A conductive paste and its application

By using glass and conductive materials with specific chemical composition in the conductive paste, the problem of poor corrosion and adhesion effect of conductive paste during the electroplating process is solved, the stability of the conductive layer and the plating characteristics are improved, and the electronics are satisfied Production requirements for components.

CN118136305BActive Publication Date: 2024-11-08FOSHAN SHUNDE BAIRUIXIN ELECTRONIC MATERIAL CO LTD
View PDF 14 Cites 0 Cited by

Patent Information

Application Number
CN202410236259.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-02-29
Publication Date
2024-11-08
Estimated Expiration
2044-02-29

Smart Images

  • Figure BDA0004726283100000081
    Figure BDA0004726283100000081
  • Figure BDA0004726283100000091
    Figure BDA0004726283100000091
  • Figure BDA0004726283100000092
    Figure BDA0004726283100000092
Patent Text Reader

Abstract

The present invention provides a conductive paste and its application, the conductive paste comprises a conductive material, glass, and a color developer, the chemical composition of the glass comprises: boron oxide, silicon dioxide, and manganese monoxide; the mass ratio of boron oxide to silicon dioxide is 1.2-1.8:1, and the proportion of manganese monoxide in the glass is not higher than 20wt%. The conductive paste has excellent adhesion performance and is conducive to subsequent electroplating treatment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of electronic functional materials, and in particular, relates to a conductive paste and application thereof. Background Art

[0002] Conductive paste is an important and indispensable material in modern electronic products. Most electrical components are connected to the circuit board through the conductor formed by metallization of the conductive paste. Glass is the bonding phase of the conductive paste. It bonds the conductive paste to the circuit board during the sintering process. Therefore, the choice of glass will affect the adhesion between the conductive paste and the electrical components. For electrical components that need to be electroplated later, the glass in the conductive paste is easily corroded in the plating solution, causing the electronic components to fail during the application process.

[0003] Therefore, it is necessary to seek a conductive paste with good electroplating properties and convenient for subsequent electroplating. Summary of the invention

[0004] The object of the present invention is to provide a conductive paste and application thereof, wherein the conductive paste has excellent electroplating properties and is beneficial to subsequent electroplating treatment.

[0005] According to one aspect of the present invention, a conductive paste is provided, comprising a conductive material, glass, and a color developer. The chemical composition of the glass comprises: boron oxide (B2O3), silicon dioxide (SiO2), and manganese monoxide (MnO); the mass ratio of boron oxide to silicon dioxide is 1.2 to 1.8:1, and the proportion of manganese monoxide in the glass is not higher than 20wt%. The conductive paste provided by the present invention has excellent adhesion performance, and has good electroplating characteristics after the conductive paste is formed, which is beneficial to subsequent electroplating treatment. When the chemical composition and ratio of the glass meet the above conditions, the softening point of the glass is moderate and the corrosion resistance of the plating solution is good. Therefore, when the conductive paste is prepared by the above glass, the adhesion performance between the conductive paste and the substrate coated with the conductive paste can be improved. At high temperature, the glass will be fused with a small amount of oxide components in the substrate, so that the conductive paste and the substrate are firmly bonded and not easy to fall off, meeting the needs of refined and large-scale mass production. In addition, the inventors found that when the chemical composition of the glass meets the above requirements, the glass has good corrosion resistance to plating solution, is not easily dissolved by strongly acidic or alkaline plating solutions, can withstand the electroplating process, and has a good adhesion effect, thereby improving the electroplating characteristics of the conductive paste. If the mass ratio of B2O3 to SiO2 in the chemical composition of the glass is less than 1.2, the softening point of the glass is too high. Under the same environmental conditions, the bonding performance of the glass decreases, which easily leads to poor adhesion between the conductive paste and the substrate. Moreover, the sintering performance of the conductive paste is poor at this time, and there are many pores in the conductive layer formed after sintering and curing. The plating solution easily penetrates into the conductive layer through the pores, causing the electronic components to fail during the application process. If the mass ratio of B2O3 to SiO2 in the chemical composition of the glass is greater than 1.8, the glass has poor corrosion resistance to plating solution. After the glass is corroded by the plating solution, the structural stability of the conductive layer formed by the conductive paste is poor, and the adhesion effect between the substrate and the conductive adhesive cannot be ensured. In addition, MnO in the glass can have a synergistic effect with B2O3 and SiO2. If the MnO content is too high, the reaction between the glass and the substrate will be excessive, and a large amount of heat will be released during the welding process. The conductive layer formed by the conductive paste and the substrate will easily crack, affecting the stability of the overall structure.

[0006] Preferably, the chemical composition of the glass further includes zinc oxide (ZnO) and aluminum oxide (Al2O3), wherein the proportion of zinc oxide in the glass is not higher than 15wt%, and the proportion of aluminum oxide in the glass is not higher than 20wt%. Introducing the above components into the glass can improve the adhesion of the conductive paste, that is, promote the strong adhesion between the conductive paste and the substrate. If the addition amount of ZnO and / or Al2O3 in the glass is too high, the glass is easy to crystallize, which makes the fluidity of the conductive paste worse, thereby affecting the adhesion and electroplating characteristics of the conductive paste.

[0007] Preferably, the proportion of boron oxide in the glass is 14-30 wt %.

[0008] Preferably, the chemical composition of the glass further includes a first component, the first component is at least one of calcium oxide (CaO), strontium oxide (SrO), and barium oxide (BaO), and the first component accounts for no more than 60wt% of the glass. Introducing the first component into the glass can improve the welding heat resistance of the conductive paste, and after the conductive paste is cured to form a conductive layer, the structural stability of the conductive layer is good. If the content of the first component is too much, the reaction between the glass and the substrate is excessive, a large amount of heat will be released during the welding process, and the conductive layer formed by the conductive paste and the substrate are prone to cracks, that is, the welding heat resistance of the conductive paste is reduced, which is easy to affect the overall structural stability.

[0009] Preferably, the chemical composition of the glass includes 30-60wt% of the first component and 0.1-20wt% of manganese monoxide, calculated by mass percentage. By optimizing the minimum addition amount of the first component and manganese monoxide, the bonding performance of the glass can be improved, that is, the adhesion of the conductive paste can be improved, thereby promoting a firm fit between the conductive paste and the substrate. If the content of the first component and / or MnO is too little, the reaction activity between the glass and the substrate is reduced, thereby affecting the adhesion effect between the conductive paste and the substrate, and the adhesion is reduced.

[0010] Preferably, the average particle size of the glass is 2 to 5 μm.

[0011] Preferably, the method for preparing glass includes the following operations: weighing raw materials for preparing glass according to amount, keeping the raw materials for preparing glass at a temperature of 1400-1600°C for 0.5-1.5 hours to obtain a melt; transferring the melt to an environment of 0-30°C to cool and shape, thereby obtaining glass.

[0012] Preferably, the average particle size of the conductive material is 0.3 to 10 μm. When a conductive material in the above-mentioned particle size range is used to prepare a conductive paste, the conductive paste has good conductivity, and the conductive layer formed by the conductive paste has good structural stability. In particular, when the above-mentioned conductive material is combined with glass with an average particle size of 2 to 5 μm to prepare a conductive material, the adhesion effect between the conductive paste and the substrate is good. If the average particle size of the conductive material is too small, the conductive material will shrink during the sintering and curing process to form a conductive layer, which may easily lead to cracks in the conductive layer, and the plating solution may penetrate into the cracks, thereby affecting the structural stability of the conductive layer. If the average particle size of the conductive material is too large, gaps may easily exist between the conductive materials and between the conductive material and the glass, resulting in a decrease in the compactness of the conductive layer, and it is also easy to cause the plating solution to penetrate into the conductive layer, resulting in a decrease in the adhesion effect.

[0013] Preferably, the conductive material includes at least one of silver (Ag), gold (Au), copper (Cu), nickel (Ni), platinum (Pt), and palladium (Pd).

[0014] Preferably, the vehicle comprises a resin and a solvent.

[0015] Preferably, calculated by mass ratio, resin:solvent=60-80:20-40.

[0016] Preferably, the conductive material accounts for 60-80% of the conductive paste according to the mass ratio, and the mass ratio of the glass to the conductive material is 0.03-0.15: 1. Preferably, the method for preparing the conductive paste comprises the following operations: weighing raw materials for preparing the conductive paste according to the amount, mixing the raw materials for preparing the conductive paste at a temperature of 25-35° C. to obtain the conductive paste.

[0017] According to another aspect of the present invention, there is provided a use of the conductive paste in an electronic device. DETAILED DESCRIPTION

[0018] In order to enable those skilled in the art to better understand the technical solutions of the present invention, the technical solutions of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.

[0019] Example 1

[0020] (1) Preparation of glass

[0021] Calculated by mass percentage, the raw materials used to prepare the glass include: B2O3 14wt%, SiO2 10wt%, ZnO14wt%, Al2O3 15wt%, MnO 3wt%, SrO 44wt%. It is calculated that the mass ratio of B2O3 to SiO2 is 1.4:1, and the first component accounts for 44wt% in the glass.

[0022] The method for preparing glass includes the following operations:

[0023] Weighing raw materials for preparing glass according to amount, and keeping the raw materials for preparing glass at a temperature of 1500° C. for 1 hour to obtain a melt;

[0024] The melt was transferred to water at 20°C for water cooling and cooling to obtain glass. The glass was then crushed using a ball mill to obtain glass with an average particle size of 2 μm.

[0025] (2) Preparation of conductive paste

[0026] Calculated by mass percentage, the raw materials used to prepare the conductive paste include: 70wt% conductive material, 4.9wt% of the above-mentioned glass, and 25.1wt% color developer. Among them, the conductive material is copper powder with an average particle size of 2μm, and the color developer is resin and solvent, and the mass ratio of resin to solvent is 7:3. In other embodiments, the type of conductive material, the type of resin and solvent, and the ratio of resin to solvent can be adjusted according to different needs, provided that the normal use of the conductive paste is not affected.

[0027] The preparation method of the conductive paste includes the following operations: weighing raw materials for preparing the conductive paste according to quantity, putting the raw materials for preparing the conductive paste into a three-roll pulping machine, and kneading at a temperature of 25 to 35° C. to obtain a conductive paste.

[0028] Example 2

[0029] This embodiment refers to the preparation method provided in Example 1 to prepare a conductive paste. The difference between this embodiment and Example 1 is that in the process of preparing glass, the mass ratio of B2O3 to SiO2 is 1.2:1. The other raw material ratios and preparation methods are strictly consistent with those in Example 1.

[0030] Example 3

[0031] This embodiment refers to the preparation method provided in Example 1 to prepare a conductive paste. The difference between this embodiment and Example 1 is that in the process of preparing glass, the mass ratio of B2O3 to SiO2 is 1.8:1. The other raw material ratios and preparation methods are strictly consistent with those in Example 1.

[0032] Example 4

[0033] This embodiment refers to the preparation method provided in Example 1 to prepare a conductive paste. The difference between this embodiment and Example 1 is that in the process of preparing glass, the feeding amount of MnO is adjusted to 0.1wt%. The other raw material ratios and preparation methods are strictly consistent with those in Example 1.

[0034] Example 5

[0035] This embodiment refers to the preparation method provided in Example 1 to prepare a conductive paste. The difference between this embodiment and Example 1 is that in the process of preparing glass, the feeding amount of MnO is adjusted to 20wt%. The other raw material ratios and preparation methods are strictly consistent with those in Example 1.

[0036] Example 6

[0037] This embodiment refers to the preparation method provided in Example 1 to prepare a conductive paste. The difference between this embodiment and Example 1 is that in the process of preparing glass, the feed amount of ZnO is adjusted to 20wt%, and Al2O3 is omitted from the raw materials for preparing glass. The remaining raw material ratios and preparation methods are strictly consistent with those in Example 1.

[0038] Example 7

[0039] This embodiment refers to the preparation method provided in Example 1 to prepare a conductive paste. The difference between this embodiment and Example 1 is that in the process of preparing glass, the feed amount of Al2O3 is adjusted to 25wt%. The other raw material ratios and preparation methods are strictly consistent with Example 1.

[0040] Example 8

[0041] This embodiment refers to the preparation method provided in Example 1 to prepare a conductive paste. The difference between this embodiment and Example 1 is that in the process of preparing glass, the feed amount of the first component is adjusted to 25wt%. The other raw material ratios and preparation methods are strictly consistent with Example 1.

[0042] Example 9

[0043] This embodiment refers to the preparation method provided in Example 1 to prepare a conductive paste. The difference between this embodiment and Example 1 is that in the process of preparing glass, the feed amount of the first component is adjusted to 30wt%. The other raw material ratios and preparation methods are strictly consistent with Example 1.

[0044] Example 10

[0045] This embodiment refers to the preparation method provided in Example 1 to prepare a conductive paste. The difference between this embodiment and Example 1 is that in the process of preparing glass, the feed amount of the first component is adjusted to 60wt%. The other raw material ratios and preparation methods are strictly consistent with Example 1.

[0046] Embodiment 11

[0047] This embodiment refers to the preparation method provided in Example 1 to prepare a conductive paste. The difference between this embodiment and Example 1 is that in the process of preparing glass, the feed amount of the first component is adjusted to 65wt%. The other raw material ratios and preparation methods are strictly consistent with Example 1.

[0048] Example 12

[0049] This embodiment refers to the preparation method provided in Example 1 to prepare a conductive paste. The difference between this embodiment and Example 1 is that in the process of preparing glass, an equal mass of CaO is used to replace SrO in Example 1. The rest of the raw material ratios and preparation methods are strictly consistent with those in Example 1.

[0050] Embodiment 13

[0051] This embodiment refers to the preparation method provided in Example 1 to prepare a conductive paste. The difference between this embodiment and Example 1 is that in the process of preparing glass, BaO of equal mass is used to replace SrO in Example 1. The rest of the raw material ratios and preparation methods are strictly consistent with Example 1.

[0052] Embodiment 14

[0053] This embodiment refers to the preparation method provided in Example 1 to prepare a conductive paste. The difference between this embodiment and Example 1 is that in the process of preparing the conductive paste, copper powder with an average particle size of 0.3 μm is used. The rest of the raw material ratios and preparation methods are strictly consistent with those in Example 1.

[0054] Embodiment 15

[0055] This embodiment refers to the preparation method provided in Example 1 to prepare a conductive paste. The difference between this embodiment and Example 1 is that in the process of preparing the conductive paste, copper powder with an average particle size of 10 μm is used. The rest of the raw material ratios and preparation methods are strictly consistent with those in Example 1.

[0056] Comparative Example 1

[0057] This comparative example refers to the preparation method provided in Example 1 to prepare a conductive paste. The difference between this comparative example and Example 1 is that in the process of preparing glass, the mass ratio of B2O3 to SiO2 is 1:1. The other raw material ratios and preparation methods are strictly consistent with Example 1.

[0058] Comparative Example 2

[0059] This comparative example refers to the preparation method provided in Example 1 to prepare a conductive paste. The difference between this comparative example and Example 1 is that in the process of preparing glass, the mass ratio of B2O3 to SiO2 is 2:1. The other raw material ratios and preparation methods are strictly consistent with Example 1.

[0060] Comparative Example 3

[0061] This comparative example refers to the preparation method provided in Example 1 to prepare a conductive paste. The difference between this comparative example and Example 1 is that in the process of preparing glass, the first component of equal mass is used to replace MnO in Example 1. The remaining raw material ratios and preparation methods are strictly consistent with Example 1.

[0062] Comparative Example 4

[0063] This comparative example refers to the preparation method provided in Example 1 to prepare a conductive paste. The difference between this comparative example and Example 1 is that in the process of preparing glass, the feeding amount of MnO is adjusted to 22wt%. The other raw material ratios and preparation methods are strictly consistent with Example 1.

[0064] Test Case

[0065] Test object: The conductive pastes provided in Examples 1 to 16 and Comparative Examples 1 to 4 were applied to 1203-sized Ni internal electrode multilayer capacitors by dip coating, and dried. Then, the conductive pastes were sintered at a set temperature of 800°C for 10 minutes under N2 atmosphere to solidify the conductive pastes into conductive layers. The internal electrode multilayer capacitors coated with the conductive pastes were then electroplated with Ni and Sn to obtain samples, which were used as test objects.

[0066] Test items and test methods:

[0067] (1) Adhesion strength: The test object is welded on a PCB substrate with wiring (substrate for adhesion strength, material: glass epoxy resin), and pressure is applied from the side at a speed of 1 mm / s. The measured breaking strength is the adhesion strength. The number of samples is 30 for each condition, and the average value is taken.

[0068] (2) Bending failure rate: Solder the test object on the wiring PCB substrate (thickness: 1.6mm) used for the bending test, and bend the substrate 2mm for 10 seconds. Then grind the test object and observe the cross section to see if there are any cracks on the test object. The number of test samples is 30 for each condition, and the bending failure rate is calculated. Bending failure rate = (number of test objects with cracks / total number of test samples) × 100%.

[0069] (3) Soldering characteristics: At 245°C, immerse the test object in a solder bath containing molten Sn-3.5Ag-0.5Cu solder for 5 seconds. The test object is judged to be qualified if the creeping area is above 95%. The number of test samples is 30 for each condition, and the soldering defect rate is calculated. Soldering defect rate = (number of test objects with unqualified creeping area / total number of test samples) × 100%.

[0070] (4) Soldering heat resistance characteristics: Immerse the test object in a molten solder bath for 3 seconds at 350°C. The solder is molten Sn-3.5Ag-0.5Cu. Observe the surface of the test object to determine whether there are cracks. The number of test samples is 30 for each condition, and the welding heat resistance failure rate is calculated. Welding heat resistance failure rate = (number of test objects with cracks / total number of test samples) × 100%.

[0071] Test results: The chemical composition and size of the products of each test object are shown in Table 1, and the test results are shown in Table 2.

[0072] Table 1. Chemical composition of glass and particle size of conductive materials in each test object

[0073]

[0074]

[0075] Table 2. Test results of each subject

[0076]

[0077]

[0078] Result analysis:

[0079] The conductive pastes provided in Examples 1 to 15 were compared with those provided in Comparative Examples 1 to 4. As shown in Table 2, compared with the corresponding test performances of Comparative Examples 1 to 4, the conductive layers formed by the conductive pastes used in the other experimental groups have excellent electroplating properties and soldering properties, among which the conductive paste provided in Example 1 has the best comprehensive properties. After electroplating with Ni and Sn, not only is the adhesion strength between the conductive layer and the substrate layer large and not easy to bend, but the conductive layer also has good welding properties and welding heat resistance properties.

[0080] Furthermore, by comparing the conductive pastes provided in Examples 1 to 3 with those provided in Comparative Examples 1 to 2, it can be found that, as the ratio of B2O3 / SiO2 increases, the electroplating properties of the conductive pastes first increase and then decrease. And when the ratio of B2O3 / SiO2 is in the range of 1.2 to 1.8, the conductive pastes exhibit excellent electroplating properties.

[0081] By comparing the test performance of Example 1 with Comparative Examples 3 to 4 in Table 2, it can be found that compared with the test performance of Comparative Examples 3 to 4, the electroplating performance of the conductive layer of Example 1 is better, which is beneficial to the subsequent electroplating treatment. This shows that when there is no MnO or the content of MnO is too high, the conductive layer formed by the conductive paste is prone to cracks, which is easy to affect the adhesion and electroplating characteristics of the conductive layer formed by the conductive paste.

[0082] The above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the protection scope of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. A conductive paste, characterized in that: The invention comprises a conductive material, glass and a color developing agent, wherein the chemical composition of the glass comprises: boron oxide, silicon dioxide, manganese monoxide, zinc oxide, aluminum oxide and a first component; the mass ratio of boron oxide to silicon dioxide is 1.2-1.8:1, the proportion of manganese monoxide in the glass is not higher than 20 wt%, the proportion of zinc oxide in the glass is not higher than 15 wt%, the proportion of aluminum oxide in the glass is not higher than 20 wt%, and the first component is at least one of calcium oxide, strontium oxide and barium oxide, and the proportion of the first component in the glass is not higher than 60 wt%.

2. The conductive paste according to claim 1, characterized in that: Calculated by mass percentage, the chemical composition of the glass includes 30-60 wt% of the first component and 0.1-20 wt% of manganese monoxide.

3. The conductive paste according to claim 1, characterized in that: The average particle size of the glass is 2-5 μm.

4. The conductive paste according to any one of claims 1 to 3, characterized in that: The method for preparing the glass comprises the following operations: Weighing raw materials for preparing the glass according to amount, and keeping the raw materials for preparing the glass at a temperature of 1400-1600° C. for 0.5-1.5 hours to obtain a melt; The melt is transferred to an environment of 0-30° C. to be cooled and shaped, thereby obtaining the glass.

5. The conductive paste according to claim 1, characterized in that: The average particle size of the conductive material is 0.3-10 μm.

6. The conductive paste according to claim 5, characterized in that: The conductive material includes at least one of silver, gold, copper, nickel, platinum and palladium.

7. The conductive paste according to any one of claims 1 to 6, characterized in that: Calculated by mass ratio, the conductive material accounts for 60-80% of the conductive paste, and the mass ratio of the glass to the conductive material is 0.03-0.15:

1.

8. Use of the conductive paste according to any one of claims 1 to 7 in electronic devices.

Citation Information

Patent Citations

  • Resistor composition

    CA1036346A

  • Paste composition for electrode, and solar cell element and solar cell

    CN103930950A

  • Conductive paste for solar cell and preparation method of conductive paste

    CN105679400A

  • Paste for high temperature sintering

    CN1066145A

  • Surface electrode silver paste for chip type resistor and preparation method for surface electrode silver paste

    CN106683746A