure 1 It can be seen that compared with the control group, the core agents of Examples 1 to 3 can significantly improve the cell density; at the same time, the difference between the groups is not obvious. The above results show that the core agents of Examples 1 to 3 have a significant and effective effect of improving the cell density.

[0100] In order to verify the effects of the various components of the additive, experiments of Comparative Examples 1 to 3 were set up.

[0101] The main difference between the raw material ratio of the core agent of the comparative group 1 and the example group 1 is that polyethylene terephthalate is used instead of the polymer base material. Compared with the example group 1, it is found that the cell density of the comparative group 1 is reduced by 2×10 8 Cell / cm 3 The results indicate that the polymer matrix plays an important role in increasing the cell density.

[0102] The main difference between the raw material ratio of the core agent of the comparison group 2 and the example group 1 is that the functional additive is not included. Compared with the example group 1, the cell density of the comparison group 2 is reduced by 0.5×10 8 Cell / cm 3 The results show that functional additives play a role in improving cell density.

[0103] The main difference between the raw material ratio of the core agent of the comparison group 3 and the example group 1 is that sodium bicarbonate is not contained. Compared with the example group 1, it is found that the cell density of the comparison group 3 is reduced by 0.9×10 8 Cell / cm 3 The results show that sodium bicarbonate has a certain effect on improving the cell density.

[0104] Test 2: Mechanical properties test and result analysis:

[0105] Each group of core agents is used to foam PET. The process is as follows: after the core agent, auxiliary agent (glyceryl monostearate, the addition amount is 0.12% of the mass of the PET raw material) and the PET raw material are mixed evenly, supercritical carbon dioxide is directly extruded and foamed in the extruder. The process conditions are as follows: the temperature of each section from the feed port to the extruder outlet is set as 160℃ in zone I, 160℃ in zone II, and 180℃ in zone III. The temperature of the melt pump is 180℃, the screw speed is 40r / min, and the CO2 flow injection rate is 20-40ml / min; the mass ratio of the core agent to the PET raw material is 1-3:100. Samples of each group of test PET samples are taken to test the high temperature resistance of the PET foaming material under the same conditions. Record the relevant data in 2.

[0106] Table 2: Test data record table

[0107] Group Highest temperature resistance without change(℃) Example 1 Group 150 Example 2 Group 151 Example 3 Group 150 Comparison group 1 148 Comparison of 2 groups 140 Comparison of 3 groups 125

[0108] From Table 2 and Figure 2 It can be seen that compared with the control group, the core agents of Examples 1 to 3 can significantly improve the temperature resistance of the PET foam material; at the same time, the difference between the groups is not obvious. The above results show that the core agents of Examples 1 to 3 have a significant and effective effect of improving the high temperature resistance of the PET foam material.

[0109] In order to verify the effects of the various components of the additive, experiments of Comparative Examples 1 to 3 were set up.

[0110] The main difference between the raw material ratio of the core agent of the comparative group 1 and the example group 1 is that polyethylene terephthalate is used instead of the polymer base material. Compared with the example group 1, it is found that the maximum temperature resistance of the comparative group 1 is reduced by 2°C. This result shows that the polymer base material has little effect on the maximum temperature resistance.

[0111] The main difference between the raw material ratio of the core agent of the comparison group 2 and the example group 1 is that there is no functional additive. Compared with the example group 1, it is found that the maximum temperature resistance of the comparison group 2 is reduced by 10°C. This result shows that the functional additive has a certain effect on the maximum temperature resistance.

[0112] The main difference between the raw material ratio of the core agent of the comparison group 3 and the example group 1 is that sodium bicarbonate is not contained. Compared with the example group 1, it is found that the maximum temperature resistance of the comparison group 3 is reduced by 25°C. This result shows that sodium bicarbonate plays an important role in the maximum temperature resistance.

[0113] From the above, it can be seen that the nucleating agent for improving the cell density of supercritical physical foaming PET prepared by the present invention can not only effectively improve the cell density, but also has the effect of improving the temperature resistance of the PET foaming material. This shows that the nucleating agent for improving the cell density of supercritical physical foaming PET produced by the present invention has a broader market prospect and is more suitable for promotion.

[0114] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0115] The preferred embodiments of the present invention disclosed above are only used to help illustrate the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to the specific implementation methods described. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.

Claims

1. A nucleating agent for increasing the cell density of supercritical physical foaming PET, Features: The core agent is made of the following raw materials in parts by weight: 20 to 30 parts of polymer base material, 10 to 12 parts of functional additives, 10 to 14 parts of sodium bicarbonate, 6 to 10 parts of synergistic additives, 5 to 7 parts of lubricants, 3 to 5 parts of dispersants and 30 to 40 parts of ethyl acetate; The preparation process of the polymer base material is as follows: Ultrasonic dispersion of an appropriate amount of the composite material in an appropriate amount of N,N-dimethylformamide at a solid-liquid ratio of 0.02 to 0.05 g / mL for 20 to 30 minutes to obtain a dispersion; After the polyethylene terephthalate is melted, the dispersion is added dropwise to the melted polyethylene terephthalate at a solid-liquid ratio of 0.012 to 0.022 g / mL, and the mixture is reacted at this temperature for 8 to 10 minutes; After the reaction is completed, the obtained product is vacuum dried at a temperature of 60 to 70° C. for 12 to 14 minutes to obtain a dry product; A proper amount of aminosilicone oil is placed in a proper amount of ethylene glycol at a volume ratio of 0.2 to 0.4:1 and mixed thoroughly to obtain an aminosilicone oil mixture, and then a proper amount of dry product is placed in the aminosilicone oil mixture at a solid-liquid ratio of 0.024 to 0.036 g / mL, treated at 120 to 130°C for 3 to 4 hours, cooled to 60°C, precipitated in a proper amount of 6°C acetone, filtered, and then washed with 6°C acetone for 4 to 6 times. After washing, vacuum dried at 60 to 70°C for 12 to 14 minutes to obtain a polymer base material; The preparation process of the functional additive is as follows: Place an appropriate amount of silane coupling agent KH560 in an appropriate amount of 10% ethanol aqueous solution at a volume ratio of 0.12 to 0.22:1, mix thoroughly, adjust the pH value to 4, seal and let stand for 60 to 70 minutes to obtain a standing solution; Place an appropriate amount of functional material in an appropriate amount of static liquid at a solid-liquid ratio of 0.045 to 0.055:1, heat to 70 to 72°C, stir at 80 to 100 r / min for 20 to 24 hours, filter, rinse with deionized water 2 to 4 times, and dry in a drying oven at 70°C for 26 hours to obtain a functional additive; The composite material is prepared by mixing crotonic acid, styrene and dicumyl peroxide in a mass ratio of 0.3-0.6:0.5-0.8:

1. The functional material is prepared by mixing hydrotalcite and montmorillonite in a mass ratio of 0.4 to 0.6:

1. The synergistic aid is prepared by mixing triethylenetetramine, sodium dodecylbenzene sulfonate and 2,4,6-tris(dimethylaminomethyl)phenol in a mass ratio of 0.2-0.4:0.3-0.7:

1.

2. According to the nucleating agent for improving the cell density of supercritical physical foaming PET as described in claim 1, Features: The lubricant is selected from any one of zinc stearate and calcium stearate.

3. According to the nucleating agent for improving the cell density of supercritical physical foaming PET as described in claim 1, Features: The dispersant is selected from any one of stearamide and hexenyl bisstearamide.

4. A method for preparing a nucleating agent for increasing the cell density of supercritical physical foaming PET according to any one of claims 1 to 3, It is characterized in that The following steps are involved: Step 1, accurately weigh the polymer base material, functional additive, sodium bicarbonate, synergist, lubricant, dispersant and ethyl acetate respectively, then ultrasonically disperse the polymer base material in ethyl acetate for 20 to 30 minutes, then add sodium bicarbonate, and stir at 450 to 550 r / min and room temperature for 20 to 30 minutes, then add the synergist, continue stirring for 15 to 17 minutes, then heat to 60°C for 300 to 320 minutes, take samples, filter, rinse with deionized water for 3 to 7 times, and place the obtained product in a vacuum drying oven at 60°C for 24 hours to obtain a pre-product; Step 2: pre-disperse the pre-product, functional additives, lubricants and dispersants, and obtain the core agent by mixing and granulating the obtained product.