Additive and subtractive composite manufacturing processes based on ultra-high-speed laser cladding and laser 3D printing

By using an additive and subtractive composite manufacturing process combining ultra-high-speed laser cladding and laser 3D printing, the problem of incomplete screw coating coverage has been solved, improving the screw's wear resistance and corrosion resistance, while also reducing costs.

CN118086888BActive Publication Date: 2026-11-17SOUTHWEST JIAOTONG UNIV +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311840884.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-27
Publication Date
2026-11-17
Estimated Expiration
2043-12-27

AI Technical Summary

Technical Problem

Existing technologies struggle to achieve complete coating coverage in the complex structure of screws, resulting in poor reinforcement of the bottom and sides, failing to meet the requirements for wear resistance and corrosion resistance.

Method used

Using an additive and subtractive composite manufacturing process combining ultra-high-speed laser cladding and laser 3D printing, the screw is cut into easily machinable parts. HAST C276-M Hastelloy cladding powder is used to prepare a coating on the bottom surface of the screw and the helical blades, and then the parts are rejoined by welding to form a high-hardness coating.

Benefits of technology

This achieves complete coverage of the screw coating, improving the screw's wear and corrosion resistance while reducing processing costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118086888B_ABST
    Figure CN118086888B_ABST
Patent Text Reader

Abstract

This invention discloses a composite additive and subtractive manufacturing process based on ultra-high-speed laser cladding and laser 3D printing, comprising the following steps: S1: cutting and separating the target heterogeneous component to achieve subtractive material processing; S2: performing laser additive manufacturing on the cut and separated components based on ultra-high-speed laser cladding and laser 3D printing, so that the working surfaces of the cut and separated components all obtain the required target coating; S3: reassembling the cut and separated components to obtain the target heterogeneous component that meets the target requirements. This invention can solve the problems of limited working space and poor accessibility of the cladding head caused by the complex structure of heterogeneous components and the limited size of the laser cladding head; it ensures that a high-quality cladding layer can be obtained in complex spaces, effectively improving various properties of heterogeneous components such as corrosion resistance and wear resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of metal materials technology, and in particular to an additive and subtractive composite manufacturing process based on ultra-high-speed laser cladding and laser 3D printing. Background Technology

[0002] With the rapid development of mechanical engineering in the 21st century, along with the rapid development of large-scale projects such as urban transportation, high-speed rail and light rail, bridge engineering, aerospace, and nuclear energy engineering, there is a greater demand for basic components in mechanical engineering that require high precision and good performance.

[0003] A screw is a cylinder or cone with helical grooves cut on its outer surface. It is widely used as a basic component in industry and is an indispensable part of equipment such as vacuum pumps, injection molding machines, and CNC lathes. During the extrusion process, screws must withstand high temperatures, corrosion, and severe wear, and operate under high torque. Therefore, screws themselves must meet requirements such as high temperature resistance, resistance to deformation at high temperatures, wear resistance, corrosion resistance, and high strength. Optimizing the processing of screws to meet their service environment has become an important research direction that urgently needs development. Summary of the Invention

[0004] To address the aforementioned problems, this invention aims to provide an additive and subtractive composite manufacturing process based on ultra-high-speed laser cladding and laser 3D printing.

[0005] The technical solution of the present invention is as follows:

[0006] An additive-subtractive composite manufacturing process based on ultra-high-speed laser cladding and laser 3D printing includes the following steps:

[0007] S1: Cut and separate the target non-standard components to achieve material reduction;

[0008] S2: Based on ultra-high-speed laser cladding and laser 3D printing, laser additive manufacturing is performed on the cut and separated parts to ensure that the working surfaces of the cut and separated parts all obtain the required target coating.

[0009] S3: Reassemble the cut and separated parts to obtain the target component that meets the target requirements.

[0010] Preferably, the target component is a screw.

[0011] Preferably, in step S1, when cutting and separating the target component, a lathe is used to cut and separate it along the junction of the side and bottom of the screw spiral groove.

[0012] Preferably, the screw is made of QT500-7 cast iron.

[0013] Preferably, the QT500-7 cast iron comprises, by weight percentage, 2.5-3.9% C, less than or equal to 0.08% P, less than or equal to 0.03% S, 0.3-0.8% Mn, 2.5-3.0% Si, and the balance being Fe.

[0014] Preferably, in step S2, the target coating uses HAST C276-M Hastelloy cladding powder as the coating material.

[0015] Preferably, the HAST C276-M Hastelloy alloy deposited powder comprises, by weight percentage: C 0.14%, P 0.01%, Mo 16.00%, W 4.60%, Fe 3.10%, Mn 1.30%, Cr 15.70%, Si 0.70%, V 0.60%, with the balance being Ni.

[0016] Preferably, in step S2, when performing laser additive manufacturing, a coating is prepared by using an ultra-high-speed laser to clad the bottom surface of the cut screw where it is not connected to the spiral groove, and the coating is obtained by using laser 3D printing on the screw spiral blades.

[0017] As a preferred option, the RFL-C6000 laser system was used for laser cladding experiments. During the laser cladding experiments, the laser power was 1600W, the motor powder feeding speed was 1.8r / min or 2.0r / min, the scanning rate was 350mm / min, and the protective gas flow rate was 40L / min.

[0018] Preferably, in step S3, welding technology is used to reassemble the cut and separated parts.

[0019] The beneficial effects of this invention are:

[0020] This invention solves the technical problem that the coating on the bottom and side surfaces of screws is incomplete and fails to achieve a strengthening effect due to the size limitations of the laser head and the structural constraints of complex components. Compared to using 3D printing technology to process complex components such as screws and vacuum pumps, this invention is more cost-effective, and the resulting coating has higher hardness, effectively improving the wear resistance and corrosion resistance of the screw. Attached Figure Description

[0021] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0022] Figure 1 This is a schematic diagram of the macroscopic microstructure of the coating and substrate of a laser-clad part in Group 1 of a specific embodiment.

[0023] Figure 2 This is a schematic diagram of the macroscopic microstructure of the coating and substrate of a laser-clad part in Group 2 of a specific embodiment.

[0024] Figure 3 This is a schematic diagram of the macroscopic microstructure of the coating and substrate of a laser-clad part in Group 3 of a specific embodiment.

[0025] Figure 4 This is a schematic diagram of the macroscopic microstructure of the coating and substrate of a laser-clad part in Group 4 of a specific embodiment.

[0026] Figure 5 This is a schematic diagram of the macroscopic microstructure of the coating and substrate of a laser-clad part in Group 5 of a specific embodiment.

[0027] Figure 6 This is a schematic diagram showing the hardness test results of the coating substrate of laser-clad parts in each group in a specific embodiment.

[0028] Figure 7 This is a schematic diagram showing the corrosion performance test results of laser-clad parts without machined coatings in each group according to a specific embodiment;

[0029] Figure 8 This is a schematic diagram showing the corrosion performance test results of the polished coating of laser-clad parts in each group according to a specific embodiment. Detailed Implementation

[0030] The present invention will be further described below with reference to the accompanying drawings and embodiments. It should be noted that, unless otherwise specified, the embodiments and technical features described in this application can be combined with each other. It should also be pointed out that, unless otherwise indicated, all technical and scientific terms used in this application have the same meaning as commonly understood by one of ordinary skill in the art to which this application pertains. The terms "comprising" or "including" and similar words used in this invention refer to elements or objects preceding the word that encompass the elements or objects listed following the word and their equivalents, without excluding other elements or objects.

[0031] This invention provides an additive-subtractive composite manufacturing process based on ultra-high-speed laser cladding and laser 3D printing, comprising the following steps:

[0032] S1: Cut and separate the target component to achieve material reduction.

[0033] In one specific embodiment, the target component is a screw. When cutting and separating the target component, a lathe is used to cut and separate it along the junction of the side and bottom of the screw's helical groove.

[0034] Optionally, the screw is made of QT500-7 cast iron; the QT500-7 cast iron, by weight percentage, includes 2.5-3.9% C, less than or equal to 0.08% P, less than or equal to 0.03% S, 0.3-0.8% Mn, 2.5-3.0% Si, and the balance is Fe.

[0035] In the above embodiment, since the laser head used in the subsequent processing is large in size and cannot reach into the narrow spiral groove area of ​​the screw, it is difficult to directly clad the bottom surface of this part of the spiral groove and the sides of all the spiral grooves. Therefore, it is necessary to use equipment to cut along the spiral pattern at the junction of the side and bottom surfaces of the spiral groove of the screw, dividing it into two parts: a spiral blade and a cylindrical screw. A high-speed steel end mill is used, and the cutting speed is controlled at 20m / min, and the workpiece feed speed is 0.15mm / z to complete the subtractive material process.

[0036] S2: Based on ultra-high-speed laser cladding and laser 3D printing, laser additive manufacturing is performed on the cut and separated parts to ensure that the working surfaces of the cut and separated parts all obtain the required target coating.

[0037] In one specific embodiment, the target coating uses HAST C276-M Hastelloy alloy cladding powder as the coating material; the HAST C276-M Hastelloy alloy cladding powder, by weight percentage, comprises C 0.14%, P 0.01%, Mo 16.00%, W 4.60%, Fe 3.10%, Mn 1.30%, Cr 15.70%, Si 0.70%, V 0.60%, with the balance being Ni.

[0038] In one specific embodiment, during laser additive manufacturing, an ultra-high-speed laser is used to clad the bottom surface of the cut screw where it is not connected to the spiral groove to prepare a coating, and then laser 3D printing is used to apply the coating to the screw spiral blades.

[0039] Optionally, the RFL-C6000 laser system is used to conduct laser cladding experiments. When conducting laser cladding experiments, the laser power is 1600W, the motor powder feeding speed is 1.8r / min or 2.0r / min, the scanning rate is 350mm / min, and the protective gas flow rate is 40L / min.

[0040] It should be noted that the above parameters are process parameters obtained by the present invention through the following experiments. When using the present invention, other process parameters may also be adopted according to requirements.

[0041] Deposit 65×70mm on QT500-7 board. 2 Laser cladding was used to obtain parts with a single-layer HAST C276-M Hastelloy alloy coating. During the process, an RFL-C6000 laser system was used for laser cladding experiments. This system includes a fiber-optic 6.0K solid-state laser and a coaxial laser deposition head with a lens focal length of 300mm. Argon gas was used as both the powder carrier gas and the protective gas. Specific laser cladding process parameters are shown in Table 1.

[0042] Table 1 Laser Cladding Process Parameters

[0043]

[0044] The macroscopic morphology of the laser-clad parts obtained in each experiment was good, and the macroscopic microstructure of the coating and the substrate was as follows: Figure 1-5 As shown. From Figure 1-5 It can be seen that no cracks or defects were observed in the coating, and the coating and the substrate had good metallurgical bonding; a small amount of pores were visible in the coating. The dilution rate and porosity of coatings prepared by different processes were statistically analyzed, and the results are shown in Table 2:

[0045] Table 2 Deformation of Laser Cladding Parts

[0046]

[0047] As can be seen from Table 2, the dilution rates of groups 3 and 5 are relatively low, at 18.32% and 15.91% respectively; the porosities are 0.12% and 0.18% respectively, which are relatively small values ​​among the five processes.

[0048] The deformation of the laser-clad part was tested. One side of the part was fixed on a plane, and the warping at the middle and corners of the opposite side was measured. The deformation is shown in Table 3.

[0049] Table 3 Deformation of Laser Cladding Parts

[0050]

[0051] As can be seen from Table 3, the deformation of groups 3 and 5 is the smallest. The warping at the middle of the edge of groups 3 and 5 is 1 mm, and the warping at the corner is 2.5 mm.

[0052] The hardness of the laser-clad parts was tested, and the results are as follows: Figure 6 As shown. From Figure 6 It can be seen that the coating hardness is between 325 and 400 Hv1, and the substrate hardness is between 150 and 225 Hv1. The hardness of each laser-clad part is good.

[0053] Salt spray corrosion tests were conducted on laser-clad parts according to ISO 0376-81976 standards. A 5wt% NaCl solution was continuously sprayed, and the test chamber temperature was maintained at (35±1)℃ with a pH of 7.5. Before the test, the surface of the coating on a 30mm×20mm×10mm sample was polished with 600# sandpaper, cleaned with alcohol, and then the five uncoated sides were sealed with epoxy resin. After continuous spraying for 24h, 48h, 72h, 144h, and 288h, the surface morphology of the sample was observed, and the sample was dried with hot air and weighed to measure the increase in corrosion mass. The changes in corrosion mass for the polished and uncoated samples over time were obtained as follows: Figure 7-8 As shown. From Figure 7-8 It can be seen that the corrosion resistance of each laser-clad part is good.

[0054] Based on the above test results, the laser-clad parts prepared in groups 3 and 5 exhibited smaller deformation, dilution rate, and porosity, and also demonstrated better hardness and corrosion resistance. Therefore, when using QT500-7 cast iron screws as the target component and HASTC276-M Hastelloy cladding powder as the coating material, the parameters corresponding to groups 3 and 5 are adopted as the preferred process parameters.

[0055] In the above embodiments, an ultra-high-speed laser cladding method is used to prepare a coating on the bottom and side surfaces of the screw spiral groove. Compared with welding methods such as overlay welding, spray welding, and traditional laser cladding, ultra-high-speed laser cladding has a smaller dilution, denser structure, is suitable for a wider range of cladding materials, has higher energy utilization, and results in better bonding between the substrate and the coating.

[0056] Furthermore, due to the "trapezoidal groove" structure of the screw, its spatial structure is quite complex, making it unsuitable for existing conventional laser cladding heads. The additive-subtractive composite manufacturing process based on ultra-high-speed laser cladding and laser 3D printing addresses the limitations of the cladding head's operating space and accessibility caused by the complex structure of the component and the size constraints of the laser cladding head. This allows ultra-high-speed cladding technology to be applied to such complex components, expanding the laser scanning area and achieving higher coating coverage, thus meeting the operational requirements of the components in service. It also ensures a high-quality cladding layer is obtained even in complex environments, effectively improving the screw's corrosion and wear resistance.

[0057] S3: Reassemble the cut and separated parts to obtain the target component that meets the target requirements.

[0058] In one specific embodiment, welding technology is used to reassemble the cut and separated components.

[0059] This invention solves the technical problem that the coating on the bottom and side surfaces of screws is incomplete and fails to achieve a strengthening effect due to the size limitations of the laser head and the structural constraints of complex components. Compared to using 3D printing technology to process complex components such as screws and vacuum pumps, this invention is more cost-effective, and the resulting coating has higher hardness, effectively improving the wear resistance and corrosion resistance of the screw.

[0060] The above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention in any way. Although the present invention has been disclosed above with reference to preferred embodiments, it is not intended to limit the present invention. Any person skilled in the art can make some modifications or alterations to the above-disclosed technical content to create equivalent embodiments without departing from the scope of the present invention. Any simple modifications, equivalent changes, and alterations made to the above embodiments based on the technical essence of the present invention without departing from the scope of the present invention shall still fall within the scope of the present invention.

Claims

1. A composite manufacturing process for additive and subtractive materials based on ultra-high-speed laser cladding and laser 3D printing, characterized in that, Includes the following steps: S1: The target component is cut and separated to achieve material reduction; the target component is a screw. When cutting and separating the target component, a turning machine is used to cut and separate it along the junction of the side and bottom of the screw's spiral groove. S2: Based on ultra-high-speed laser cladding and laser 3D printing, laser additive manufacturing is performed on the cut and separated parts to ensure that the working surfaces of the cut and separated parts all obtain the required target coating. When performing laser additive manufacturing, a coating is prepared by cladding an ultra-high-speed laser onto the bottom surface of the screw that is not connected to the spiral groove after cutting, and then the coating is obtained by laser 3D printing on the screw spiral blades. The target coating uses HAST C276-M Hastelloy cladding powder as the coating material; S3: Reassemble the cut and separated parts to obtain the target component that meets the target requirements.

2. The additive-subtractive composite manufacturing process based on ultra-high-speed laser cladding and laser 3D printing according to claim 1, characterized in that, The screw is made of QT500-7 cast iron.

3. The additive and subtractive composite manufacturing process based on ultra-high-speed laser cladding and laser 3D printing according to claim 2, characterized in that, The QT500-7 cast iron, by weight percentage, comprises 2.5-3.9% C, less than or equal to 0.08% P, less than or equal to 0.03% S, 0.3-0.8% Mn, 2.5-3.0% Si, and the balance is Fe.

4. The additive-subtractive composite manufacturing process based on ultra-high-speed laser cladding and laser 3D printing according to claim 1, characterized in that, The HAST C276-M Hastelloy alloy deposited powder, by weight percentage, comprises 0.14% C, 0.01% P, 16.00% Mo, 4.60% W, 3.10% Fe, 1.30% Mn, 15.70% Cr, 0.70% Si, 0.60% V, with the balance being Ni.

5. The additive-subtractive composite manufacturing process based on ultra-high-speed laser cladding and laser 3D printing according to claim 1, characterized in that, The laser cladding experiment was conducted using the RFL-C6000 laser system. The laser power was 1600 W, the motor powder feeding speed was 1.8 r / min or 2.0 r / min, the scanning rate was 350 mm / min, and the protective gas flow rate was 40 L / min.

6. The additive-subtractive composite manufacturing process based on ultra-high-speed laser cladding and laser 3D printing according to any one of claims 1-5, characterized in that, In step S3, welding technology is used to reassemble the cut and separated components.

Citation Information

Patent Citations

  • Laser near-net forming method of special-shaped deep-cavity thin-walled cabin

    CN109277567A

  • Injection molding machine screw and manufacturing method thereof

    CN111097908A