A method for comprehensive recycling of titanium tetrachloride inert waste residue
By using a full flotation process and appropriate reagents, the problem of low separation efficiency of valuable components in titanium tetrachloride inert waste residue has been solved, achieving efficient and simple resource recovery and environmental protection, which is suitable for industrial applications.
Patent Information
- Application Number
- CN202410410743.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-07
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2044-04-07
AI Technical Summary
In the existing technology, the recycling of titanium tetrachloride inert waste residue has problems such as low grade of valuable components, low recovery rate and complicated process flow, resulting in resource waste and environmental pollution. Moreover, the existing process is difficult to achieve efficient and simple industrial production.
By adopting a full flotation process and controlling the pulp concentration and selecting appropriate flotation reagents, petroleum coke, rutile and quartz sand in titanium tetrachloride inert waste residue are separated. The flotation process of one roughing and two scavenging or one roughing, one scavenging and four cleaning is used, combined with KL collector, modified fatty acid and gangue inhibitor, to achieve efficient separation.
It yields high-grade petroleum coke concentrate, rutile concentrate, and quartz concentrate with a recovery rate of over 85%, solving the problems of resource waste and environmental pollution, and realizing the reduction and resource utilization of waste residue, making it suitable for industrial production.
Smart Images

Figure CN118106130B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of mineral processing technology, and more specifically, to a method for the comprehensive recycling and utilization of titanium tetrachloride inert waste residue. Background Technology
[0002] Titanium tetrachloride, a key raw material for the production of sponge titanium and titanium dioxide, generates a large amount of inert waste residue during the chlorination process. This residue is highly hygroscopic in air, releasing a large amount of pungent gas, and its aqueous solution is strongly acidic. Statistics show that approximately 10% of the inert waste residue is generated for every ton of titanium tetrachloride produced. If this inert waste residue is not properly disposed of in a timely manner, it will cause significant pollution to the natural environment and inevitably pose serious health risks.
[0003] At present, the treatment of inert waste residue is mainly based on neutralization and landfill, chemical leaching, and mineral processing and recycling. The main problems are as follows: (1) The grade of the recovered valuable components is low: the existing process for recovering petroleum coke, rutile and other products in inert waste residue has the problem that the TiO2 grade in rutile concentrate is less than 70% and the C grade in petroleum coke concentrate is less than 75%, so they cannot be directly utilized; (2) The recovery rate of valuable components in inert waste residue is low: at present, flotation is mostly used to recover petroleum coke in inert waste residue, and gravity separation and electrostatic separation are used to recover rutile from tailings, but the recovery rate of rutile is less than 70%, resulting in a large waste of titanium resources; (3) The process flow of inert waste residue recycling is complicated: at present, gravity separation, flotation and magnetic separation are mainly used for the recycling of inert waste residue. The existing process often uses magnetic separation + gravity separation + flotation, chemical leaching + flotation and other combined processing processes. Compared with a single mineral processing method, the combined process flow of multiple mineral processing methods is complicated and difficult to operate.
[0004] Currently, domestic enterprises and research institutes have conducted extensive research and development on new technologies for the "reduction, harmlessness, and resource utilization" of chlorinated slag. Patent application CN114377860A discloses a method for the resource utilization of chlorinated dust collection slag from the chlorination process for titanium dioxide production. The method involves sequential pulping, solid-liquid separation, and washing. The titanium-containing slag is then pulped again, and flotation reagents are added for flotation. The resulting petroleum coke concentrate is then washed, filtered, pelletized, and dried. The titanium-containing slurry undergoes solid-liquid separation and drying to obtain titanium-containing minerals. The petroleum coke pellets, titanium-containing minerals, titanium concentrate, and anthracite are then smelted to obtain titanium slag, which is used as a raw material for the sulfuric acid process in titanium dioxide production. Although this process separates petroleum coke and rutile, the TiO2 grade of the obtained rutile concentrate is below 70%, failing to meet the requirements for separate sale. Furthermore, using it as a raw material for the sulfuric acid process in titanium dioxide production can easily lead to a decrease in acidolysis rate and the introduction of excessive impurities. The invention patent application CN115999764A discloses a method for recycling and treating chlorinated waste residue and its application. The main steps are: first, the inert waste residue is slurryed, filtered, dried, and then subjected to electrostatic separation for desilication. The desilication material is then subjected to flotation to separate petroleum coke and rutile, with diesel or kerosene as the collector. The resulting petroleum coke concentrate has a C grade of 74.12% and a C recovery rate of 85.54%; the rutile concentrate has a TiO2 grade of 90.12% and a TiO2 recovery rate of 83.77%; and the quartz concentrate has a SiO2 grade of 50.15%. This patent uses a combined electrostatic separation and flotation process, which has problems such as a complex process flow, high energy consumption in electrostatic separation, high production costs, and low SiO2 grade in the quartz concentrate. The invention patent application with publication number CN115487933A discloses a method for separating and recycling coke slag from titanium dioxide ore produced by the chloride process. The method involves adding water to the coke slag from the chloride process titanium dioxide ore, stirring to form a slurry, and then diluting the slurry at a flow rate of 15-20 ml. 3 With a feed rate of / h, flotation reagents are added, and compressed air is used for bubbling. The material is then separated through four stages of flotation to obtain coking foam and bottom material. The coking foam from stages 1 to 4 is collected and combined, filtered, and dried to obtain carbon concentrate. The bottom material from stages 1 to 3 is conveyed to the next flotation stage, and the bottom material from stage 4 is separated into ore belts through two shaking tables. Although this process separates petroleum coke and rutile, yielding petroleum coke concentrate with a C grade of 61.30% and rutile concentrate with a TiO2 grade of 81.90%, the process has the following problems: low separation efficiency (tailings TiO2% > 15%), low recovery rate (only 50%), high operation difficulty, high water consumption, and large equipment footprint. It still requires site storage for tailings, does not completely solve environmental problems, and its economic benefits have not been maximized. Summary of the Invention
[0005] One of the objectives of this invention is to provide a process flow and control parameters for the comprehensive recycling of titanium tetrachloride inert waste residue. The process is simple, efficient, and has a high product recovery rate, making it suitable for industrial production. The process parameters are precisely controlled at each stage, ensuring stable and efficient production operation.
[0006] The second objective of this invention is to provide a reagent system for the comprehensive recycling of titanium tetrachloride inert waste residue, which is inexpensive, uses widely available raw materials, and is non-toxic, harmless, and environmentally friendly. It requires fewer types of flotation reagents and has low unit consumption.
[0007] The third objective of this invention is to provide a method for reducing and rendering harmless titanium tetrachloride inert waste residue, ultimately achieving comprehensive recycling of solid waste and obtaining three products: high-grade petroleum coke concentrate, rutile concentrate, and quartz concentrate.
[0008] The following technical solution is adopted:
[0009] In a first aspect, the present invention provides a process flow and control parameters for the comprehensive recycling and utilization of titanium tetrachloride inert waste residue, including the following steps:
[0010] (1) Pulping: Titanium tetrachloride inert waste residue is mixed with water and stirred to obtain mineral slurry;
[0011] (2) Flotation of petroleum coke: The slurry from step (1) enters the petroleum coke flotation system to obtain petroleum coke concentrate and flotation tailings;
[0012] (3) Concentration: The flotation tailings from step (2) are concentrated and dewatered in a plate thickener to obtain concentrated underflow product; (4) Rutile flotation: The concentrated underflow product from step (3) is fed into a rutile flotation system to obtain rutile concentrate and quartz concentrate.
[0013] Furthermore, in step (1), the pulping process requires the pulp concentration to be controlled between 15% and 40%.
[0014] Preferably, the pulp concentration needs to be controlled at 20% to 35% during the pulping process;
[0015] Preferably, the pulp concentration needs to be controlled at 25% to 30% during the pulping process.
[0016] Furthermore, in step (2), the slurry feed concentration in the petroleum coke flotation process is controlled at 25% to 30%, and the process flow adopts one roughing and two scavenging steps.
[0017] Furthermore, in step (3), the concentration process uses a slant plate thickener, and the concentration of the concentrated underflow product needs to be controlled between 45% and 70%.
[0018] Furthermore, in step (4), the slurry concentration in the rutile flotation process needs to be controlled at 45% to 70%, and the process flow adopts one roughing, one scavenging, and four cleaning steps.
[0019] Secondly, the present invention provides a flotation reagent and reagent system for the comprehensive recycling and utilization of titanium tetrachloride inert waste residue, comprising the following steps:
[0020] (1) Flotation of petroleum coke: Titanium tetrachloride inert waste residue is slurryed and stirred to obtain slurry. Petroleum coke collector is added to the slurry to carry out petroleum coke flotation to obtain petroleum coke concentrate and decarbonized tailings.
[0021] (2) Rutile flotation: Rutile flotation reagents are added to the decarbonized tailings to carry out rutile flotation, and rutile concentrate and quartz concentrate are obtained.
[0022] Further, in step (1) flotation of petroleum coke, the petroleum coke collector used for flotation of petroleum coke is KL collector produced by the Changsha Design Institute of Chemical Industry.
[0023] Further, in step (1) flotation of petroleum coke: the amount of collector used for roughing petroleum coke is 400g / t to 800g / t, the amount of collector used for scavenging petroleum coke is 100g / t to 300g / t, and the amount of collector used for scavenging petroleum coke is 200g / t to 400g / t.
[0024] Further, in step (2), rutile is floated. The reagents used for rutile flotation include gangue inhibitors, main collectors and auxiliary collectors.
[0025] Furthermore, gangue inhibitors include one or two of oxalic acid, sodium fluorosilicate, and sodium silicate;
[0026] Preferably, the gangue inhibitor is a compound of oxalic acid and sodium silicate;
[0027] Preferably, the mass ratio of oxalic acid to sodium silicate is 40:60;
[0028] Preferably, the sodium silicate modulus is 2.9;
[0029] Preferably, sodium silicate is in liquid form.
[0030] Furthermore, the main collector is modified fatty acid, which is selected from HB-T3 produced by Hebei Hengyuan Oil Factory.
[0031] Furthermore, the auxiliary collector is diesel fuel.
[0032] Further, in step (2) flotation of rutile: the amount of gangue inhibitor used in roughing is 1500g / t to 3000g / t, the amount of main collector is 2500g / t to 4000g / t, the amount of auxiliary collector is 400g / t to 800g / t, the amount of gangue inhibitor used in scavenging is 600g / t to 1000g / t, the amount of main collector is 800g / t to 1500g / t, the amount of auxiliary collector is 100g / t to 300g / t, the amount of gangue inhibitor used in finishing one is 0g / t, the amount of gangue inhibitor used in finishing two is 300g / t to 800g / t, the amount of gangue inhibitor used in finishing three is 300g / t to 800g / t, and the amount of gangue inhibitor used in finishing four is 300g / t to 800g / t.
[0033] Compared with the prior art, the present invention has the following beneficial effects:
[0034] (1) The present invention has a high recovery rate of each useful component in titanium tetrachloride inert waste residue. The present invention provides a comprehensive recycling process and control parameters for titanium tetrachloride inert waste residue. The process of pre-separating hydrophobic petroleum coke using a roughing and scavenging flotation process can obtain qualified carbon concentrate with a carbon recovery rate of over 90%. Then, the tailings of carbon beneficiation are subjected to a roughing, scavenging and cleaning flotation process to finally obtain qualified rutile concentrate with a TiO2 yield of over 85%. The recovery rate of rutile concentrate is more than 30% higher than that of gravity separation process.
[0035] (2) The final product of the present invention has good quality. Through the process flow method of the present invention, inert waste residue with carbon grade of 30% to 50% and TiO2 grade of 20% to 30% can be selected as carbon concentrate with carbon grade greater than 75%, rutile concentrate with TiO2 grade greater than 85% and quartz concentrate with SiO2 grade greater than 50%. The quality of the three products all meet the sales standards. The petroleum coke obtained can be used for power generation in power plants, rutile can be mixed with ilmenite as a raw material for preparing titanium tetrachloride, and quartz concentrate can be used as a raw material for the production of water glass, etc.
[0036] (3) This invention is the first to use a full flotation process to recover petroleum coke, rutile and quartz sand from titanium tetrachloride inert waste residue, realizing the reduction, resource utilization and harmless treatment of titanium tetrachloride inert waste residue, which not only solves the problems of large space occupation and serious environmental pollution caused by waste residue storage, but also obtains good economic benefits.
[0037] (4) The process flow of this invention is simple, easy to operate, and suitable for industrial production. This invention uses a full flotation process to recover and utilize titanium tetrachloride inert waste residue. Based on the specific gravity differences, surface hydrophobicity, and electrochemical properties of the components in the titanium tetrachloride inert waste residue, a roughing and scavenging flotation process is used to pre-separate the petroleum coke with better hydrophobicity. By controlling the pulp concentration and thus the viscosity of the material, the components in the titanium tetrachloride inert waste residue are evenly dispersed in the pulp system. Under the multi-stage turbulence generated by the impeller of the flotation machine, the collision mineralization probability of petroleum coke and collector can be increased, thereby promoting the capture of petroleum coke with better hydrophobicity by bubbles, improving the separation efficiency, and selecting qualified petroleum coke concentrate. The tailings after carbon separation not only contain fine-grained rutile minerals, but also a large number of high-valence metal ions, silicon-aluminum homogeneous bodies, and hydrochloric acid, making separation difficult. Through the roughing, scavenging, and cleaning flotation process of this invention and the combined effect of gangue inhibitors and collectors with good synergistic effects, high-quality rutile concentrate and qualified quartz concentrate can be effectively selected. Attached Figure Description
[0038] To more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings used in the embodiments will be briefly introduced below. It should be understood that the following drawings only show some embodiments of the present invention and should not be regarded as a limitation on the scope. For those skilled in the art, other related drawings can be obtained based on these drawings without creative effort.
[0039] Figure 1 A process flow diagram of a mineral processing test provided in an embodiment of the present invention. Detailed Implementation
[0040] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Where specific conditions are not specified in the embodiments, conventional conditions or conditions recommended by the manufacturer shall apply. Reagents or instruments whose manufacturers are not specified are all conventional products that can be purchased commercially.
[0041] Given the low concentrate grade, low recovery rate, and complex process flow of existing processes, this invention proposes for the first time a method using a full flotation process to recover petroleum coke, rutile, and quartz sand from inert waste residue. Using the comprehensive recycling method for titanium tetrachloride inert waste residue provided by this invention, petroleum coke concentrate with a C grade greater than 75%, rutile concentrate with a TiO2 grade greater than 85%, and quartz concentrate with a SiO2 grade greater than 50% can be obtained.
[0042] The following is a detailed description of a method for the comprehensive recycling and utilization of titanium tetrachloride inert waste residue provided by an embodiment of the present invention.
[0043] This invention provides a method for the comprehensive recycling of titanium tetrachloride inert waste residue, which includes: separating the slurry obtained by stirring the titanium tetrachloride inert waste residue into petroleum coke, and then separating it into rutile to obtain petroleum coke concentrate, rutile concentrate and quartz concentrate.
[0044] In the above method, for the inert titanium tetrachloride slag, a decarbonization operation is first carried out to remove the petroleum coke to obtain petroleum coke concentrate and flotation tailings. At the same time, the impurities in the inert titanium tetrachloride slag are reduced, which is beneficial to the subsequent flotation of rutile and ensures that the rutile grade reaches more than 85%. Then, the flotation tailings are subjected to rutile flotation to obtain rutile concentrate and quartz concentrate.
[0045] In some implementations, the following steps are included:
[0046] (1) Pulping: Titanium tetrachloride inert waste residue is mixed with water and stirred to obtain mineral slurry;
[0047] (2) Flotation of petroleum coke: The slurry from step (1) enters the petroleum coke flotation system to obtain petroleum coke concentrate and decarbonized tailings;
[0048] (3) Concentration: The decarbonized tailings from step (2) are fed into a thickener for concentration and dewatering to obtain concentrated underflow product;
[0049] (4) Flotation of rutile: The concentrated underflow product from step (3) enters the rutile flotation system to obtain rutile concentrate and quartz concentrate.
[0050] This invention provides a method for the comprehensive recycling of titanium tetrachloride inert waste residue, comprising: mixing titanium tetrachloride inert waste residue with water to obtain a slurry; directly adding a petroleum coke collector to the slurry for flotation to obtain petroleum coke concentrate and decarbonized tailings; and then adding rutile flotation reagents to the decarbonized tailings for flotation to obtain rutile concentrate and quartz concentrate. In the rutile flotation operation, due to the properties of the minerals and reagents, the flotation pH is maintained between 1.5 and 2.0, eliminating the need for pH adjusters. Simultaneously, the rutile flotation reagents also selectively inhibit quartz, allowing for the rapid separation of qualified rutile concentrate and quartz concentrate. The comprehensive recycling method for titanium tetrachloride inert waste provided by this invention has the characteristics of simple process, high recovery rate and high product grade. The obtained petroleum coke concentrate has a C grade of 78.13%, rutile concentrate has a TiO2 grade of 89.36% and quartz concentrate has a SiO2 grade of 55.03%, and the recovery rate of all of them is greater than 85%, which effectively realizes the resource utilization of titanium tetrachloride inert waste.
[0051] In some embodiments, the preparation of the slurry includes: adding water to titanium tetrachloride inert waste residue, stirring and concentrating to obtain the slurry.
[0052] In some embodiments, the carbon content in the titanium tetrachloride inert waste residue is 30%–50%, and the TiO2 content is 22%–35%.
[0053] In some embodiments, the mass fraction of minerals in the flotation pulp is 25% to 30%.
[0054] In some implementations, step (2) flotation of petroleum coke adopts a process flow of one roughing and two scavenging steps.
[0055] In some implementations, the pulp concentration of flotation petroleum coke is controlled at 25% to 30%.
[0056] In some embodiments, the reagent for flotation of petroleum coke is a petroleum coke collector, specifically the KL collector produced by the Changsha Design Institute of the Ministry of Chemical Industry.
[0057] In some implementation methods, the amount of petroleum coke collector added is calculated per ton of waste residue: the amount of crude petroleum coke collector is 400g / t to 800g / t, the amount of first-stage petroleum coke collector is 100g / t to 300g / t, and the amount of second-stage petroleum coke collector is 200g / t to 400g / t.
[0058] In some implementations, the crude petroleum coke collector is selected at a rate of 600 g / t, the first scavenging agent at a rate of 200 g / t, and the second scavenging agent at a rate of 300 g / t.
[0059] In some implementations, step (3) concentration is performed using a slant plate thickener for concentration and dehydration.
[0060] In some implementations, the thickening process requires controlling the slurry concentration to be between 40% and 70%.
[0061] In some implementations, step (4) flotation of rutile adopts a process flow of one roughing, one scavenging, and four refining steps.
[0062] In some implementations, the pulp concentration for flotation of rutile is controlled at 45% to 70%.
[0063] In some implementations, rutile flotation reagents mainly include gangue inhibitors, primary collectors, and secondary collectors.
[0064] In some embodiments, gangue inhibitors include one or two of oxalic acid, sodium fluorosilicate, and sodium silicate.
[0065] In some embodiments, the gangue inhibitor is a compound of oxalic acid and sodium silicate.
[0066] In some embodiments, the mass ratio of oxalic acid to sodium silicate is 40:60.
[0067] In some embodiments, the sodium silicate has a modulus of 2.9 and is in a liquid state.
[0068] In some implementations, the main collector is a modified fatty acid, which is selected from HB-T3 produced by Hebei Hengyuan Oil Factory.
[0069] In some implementations, the auxiliary collector is diesel fuel.
[0070] In some implementation methods, the flotation reagent addition is calculated per ton of raw ore: 1500g / t to 3000g / t for rougher gangue inhibitor, 2500g / t to 4000g / t for main collector, 400g / t to 800g / t for auxiliary collector, 600g / t to 1000g / t for scavenger gangue inhibitor, 800g / t to 1500g / t for main collector, 100g / t to 300g / t for auxiliary collector, 0g / t for gangue inhibitor in the first stage of refinement, 300g / t to 800g / t for gangue inhibitor in the second stage of refinement, 300g / t to 800g / t for gangue inhibitor in the third stage of refinement, and 300g / t to 800g / t for gangue inhibitor in the fourth stage of refinement.
[0071] This invention provides a comprehensive recycling method for titanium tetrachloride inert waste residue, which can comprehensively recover useful minerals from the waste residue to obtain high-quality petroleum coke concentrate, rutile concentrate, and quartz concentrate. This method achieves resource utilization and harmless treatment of the waste residue, solving the problems of large space occupation and serious environmental pollution caused by waste residue storage, while also yielding good economic benefits.
[0072] The features and performance of the present invention will be further described in detail below with reference to embodiments.
[0073] Example 1
[0074] A method for comprehensive recycling of titanium tetrachloride inert waste residue, see [link to relevant documentation]. Figure 1 The process includes the following steps: preparing flotation slurry; adding water and stirring to concentrate titanium tetrachloride inert waste residue with a C grade of 36.62% and a TiO2 grade of 24.13% into a flotation slurry of 20% to 30%;
[0075] Petroleum coke sorting: This operation section adopts a coarse and scavenging process; the amount of petroleum coke collector added is calculated per ton of waste residue: 600g / t for coarse selection, 200g / t for scavenging one, and 300g / t for scavenging two.
[0076] Rutile Separation: The decarbonized tailings concentration is 60%. Rutile flotation reagents are added for flotation to obtain rutile concentrate and quartz concentrate. This operation section adopts a flotation process of one roughing, one scavenging, and four cleaning stages. The dosage of rutile flotation reagents is calculated per ton of raw ore: roughing gangue depressant 2000g / t, main collector 3000g / t, auxiliary collector 600g / t, scavenging gangue depressant 800g / t, main collector 1000g / t, auxiliary collector 200g / t, cleaning gangue depressant 0g / t, cleaning gangue depressant 500g / t, cleaning gangue depressant 500g / t, and cleaning gangue depressant 500g / t.
[0077] The obtained petroleum coke concentrate had a carbon grade of 78.13% and a carbon recovery rate of 90.06%, the rutile concentrate had a TiO2 grade of 89.36% and a TiO2 recovery rate of 89.95%, and the quartz concentrate had a SiO2 grade of 55.03%.
[0078] Example 2
[0079] Prepare flotation slurry; titanium tetrachloride inert waste residue with C grade of 36.62% and TiO2 grade of 24.13% is mixed with water and concentrated to a flotation slurry of 20% to 30%;
[0080] Petroleum coke separation: Petroleum coke collector is added for flotation to obtain petroleum coke concentrate and decarbonized tailings. This operation section adopts a one-roughing and two-scavenging process. The amount of petroleum coke collector added is calculated per ton of waste residue: 600g / t for roughing, 200g / t for scavenging one, and 300g / t for scavenging two.
[0081] Rutile Separation: The decarbonized tailings concentration is 60%. Rutile flotation reagents are added for flotation to obtain rutile concentrate and quartz concentrate. This operation section adopts a flotation process of one roughing, one scavenging, and four cleaning stages. The dosage of rutile flotation reagents is calculated per ton of raw ore as follows: roughing gangue depressant 2000g / t, main collector 2000g / t, auxiliary collector 500g / t; scavenging gangue depressant 800g / t, main collector 800g / t, auxiliary collector 100g / t; cleaning gangue depressant 0g / t; cleaning gangue depressant 400g / t; cleaning gangue depressant 400g / t; cleaning gangue depressant 400g / t.
[0082] The obtained petroleum coke concentrate had a carbon grade of 78.13% and a carbon recovery rate of 90.06%, the rutile concentrate had a TiO2 grade of 88.84% and a TiO2 recovery rate of 88.93%, and the quartz concentrate had a SiO2 grade of 50.93%.
[0083] Example 3
[0084] Prepare flotation slurry; add water to inert titanium tetrachloride waste residue with C grade of 36.62% and TiO2 grade of 24.13% and stir to concentrate it into a flotation slurry of 20% to 30%;
[0085] Petroleum coke separation: Petroleum coke collector is added for flotation to obtain petroleum coke concentrate and decarbonized tailings. This operation section adopts a one-roughing and two-scavenging process. The amount of petroleum coke collector added is calculated per ton of waste residue: 600g / t for roughing, 200g / t for scavenging one, and 300g / t for scavenging two.
[0086] Rutile Separation: The decarbonized tailings concentration is 60%. Rutile flotation reagents are added for flotation to obtain rutile concentrate and quartz concentrate. This operation section adopts a flotation process of one roughing, one scavenging, and four cleaning stages. The dosage of rutile flotation reagents is calculated per ton of raw ore as follows: roughing gangue depressant 1500g / t, main collector 3000g / t, auxiliary collector 500g / t; scavenging gangue depressant 800g / t, main collector 800g / t, auxiliary collector 100g / t; cleaning gangue depressant 0g / t; cleaning gangue depressant 300g / t; cleaning gangue depressant 300g / t; cleaning gangue depressant 300g / t; cleaning gangue depressant 300g / t.
[0087] The obtained petroleum coke concentrate had a carbon grade of 78.13% and a carbon recovery rate of 90.06%, the rutile concentrate had a TiO2 grade of 86.26% and a TiO2 recovery rate of 91.93%, and the quartz concentrate had a SiO2 grade of 56.93%.
[0088] Example 4
[0089] Prepare flotation slurry; add water to inert titanium tetrachloride waste residue with C grade of 36.62% and TiO2 grade of 24.13% and stir to concentrate it into a flotation slurry of 20% to 30%;
[0090] Petroleum coke separation: Petroleum coke collector is added for flotation to obtain petroleum coke concentrate and decarbonized tailings. This operation section adopts a one-roughing and two-scavenging process. The amount of petroleum coke collector added is calculated per ton of waste residue: 600g / t for roughing, 200g / t for scavenging one, and 300g / t for scavenging two.
[0091] Rutile Separation: The decarbonized tailings concentration is 60%. Rutile flotation reagents are added for flotation to obtain rutile concentrate and quartz concentrate. This operation section adopts a flotation process of one rougher, one scavenger, and four cleaners. The dosage of rutile flotation reagents is calculated per ton of raw ore: rougher gangue depressant 2000g / t, main collector 3000g / t, auxiliary collector 500g / t; scavenger gangue depressant 600g / t, main collector 1500g / t, auxiliary collector 100g / t~300g / t; cleaner 1 gangue depressant 0g / t; cleaner 2 gangue depressant 300g / t; cleaner 3 gangue depressant 800g / t; cleaner 4 gangue depressant 300g / t.
[0092] The obtained petroleum coke concentrate had a carbon grade of 78.13% and a carbon recovery rate of 90.06%, the rutile concentrate had a TiO2 grade of 90.05% and a TiO2 recovery rate of 93.86%, and the quartz concentrate had a SiO2 grade of 56.98%.
[0093] Example 5
[0094] Prepare flotation slurry; add water to inert titanium tetrachloride waste residue with C grade of 36.62% and TiO2 grade of 24.13% and stir to concentrate it into a flotation slurry of 20% to 30%;
[0095] Petroleum coke separation: Petroleum coke collector is added for flotation to obtain petroleum coke concentrate and decarbonized tailings. This operation section adopts a one-roughing and two-scavenging process. The amount of petroleum coke collector added is calculated per ton of waste residue: 600g / t for roughing, 200g / t for scavenging one, and 300g / t for scavenging two.
[0096] Rutile Separation: The decarbonized tailings concentration is 60%. Rutile flotation reagents are added for flotation to obtain rutile concentrate and quartz concentrate. This operation section adopts a flotation process of one rougher, one scavenger, and four cleaners. The dosage of rutile flotation reagents is calculated per ton of raw ore as follows: rougher gangue depressant dosage is 2000 g / t, main collector dosage is 2500 g / t, auxiliary collector dosage is 800 g / t; scavenger gangue depressant dosage is 600 g / t, main collector dosage is 1500 g / t, auxiliary collector dosage is 100 g / t to 300 g / t; cleaner 1 gangue depressant dosage is 0 g / t; cleaner 2 gangue depressant dosage is 800 g / t; cleaner 3 gangue depressant dosage is 800 g / t; cleaner 4 gangue depressant dosage is 800 g / t.
[0097] The obtained petroleum coke concentrate had a carbon grade of 78.13% and a carbon recovery rate of 90.06%, the rutile concentrate had a TiO2 grade of 89.16% and a TiO2 recovery rate of 89.86%, and the quartz concentrate had a SiO2 grade of 54.98%.
[0098] Example 6
[0099] Prepare flotation slurry; add water to inert titanium tetrachloride waste residue with C grade of 36.62% and TiO2 grade of 24.13% and stir to concentrate it into a flotation slurry of 20% to 30%;
[0100] Petroleum coke separation: Petroleum coke collector is added for flotation to obtain petroleum coke concentrate and decarbonized tailings. This operation section adopts a one-roughing and two-scavenging process. The amount of petroleum coke collector added is calculated per ton of waste residue: 600g / t for roughing, 200g / t for scavenging one, and 300g / t for scavenging two.
[0101] Rutile Separation: The decarbonized tailings concentration is 60%. Rutile flotation reagents are added for flotation to obtain rutile concentrate and quartz concentrate. This operation section adopts a flotation process of one rougher, one scavenger, and four cleaners. The dosage of rutile flotation reagents is calculated per ton of raw ore as follows: rougher gangue depressant dosage is 1500 g / t, main collector dosage is 4000 g / t, auxiliary collector dosage is 800 g / t; scavenger gangue depressant dosage is 1000 g / t, collector dosage is 1500 g / t, auxiliary collector dosage is 300 g / t; cleaner 1 gangue depressant dosage is 0 g / t; cleaner 2 gangue depressant dosage is 800 g / t; cleaner 3 gangue depressant dosage is 300 g / t; cleaner 4 gangue depressant dosage is 300 g / t.
[0102] The obtained petroleum coke concentrate had a C grade of 78.13% and a C recovery rate of 90.06%, the rutile concentrate had a TiO2 grade of 89.86% and a TiO2 recovery rate of 93.34%, and the quartz concentrate had a SiO2 grade of 55.58%.
[0103] Comparative Example 1
[0104] Similar to the steps in Example 1, the only difference is that the tailings after decarbonization are subjected to gravity separation to recover rutile, resulting in a rutile concentrate with a TiO2 grade of 80.79% and a TiO2 recovery rate of only 54.97%.
[0105] The main reason is that the mineral particles in the waste residue after decarbonization are relatively fine, and the fine-grained rutile cannot be effectively recovered by gravity separation.
[0106] Comparative Example 2
[0107] Similar to the steps in Example 1, the only difference is that the rutile sorting process is changed to a one-roughing, four-refining stage. The rutile sorting yielded a rutile concentrate with a TiO2 grade of 91.26% and a TiO2 recovery rate of 56.38%.
[0108] Because the rutile sorting process reduced the scavenging stage, the rutile in the inert waste was not fully recovered, resulting in a decrease in TiO2 recovery rate of the rutile concentrate despite an increase in concentrate grade.
[0109] Comparative Example 3
[0110] Similar to the steps in Example 1, the only difference is that the amount of roughing collector used in the rutile separation stage is changed to 5000 g / t. The TiO2 grade of the rutile concentrate obtained from the rutile separation is 88.21%, and the TiO2 recovery rate is 90.26%.
[0111] Comparative Example 4
[0112] Similar to the steps in Example 1, the only difference is that the amount of gangue inhibitor used in the roughing stage of rutile separation is changed to 1000 g / t. The TiO2 grade of the rutile concentrate after rutile separation is 86.11%, and the TiO2 recovery rate is 82.86%.
[0113] Comparative Example 5
[0114] The difference between this comparative example and Example 1 is that the flotation pulp concentration is adjusted to 40%, while the other conditions are the same as in Example 1.
[0115] The final petroleum coke concentrate had a C grade of 73.42% and a C recovery rate of 89.28%, the rutile concentrate had a TiO2 grade of 85.84% and a TiO2 recovery rate of 85.93%, and the quartz concentrate had a SiO2 grade of 53.93%.
[0116] Due to the high pulp concentration, the viscosity of the petroleum coke flotation separation system is too high, resulting in a significant decrease in the grade of petroleum coke. The excessively high concentration also leads to insufficient reagent dosage in the rutile flotation system, resulting in a decline in both rutile quality and recovery rate.
[0117] Comparative Example 6
[0118] The difference between this comparative example and Example 1 is that the flotation pulp concentration is adjusted to 15%, while the other conditions are the same as in Example 1.
[0119] The final petroleum coke concentrate had a C grade of 73.87% and a C recovery rate of 87.32%, the rutile concentrate had a grade of 90.23% and a TiO2 recovery rate of 91.42%, and the quartz concentrate had a SiO2 grade of 54.72%.
[0120] Due to the low pulp concentration, the probability of contact between the reagents and minerals in the petroleum coke flotation separation system decreases, resulting in the collector carrying a large amount of sludge to the surface.
[0121] Comparative Example 8
[0122] The difference from Example 1 is in the concentration process: the concentration operation requires the pulp concentration to be controlled at 30%, while the other conditions are the same as in Example 1;
[0123] The final petroleum coke concentrate had a C grade of 78.92% and a C recovery rate of 91.28%, the rutile concentrate had a TiO2 grade of 80.16% and a TiO2 recovery rate of 80.29%, and the quartz concentrate had a SiO2 grade of 49.78%.
[0124] Due to the low concentration, the slurry flow rate in the rutile flotation system increases, resulting in insufficient flotation time and a significant decrease in rutile recovery.
[0125] Comparative Example 9
[0126] The difference from Example 1 is in the concentration process: the concentration operation requires the pulp concentration to be controlled at 80%, while the other conditions are the same as in Example 1;
[0127] The final petroleum coke concentrate had a C grade of 78.73% and a C recovery rate of 90.88%, the rutile concentrate had a TiO2 grade of 87.07% and a TiO2 recovery rate of 89.49%, and the quartz concentrate had a SiO2 grade of 51.73%.
[0128] Due to the high concentration, the viscosity of the rutile flotation system pulp increases, the aeration and stirring pressure of the flotation machine is high, the flotation foam has poor fluidity, resulting in excessive entrainment of slime or gangue, leading to a decrease in grade and a decrease in recovery rate.
[0129] Using the flotation process provided in this embodiment of the invention, petroleum coke concentrate with a C grade of 78.13%, rutile concentrate with a TiO2 grade of 89.36%, and quartz concentrate with a SiO2 grade of 55.03% were obtained from titanium tetrachloride inert waste residue. The TiO2 yield was increased by 30% compared to gravity separation. The flotation effect was significantly improved, effectively increasing the comprehensive utilization rate of solid waste resources, and all product indicators were greatly improved.
[0130] Analysis of the results of the embodiments and comparative examples of the present invention leads to the following conclusions:
[0131] (1) High product quality. The method for comprehensive recycling of titanium tetrachloride inert waste provided by this invention yields rutile concentrate with a grade approximately 9% higher than that obtained by the flotation + gravity separation combined process. The recovered rutile TiO2 grade is greater than 85%, the petroleum coke concentrate C grade is greater than 75%, and the quartz sand concentrate grade is greater than 50%, all of which can be sold as individual products.
[0132] (2) High recovery rate. The process flow and control parameters for comprehensive recycling of titanium tetrachloride inert waste provided by the present invention can quickly separate three products: petroleum coke, rutile and quartz. The recovery rates of petroleum coke and rutile are both greater than 85%, and the recovery rate of rutile is 36.88% higher than that of gravity separation.
[0133] (3) Achieving the reduction and resource utilization of titanium tetrachloride inert waste residue solid waste. The present invention provides a comprehensive recycling method for titanium tetrachloride inert waste residue, which produces products with stable quality and high indicators. The production control is simple and easy to implement, providing a demonstration line for the comprehensive recycling of solid waste resources in my country;
[0134] (4) The process is simple and efficient. Petroleum coke concentrate is obtained by one roughing and two scavenging flotation process, and rutile concentrate and quartz concentrate are obtained by one roughing, one scavenging and four cleaning flotation process. The two-stage full flotation process uses unified separation equipment and is easy to operate, which increases the processing capacity per unit time by 300% compared with gravity separation.
[0135] In summary, the comprehensive recycling method for inert titanium tetrachloride waste provided in this invention, combined with relevant flotation reagents, can extract three high-quality products: petroleum coke concentrate, rutile concentrate, and quartz concentrate. Furthermore, the ore recovery rate is high, with no other byproducts, effectively utilizing mineral resources. The flotation method provided by this invention is simple and easy to implement, with a straightforward on-site process, strong feasibility, low production cost, and broad application prospects.
[0136] The above are merely preferred embodiments of the present invention and are not intended to limit the present invention. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.
Claims
1. A method for comprehensive recycling and utilization of titanium tetrachloride inert waste residue, characterized in that, Includes the following steps: (1) Pulping: Titanium tetrachloride inert waste residue is mixed with water and stirred to obtain mineral slurry; (2) Flotation of petroleum coke: The slurry from step (1) enters the petroleum coke flotation system and adopts a process flow of one roughing and two scavenging to obtain petroleum coke concentrate and flotation tailings. During the flotation of petroleum coke, the slurry concentration is controlled at 25%~30%. (3) Concentration: The flotation tailings from step (2) are fed into a thickener for concentration and dewatering to obtain concentrated underflow product. The concentration of the concentrated underflow product is controlled at 45% to 70%. (4) Flotation of rutile: The concentrated underflow product from step (3) enters the rutile flotation system and adopts a process flow of one roughing, one scavenging and four cleaning to obtain rutile concentrate and quartz concentrate. During the rutile flotation process, the pulp concentration is controlled at 45%~70%.
2. The method for comprehensive recycling and utilization of titanium tetrachloride inert waste residue according to claim 1, characterized in that, The titanium tetrachloride inert waste residue contains petroleum coke concentrate with a carbon grade of 30%~50% and rutile concentrate with a TiO2 grade of 22%~35%.
3. The method for comprehensive recycling and utilization of titanium tetrachloride inert waste residue according to claim 1, characterized in that, Step (1) The pulping process controls the pulp concentration at 15%~40%.
4. The method for comprehensive recycling of titanium tetrachloride inert waste residue according to claim 3, characterized in that, The pulping process controls the pulp concentration to be between 20% and 35%.
5. The method for comprehensive recycling and utilization of titanium tetrachloride inert waste residue according to claim 3, characterized in that, The pulping process controls the pulp concentration at 25% to 30%.
6. The method for comprehensive recycling of titanium tetrachloride inert waste residue according to claim 1, characterized in that, The reagent used for flotation of petroleum coke is a petroleum coke collector, specifically the KL collector produced by the Changsha Design Institute of the Ministry of Chemical Industry.
7. The method for comprehensive recycling of titanium tetrachloride inert waste residue according to claim 6, characterized in that, The crude selection amount of the petroleum coke collector is 400g / t~800g / t, the first scavenging amount is 100g / t~300g / t, and the second scavenging amount is 200g / t~400g / t.
8. The method for comprehensive recycling of titanium tetrachloride inert waste residue according to claim 6, characterized in that, The crude selection amount of the petroleum coke collector is 600 g / t, the first scavenging amount is 200 g / t, and the second scavenging amount is 300 g / t.
9. The method for comprehensive recycling of titanium tetrachloride inert waste residue according to claim 1, characterized in that, Step (3) Concentration: Concentration and dehydration are carried out using an inclined plate thickener.
10. The method for comprehensive recycling of titanium tetrachloride inert waste residue according to claim 1, characterized in that, Rutile flotation reagents include gangue inhibitors, primary collectors, and secondary collectors.
11. The method for comprehensive recycling of titanium tetrachloride inert waste residue according to claim 10, characterized in that, The gangue inhibitor includes one or two of oxalic acid, sodium fluorosilicate, and sodium silicate.
12. The method for comprehensive recycling and utilization of titanium tetrachloride inert waste residue according to claim 11, characterized in that, The gangue inhibitor is a compound of oxalic acid and sodium silicate.
13. The method for comprehensive recycling and utilization of titanium tetrachloride inert waste residue according to claim 11, characterized in that, The mass ratio of oxalic acid to sodium silicate is 40:
60.
14. The method for comprehensive recycling of titanium tetrachloride inert waste residue according to claim 11, characterized in that, The sodium silicate has a modulus of 2.9 and is in liquid form.
15. The method for comprehensive recycling of titanium tetrachloride inert waste residue according to claim 11, characterized in that, The dosage of gangue inhibitor for roughing is 1500g / t~3000g / t, the dosage of gangue inhibitor for scavenging is 600g / t~1000g / t, the dosage of gangue inhibitor for scavenging is 300g / t~800g / t, the dosage of gangue inhibitor for scavenging is 300g / t~800g / t, the dosage of gangue inhibitor for scavenging is 300g / t~800g / t, and the dosage of gangue inhibitor for scavenging is 300g / t~800g / t.
16. The method for comprehensive recycling and utilization of titanium tetrachloride inert waste residue according to claim 11, characterized in that, Coarse selection gangue inhibitor 2000g / t, scavenging gangue inhibitor 800g / t, refined gangue inhibitor 0g / t, refined gangue inhibitor 500g / t, refined gangue inhibitor 500g / t, refined gangue inhibitor 500g / t, refined gangue inhibitor 500g / t, refined gangue inhibitor 500g / t.
17. The method for comprehensive recycling of titanium tetrachloride inert waste residue according to claim 10, characterized in that, The main collector is a modified fatty acid.
18. The method for comprehensive recycling of titanium tetrachloride inert waste residue according to claim 17, characterized in that, The modified fatty acid is HB-T3 produced by Hebei Hengyuan Oil Factory.
19. The method for comprehensive recycling of titanium tetrachloride inert waste residue according to claim 17, characterized in that, The dosage of the main collector in the roughing process is 2500g / t~4000g / t, and the dosage of the main collector in the scavenging process is 800g / t~1500g / t.
20. The method for comprehensive recycling of titanium tetrachloride inert waste residue according to claim 17, characterized in that, The main collector dosage for roughing is 3000 g / t, and the main collector dosage for scavenging is 1000 g / t.
21. The method for comprehensive recycling of titanium tetrachloride inert waste residue according to claim 10, characterized in that, The auxiliary collector is diesel oil.
22. The method for comprehensive recycling of titanium tetrachloride inert waste residue according to claim 21, characterized in that, The dosage of the roughing auxiliary collector is 400g / t~800g / t, and the dosage of the scavenging auxiliary collector is 100g / t~300g / t.
23. The method for comprehensive recycling of titanium tetrachloride inert waste residue according to claim 21, characterized in that, The dosage of the roughing auxiliary collector is 600 g / t, and the dosage of the scavenging auxiliary collector is 200 g / t.
Citation Information
Patent Citations
Resource utilization method of chlorination process titanium dioxide chlorination dust collection slag
CN114377860A
Method for separating and recycling chlorination process titanium dioxide ore coking black slag
CN115487933A
Chlorinated waste residue recovery treatment method and application thereof
CN115999764A
Treatment method of titanium dioxide chloridizing roasting slag
CN117000418A