A method for preparing a marine flame retardant and fireproof sealing adhesive

By combining modified graphene nanomaterials with other nanomaterials, a marine flame-retardant and fireproof sealing adhesive with good flame retardancy and mechanical strength is prepared, which solves the problems of sealing adhesives in the case of fire in the existing technology. Chimney effect and low-temperature curing issues achieve good damping performance and long-term fire resistance in low-temperature environments.

CN118146750BActive Publication Date: 2024-10-01SHANGHAI HUOKE NEW MATERIAL CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410412946.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-08
Publication Date
2024-10-01
Estimated Expiration
2044-04-08

AI Technical Summary

Technical Problem

Existing marine sealing adhesives are prone to forming a chimney effect in case of fire, have insufficient flame retardant properties, are slow to cure in low-temperature environments, and have a short service life, and cannot guarantee long-term fire protection and mechanical strength.

Method used

Graphene nanomaterials are modified with fumed silica, dolomite, light calcium and other materials, combined with sodium phytate and halloysite nanotubes, to form modified reinforcing fillers and flame retardants through ultrasonic dispersion and ball mill grinding. , adding silane-terminated polyether and catalyst to prepare a marine flame-retardant and fireproof sealing adhesive with good flame retardant and mechanical strength.

Benefits of technology

It achieves good damping performance at ambient temperatures below -15°C, enhances the fire resistance and mechanical strength of the sealing adhesive, extends its service life, and improves the stability and storage period of the sealing adhesive.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004779833290000101
    Figure BDA0004779833290000101
  • Figure BDA0004779833290000111
    Figure BDA0004779833290000111
  • Figure BDA0004779833290000112
    Figure BDA0004779833290000112
Patent Text Reader

Abstract

The present invention relates to a method for preparing a marine flame retardant and fireproof sealing adhesive, and belongs to the technical field of adhesives. The method comprises the following components by weight: 20 to 30 parts of silane-terminated polyether, 20 to 25 parts of modified reinforcing fillers, 30 to 40 parts of modified flame retardants, 10 to 15 parts of plasticizers, 1 to 4 parts of coupling agents, 0.1 to 0.2 parts of catalysts, and 1 to 2 parts of smoke suppressants, wherein the modified reinforcing fillers are prepared by mixing monododecyl phosphate potassium and graphene nanomaterials modified with anthocyanin with fumed silica, dolomite, and light calcium, and the modified flame retardant is obtained by ball milling halloysite nanotubes modified with sodium phytate, rosin, and stearyl alcohol with aluminum hydroxide, magnesium hydroxide, and aluminum hypophosphite. The marine flame retardant and fireproof sealing adhesive prepared by the present invention has excellent fire resistance, flame retardancy, and mechanical strength, and has good damping performance when the ambient temperature is lower than ‑15°C.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of adhesives and relates to a method for preparing a marine flame retardant and fireproof sealing adhesive. Background Art

[0002] With the development of the shipping industry, new requirements have been put forward for the performance of ship sealing materials. In addition, since ships sail for a long time in harsh environments such as lakes and seas with changeable climates and common accidents, the materials of ship sealing components are extremely important.

[0003] Ships are large-scale transportation vehicles, so the sealing materials used on board need to have high fire resistance. Once a fire occurs, the gaps in the partitions between the cabins of the ship, the cable penetrations and other gaps can easily form a chimney effect, which becomes a pathway for the smoke and fire to spread upward. At the same time, sealing adhesives with good damping properties can help reduce the noise generated by vibration and improve the stability of the overall structure, thereby better performing its sealing function.

[0004] Fireproof sealing adhesive is a kind of adhesive material whose appearance changes with the interface of sealing materials, is difficult to flow and has basic bonding strength. It is often used to fill the gaps between various materials to play a sealing role. Polysulfide sealing adhesive, silicone sealing adhesive, epoxy sealing adhesive and polyurethane sealing adhesive are four commonly used sealing adhesives in construction and other industries. These four sealing adhesives play a great role in sealing, but at the same time, there are many shortcomings that are difficult to solve: for example, silicone sealing adhesive has poor redecoration and plasticizer is easy to migrate; the curing speed of single-component polyurethane sealing adhesive is relatively low, which will cause bubbling of the adhesive layer, forming weak links and surface stickiness; polysulfide sealing adhesive cures slowly at low temperatures, and the cured material is easily compressed and deformed, and it is easy to age and harden; rubber sealing adhesive has a strong odor; and epoxy sealant has low impact strength, very limited use temperature, and serious aging problem.

[0005] Silane-modified polyether sealing adhesives (MS sealing adhesives) have gradually become a better choice in the sealing adhesive industry because they do not require primer, are easy to operate and are reasonably priced. However, although the ordinary marine silane-modified polyether sealing adhesives on the market currently have certain flame retardant and fireproof properties, their service life is not long and they cannot guarantee long-term excellent fireproof, flame retardant properties and good mechanical strength. Summary of the invention

[0006] The object of the present invention is to provide a method for preparing a marine flame retardant and fireproof sealing adhesive, which has good flame retardancy and fireproofing properties, mechanical strength, and good damping performance under the condition that the ambient temperature is lower than -15°C.

[0007] The purpose of the present invention can be achieved through the following technical solutions:

[0008] A method for preparing a marine flame retardant and fireproof sealing adhesive, characterized in that it comprises the following steps:

[0009] S1. Pour graphene with a mass ratio of 1:40 into a potassium monododecyl phosphate aqueous solution with a concentration of 1g / L, and after ultrasonic dispersion at 25-30°C for 2h, vacuum filter and wash with deionized water. Dry the obtained solid in a 100°C constant temperature blast drying oven for 24h, immerse the dried solid in an ethanol solution of anthocyanin with a mass fraction of 1-3%, and ultrasonically treat it at 25-30°C for 1h. Dry the filter cake in a constant temperature blast drying oven at 80°C for 15h, and grind it in a ball mill at a speed of 400r / min for 2h to obtain a modified graphene nanomaterial;

[0010] Grind the fumed silica, dolomite, light calcium and modified graphene nanomaterials in a mass ratio of 1:1:(0.2-0.3):1 by a ball mill at a speed of 300 r / min for 3 h to uniformly disperse them to obtain a modified reinforcing filler;

[0011] S2, dissolving sodium phytate with deionized water to prepare a sodium phytate solution with a mass fraction of 5-10%, immersing the halloysite nanotubes in the sodium phytate solution, ultrasonically dispersing for 30 minutes, heating in a water bath to 100° C. and stirring for 1.5 hours until the solvent is completely volatilized, drying in a constant temperature blast drying oven at 80° C. for 10 hours, and then grinding the dried solid, stearyl alcohol and rosin in a mass ratio of 20: (1-1.5): 1 in a ball mill at a speed of 400 r / min for 4 hours to obtain modified halloysite nanotubes;

[0012] The modified halloysite nanotubes, aluminum hydroxide, magnesium hydroxide, and aluminum hypophosphite in a mass ratio of (10-15):10:10:(5-10) are ground by a ball mill at a speed of 300 r / min for 2 hours to make them uniformly dispersed to obtain a modified flame retardant;

[0013] S3, by weight, add 20 to 30 parts of silane-terminated polyether, 20 to 25 parts of modified reinforcing filler, and 30 to 40 parts of modified flame retardant into a mixer, evacuate to below -0.08 Pa, start a stirring paddle to stir and mix at 100 to 120° C. for 1 to 2 hours to obtain a base material;

[0014] S4, keeping the stirred base material in an environment of 120°C for 1.5h;

[0015] S5. Continue to add 10 to 15 parts of plasticizer and 1 to 2 parts of smoke suppressant to the mixer, and continue to stir and mix for 1 to 2 hours under vacuum conditions. After the mixing is completed, the moisture content in the mixture is less than 800 ppm.

[0016] S6. Cool the temperature to below 50°C, add 0.1-0.2 parts of catalyst and 1-4 parts of coupling agent into the mixer, stir and mix under vacuum conditions for 1-2 hours, wait for the materials in the mixer to cool to room temperature, empty and discharge the materials, press and fill the materials to obtain a marine flame retardant and fireproof sealing adhesive.

[0017] As a preferred technical solution of the present invention, in step S1, the fumed silica is hydrophobic and has a specific surface area of ​​200.

[0018] As a preferred technical solution of the present invention, in step S2, the inner diameter of the halloysite nanotube is 50-100 nm.

[0019] As a preferred technical solution of the present invention, in step S3, the silane-terminated polyether polymer is one of a silyl-terminated polyether and a methoxysilyl-terminated polyether.

[0020] As a preferred technical solution of the present invention, in step S5, the plasticizer includes one of dioctyl phthalate, diisononyl phthalate, and dimethyl phthalate.

[0021] As a preferred technical solution of the present invention, in step S5, the smoke suppressant is one or more of molybdenum trioxide, ammonium octamolybdate, and ferrocene.

[0022] As a preferred technical solution of the present invention, in step S6, the coupling agent is one of methyltrimethoxysilane, propyltriethoxysilane, octadecyltrimethoxysilane and isooctyltriethoxysilane.

[0023] As a preferred technical solution of the present invention, in step S6, the catalyst is one of dibutyltin diacetate, stannous octoate, and alkyne bistriphenylphosphine platinum complex.

[0024] Beneficial effects of the present invention:

[0025] (1) The use of graphene as a reinforcing filler ensures the strength of the sealing adhesive. In addition, the use of fumed silica, dolomite, and light calcium as volume-increasing fillers can not only reduce the production cost but also improve the product performance. At the same time, the surface of graphene is modified by potassium monododecyl phosphate, which can greatly improve its dispersion and binding properties in organic materials and avoid graphene agglomeration. At the same time, anthocyanins can form stable chemical bonds with graphene, thereby achieving effective modification of the graphene surface and helping to improve the compatibility of graphene with other materials. At the same time, graphene has a two-dimensional layer structure and a high specific surface area, so that it can form a dense physical isolation layer in polymer materials, play an outstanding physical isolation role, and have a certain salt spray resistance, which can increase the service life of the sealing adhesive in seawater.

[0026] (2) The surface of the fumed silica used in the reinforcing filler is hydrophobic and has good hydrophobicity. At the same time, light calcium is added as a dehydrating agent to remove excess moisture in the filler of the sealing adhesive and also to extend the storage period of the sealing adhesive.

[0027] (3) Loading sodium phytate on halloysite nanotubes with a layered structure can promote the carbonization of high molecular polymers, so that a supported carbon layer is formed on the polymer surface, which increases the stability of the carbon layer. Modified halloysite nanotubes are formed by stearyl alcohol and rosin, which improves the stability of the halloysite nanotubes. When used together with inorganic flame retardants such as aluminum hydroxide, magnesium hydroxide, and aluminum hypophosphite, the flame retardant has a better volume expansion effect, thereby enhancing the flame retardant properties of the prepared sealing adhesive. DETAILED DESCRIPTION

[0028] In order to further illustrate the technical means and effects adopted by the present invention to achieve the predetermined invention purpose, the specific implementation methods, structures, features and effects of the present invention are described in detail below in combination with the embodiments.

[0029] Example 1

[0030] S1. Pour graphene with a mass ratio of 1:40 into a potassium monododecyl phosphate aqueous solution with a concentration of 1g / L, and after ultrasonic dispersion at 25°C for 2h, vacuum filter and wash with deionized water. Dry the obtained solid in a 100°C constant temperature blast drying oven for 24h, immerse the dried solid in a 1% anthocyanin ethanol solution, ultrasonically treat it at 25°C for 1h, dry the filter cake in a 80°C constant temperature blast drying oven for 15h, and grind it in a ball mill at a speed of 400r / min for 2h to obtain a modified graphene nanomaterial;

[0031] Grind fumed silica, dolomite, light calcium and modified graphene nanomaterials in a mass ratio of 1:1:0.2:1 in a ball mill at a speed of 300 r / min for 3 h to uniformly disperse them to obtain a modified reinforcing filler;

[0032] S2, dissolving sodium phytate with deionized water to prepare a sodium phytate solution with a mass fraction of 5%, immersing halloysite nanotubes with an inner diameter of 100 nm in the sodium phytate solution, ultrasonically dispersing for 30 minutes, heating in a water bath to 100° C. and stirring for 1.5 hours until the solvent is completely volatilized, drying in a constant temperature blast drying oven at 80° C. for 10 hours, and then grinding the dried solid, stearyl alcohol and rosin in a mass ratio of 20:1:1 in a ball mill at a speed of 400 r / min for 4 hours to obtain modified halloysite nanotubes;

[0033] The modified halloysite nanotubes, aluminum hydroxide, magnesium hydroxide, and aluminum hypophosphite in a mass ratio of 10:10:10:5 were ground by a ball mill at a speed of 300 r / min for 2 hours to make them uniformly dispersed to obtain a modified flame retardant;

[0034] S3. Add 30 parts of silyl-terminated polyether, 20 parts of modified reinforcing filler and 30 parts of modified flame retardant into a mixer by weight, evacuate to below -0.08 Pa, start a stirring paddle to stir and mix at 100° C. for 1.5 hours to obtain a base material;

[0035] S4, keeping the stirred base material in an environment of 120°C for 1.5h;

[0036] S5, continue to add 15 parts of dioctyl phthalate and 1.8 parts of ferrocene into the mixer, continue to stir and mix under vacuum for 1 hour, and after mixing, the water content in the mixture is less than 800ppm;

[0037] S6. Cool the temperature to below 50°C, add 0.2 parts of dibutyltin diacetate and 3 parts of methyltrimethoxysilane into the mixer, stir and mix under vacuum conditions for 1.5 hours, wait for the materials in the mixer to cool to room temperature, empty and discharge the materials, press and fill the materials, and obtain a marine flame retardant and fireproof sealing adhesive.

[0038] Example 2

[0039] S1. Pour graphene with a mass ratio of 1:40 into a potassium monododecyl phosphate aqueous solution with a concentration of 1g / L, and after ultrasonic dispersion at 28°C for 2h, vacuum filter and wash with deionized water. Dry the obtained solid in a 100°C constant temperature blast drying oven for 24h, immerse the dried solid in a 2% anthocyanin ethanol solution, ultrasonically treat it at 28°C for 1h, dry the filter cake in a 80°C constant temperature blast drying oven for 15h, and grind it in a ball mill at a speed of 400r / min for 2h to obtain a modified graphene nanomaterial;

[0040] Grind fumed silica, dolomite, light calcium and modified graphene nanomaterials in a mass ratio of 1:1:0.25:1 in a ball mill at a speed of 300 r / min for 3 h to uniformly disperse them to obtain a modified reinforcing filler;

[0041] S2, dissolving sodium phytate with deionized water to prepare a sodium phytate solution with a mass fraction of 8%, immersing halloysite nanotubes with an inner diameter of 50 nm in the sodium phytate solution, ultrasonically dispersing for 30 minutes, heating in a water bath to 100° C. and stirring for 1.5 hours until the solvent is completely volatilized, drying in a constant temperature blast drying oven at 80° C. for 10 hours, and then grinding the dried solid, stearyl alcohol and rosin in a mass ratio of 20:1.2:1 in a ball mill at a speed of 400 r / min for 4 hours to obtain modified halloysite nanotubes;

[0042] The modified halloysite nanotubes, aluminum hydroxide, magnesium hydroxide, and aluminum hypophosphite in a mass ratio of 12:10:10:6 were ground by a ball mill at a speed of 300 r / min for 2 hours to make them uniformly dispersed to obtain a modified flame retardant;

[0043] S3. Add 25 parts of methoxysilyl-terminated polyether, 22 parts of modified reinforcing filler, and 35 parts of modified flame retardant into a mixer by weight, evacuate to below -0.08 Pa, start a stirring paddle to stir and mix at 100° C. for 1.5 hours to obtain a base material;

[0044] S4, keeping the stirred base material in an environment of 120°C for 1.5h;

[0045] S5, continue to add 13 parts of diisononyl phthalate and 1.9 parts of molybdenum trioxide into the mixer, continue to stir and mix under vacuum for 1 hour, and after mixing, the moisture content in the mixture is less than 800ppm;

[0046] S6. Cool the temperature to below 50°C, add 0.1 parts of stannous octoate and 3 parts of propyltriethoxysilane into the mixer, stir and mix under vacuum conditions for 1.5 hours, wait for the materials in the mixer to cool to room temperature, empty and discharge the materials, press and fill the materials, and obtain a marine flame retardant and fireproof sealing adhesive.

[0047] Example 3

[0048] S1. Pour graphene with a mass ratio of 1:40 into a potassium monododecyl phosphate aqueous solution with a concentration of 1g / L, and after ultrasonic dispersion at 30°C for 2h, vacuum filter and deionized water washing are performed. The obtained solid is dried in a 100°C constant temperature blast drying oven for 24h, and then the dried solid is immersed in a 3% anthocyanin ethanol solution, and ultrasonically treated at 30°C for 1h. The filter cake is placed in a 80°C constant temperature blast drying oven and dried for 15h, and then ground in a ball mill at a speed of 400r / min for 2h to obtain a modified graphene nanomaterial;

[0049] Grind fumed silica, dolomite, light calcium and modified graphene nanomaterials in a mass ratio of 1:1:0.3:1 in a ball mill at a speed of 300 r / min for 3 h to uniformly disperse them to obtain a modified reinforcing filler;

[0050] S2, dissolving sodium phytate with deionized water to prepare a sodium phytate solution with a mass fraction of 10%, immersing halloysite nanotubes with an inner diameter of 70 nm in the sodium phytate solution, ultrasonically dispersing for 30 minutes, heating in a water bath to 100° C. and stirring for 1.5 hours until the solvent is completely volatilized, drying in a constant temperature blast drying oven at 80° C. for 10 hours, and then grinding the dried solid, stearyl alcohol and rosin in a mass ratio of 20:1.5:1 in a ball mill at a speed of 400 r / min for 4 hours to obtain modified halloysite nanotubes;

[0051] The modified halloysite nanotubes, aluminum hydroxide, magnesium hydroxide, and aluminum hypophosphite in a mass ratio of 15:10:10:10 were ground by a ball mill at a speed of 300 r / min for 2 hours to make them uniformly dispersed to obtain a modified flame retardant;

[0052] S3. Add 20 parts of silyl-terminated polyether, 25 parts of modified reinforcing filler and 40 parts of modified flame retardant into a mixer by weight, evacuate to below -0.08 Pa, start a stirring paddle to stir and mix at 100° C. for 1.5 hours to obtain a base material;

[0053] S4, keeping the stirred base material in an environment of 120°C for 1.5h;

[0054] S5, continue to add 10 parts of dimethyl phthalate and 1.8 parts of ammonium octamolybdate into the mixer, continue to stir and mix under vacuum for 1.5 hours, and after mixing, the water content in the mixture is less than 800ppm;

[0055] S6. Cool the temperature to below 50°C, add 0.2 parts of alkyne bistriphenylphosphine platinum complex and 3 parts of octadecyltrimethoxysilane into the mixer, stir and mix under vacuum conditions for 2 hours, wait for the materials in the mixer to cool to room temperature, empty and discharge the materials, press and fill the materials, and obtain a marine flame retardant and fireproof sealing adhesive.

[0056] Example 4

[0057] S1. Pour graphene with a mass ratio of 1:40 into a potassium monododecyl phosphate aqueous solution with a concentration of 1g / L, and after ultrasonic dispersion at 25°C for 2h, vacuum filter and wash with deionized water. Dry the obtained solid in a 100°C constant temperature blast drying oven for 24h, immerse the dried solid in a 1% anthocyanin ethanol solution, ultrasonically treat it at 25°C for 1h, dry the filter cake in a 80°C constant temperature blast drying oven for 15h, and grind it in a ball mill at a speed of 400r / min for 2h to obtain a modified graphene nanomaterial;

[0058] Grind fumed silica, dolomite, light calcium and modified graphene nanomaterials in a mass ratio of 1:1:0.3:1 in a ball mill at a speed of 300 r / min for 3 h to uniformly disperse them to obtain a modified reinforcing filler;

[0059] S2, dissolving sodium phytate with deionized water to prepare a sodium phytate solution with a mass fraction of 7%, immersing halloysite nanotubes with an inner diameter of 100 nm in the sodium phytate solution, ultrasonically dispersing for 30 minutes, heating in a water bath to 100° C. and stirring for 1.5 hours until the solvent is completely volatilized, drying in a constant temperature blast drying oven at 80° C. for 10 hours, and then grinding the dried solid, stearyl alcohol and rosin in a mass ratio of 20:1.2:1 in a ball mill at a speed of 400 r / min for 4 hours to obtain modified halloysite nanotubes;

[0060] The modified halloysite nanotubes, aluminum hydroxide, magnesium hydroxide, and aluminum hypophosphite in a mass ratio of 15:10:10:10 were ground by a ball mill at a speed of 300 r / min for 2 hours to make them uniformly dispersed to obtain a modified flame retardant;

[0061] S3. Add 20 parts of silyl-terminated polyether, 23 parts of modified reinforcing filler and 40 parts of modified flame retardant into a mixer by weight, evacuate to below -0.08 Pa, start a stirring paddle to stir and mix at 100° C. for 1.5 hours to obtain a base material;

[0062] S4, keeping the stirred base material in an environment of 120°C for 1.5h;

[0063] S5, continue to add 11 parts of dimethyl phthalate and 1.8 parts of ferrocene into the mixer, continue to stir and mix under vacuum for 2 hours, and after mixing, the water content in the mixture is less than 800ppm;

[0064] S6. Cool the temperature to below 50°C, add 0.2 parts of dibutyltin diacetate and 4 parts of methyltrimethoxysilane into the mixer, stir and mix under vacuum conditions for 2 hours, and when the materials in the mixer are cooled to room temperature, empty the mixer to obtain a marine flame retardant and fireproof sealing adhesive.

[0065] Comparative Example 1

[0066] The difference between Comparative Example 1 and Example 1 is that no modified graphene nanomaterial is added to the reinforcing filler, and the fumed silica, dolomite and light calcium in a mass ratio of 1:1:0.2 are ground by a ball mill at a speed of 300 r / min for 3 h to make them evenly dispersed to obtain the reinforcing filler, and the other operations are the same.

[0067] Comparative Example 2

[0068] The difference between Comparative Example 2 and Example 1 is that the graphene is not modified, and the other operations are the same.

[0069] Comparative Example 3

[0070] The difference between Comparative Example 3 and Example 1 is that the halloysite nanotubes are not modified, and the other operations are the same.

[0071] Comparative Example 4

[0072] The difference between Comparative Example 4 and Example 1 is that modified halloysite nanotubes are not added to the flame retardant, and aluminum hydroxide, magnesium hydroxide, and aluminum hypophosphite in a mass ratio of 10:10:5 are ground by a ball mill at a speed of 300 r / min for 2 h to make them evenly dispersed to obtain a flame retardant, and the other operations are the same.

[0073] The performance tests of the marine flame retardant and fireproof sealing adhesives prepared in Examples 1-4 and Comparative Examples 1-4 are as follows:

[0074] 1. Limiting oxygen index According to GB / T10707-2008 "Determination of combustion performance of rubber" standard, the sample to be tested is made into a strip with a length of 130mm, a width of 6.5mm and a thickness of 3mm. It is cured at room temperature for 10min. After curing for 7d at a temperature of 23℃ and a humidity of 50%, the limiting oxygen index of the sealing adhesive is tested using an oxygen index tester;

[0075] 2. Shore hardness (Shore A): Tested in accordance with GB / T531.1-2008;

[0076] 3. Tensile shear strength: After the shear module is cured, place it at 23°C for 24 hours and then test the tensile shear strength according to the method provided in GB / T7124-2008;

[0077] 4. Water resistance: After the shear module is cured, it is placed in 30°C water for 168 hours, and then placed at 23°C for 24 hours to test the tensile shear strength (steel plate-steel plate);

[0078] 5. Salt spray resistance: After the shear module is cured, it is placed in a salt spray test chamber with a sodium chloride content of 5% and a temperature of 23°C for 500 hours, and then the tensile shear strength (steel plate-steel plate) is tested after being placed at 23°C for 24 hours;

[0079] 6. Surface drying time: Tested in accordance with GB / T 13477.5-2002;

[0080] 7. Fire resistance integrity: Tested in accordance with GB23864-2009;

[0081] 8. Test tensile strength and elongation at break according to GB / T528-2009;

[0082] 9. Flame retardancy: passed IMO FTP Code Part 5 surface flammability test.

[0083] See Table 1-2 for specific test results:

[0084] Table 1

[0085]

[0086]

[0087] Table 2

[0088]

[0089]

[0090] The marine flame retardant and fireproof sealing adhesive prepared by the method of the present invention is subjected to DMA test. The test results show that when the ambient temperature is lower than -15°C, the tangent value of the curve is greater than 0.4, indicating that the sealing adhesive has a good damping effect under conditions lower than -15°C.

[0091] It can be seen from the above that the marine fireproof sealing adhesive prepared by the method has good fireproof and flame retardant properties, as well as good salt spray resistance and water resistance.

[0092] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technical personnel in this field can make some changes or modify the technical contents disclosed above into equivalent embodiments without departing from the scope of the technical solution of the present invention. However, any brief modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention are still within the scope of the technical solution of the present invention.

Claims

1. A method for preparing a marine flame retardant and fireproof sealing adhesive, characterized in that: The following steps are involved: S1. Pour graphene with a mass ratio of 1:40 into a 1 g / L potassium monododecyl phosphate aqueous solution, disperse it by ultrasonic at 25-30 °C for 2 h, then vacuum filter it, wash it with deionized water, dry the obtained solid in a 100 °C constant temperature blast drying oven for 24 h, immerse the dried solid in an ethanol solution of anthocyanin with a mass fraction of 1-3%, and ultrasonically treat it at 25-30 °C for 1 h. Dry the filter cake in a 80 °C constant temperature blast drying oven for 15 h, and grind it in a ball mill at a speed of 400 r / min for 2 h to obtain the modified graphene nanomaterial. The fumed silica, dolomite, light calcium and modified graphene nanomaterials in a mass ratio of 1:1:(0.2-0.3):1 were ground by a ball mill at a speed of 300 r / min for 3 h to make them uniformly dispersed to obtain a modified reinforcing filler; S2. Sodium phytate was dissolved in deionized water to prepare a sodium phytate solution with a mass fraction of 5-10%, and the halloysite nanotubes were immersed in the sodium phytate solution. After ultrasonic dispersion for 30 min, the solution was heated to 100 °C in a water bath and stirred for 1.5 h until the solvent was completely volatilized. After drying in a constant temperature forced air drying oven at 80 °C for 10 h, the dried solid, stearyl alcohol and rosin with a mass ratio of 20: (1-1.5): 1 were ground in a ball mill at a speed of 400 r / min for 4 h to obtain modified halloysite nanotubes. The modified halloysite nanotubes, aluminum hydroxide, magnesium hydroxide and aluminum hypophosphite in a mass ratio of (10-15) ∶ 10 ∶ 10 ∶ (5-10) were ground by a ball mill at a speed of 300 r / min for 2 h to make them uniformly dispersed to obtain a modified flame retardant; S3. In parts by weight, add 20-30 parts of silane-terminated polyether, 20-25 parts of modified reinforcing filler, and 30-40 parts of modified flame retardant into a mixer, evacuate to below -0.08 Pa, start a stirring paddle to stir and mix at 100-120 °C for 1-2 hours to obtain a base material; S4, keeping the stirred base material in an environment of 120°C for 1.5 h; S5. Continue to add 10-15 parts of plasticizer and 1-2 parts of smoke suppressant to the mixer, and continue to stir and mix under vacuum conditions for 1-2 hours. After the mixing is completed, the moisture content in the mixture is less than 800 ppm. S6. The temperature is cooled to below 50°C, 0.1-0.2 parts of a catalyst and 1-4 parts of a coupling agent are added to the mixer, and the mixture is stirred and mixed under vacuum conditions for 1-2 hours. When the materials in the mixer are cooled to room temperature, the materials are emptied and discharged, and the materials are pressed and filled to obtain a marine flame retardant fireproof sealing adhesive, wherein the coupling agent is one of methyltrimethoxysilane, propyltriethoxysilane, octadecyltrimethoxysilane and isooctyltriethoxysilane.

2. The method for preparing the marine flame retardant and fireproof sealing adhesive according to claim 1, characterized in that: In step S1, the fumed silica is hydrophobic and has a specific surface area of ​​200.

3. The method for preparing the marine flame retardant and fireproof sealing adhesive according to claim 1, characterized in that: In step S2, the inner diameter of the halloysite nanotube is 50-100 nm.

4. The method for preparing the marine flame retardant and fireproof sealing adhesive according to claim 1, characterized in that: In step S3, the silane-terminated polyether polymer is a silyl-terminated polyether.

5. The method for preparing the marine flame retardant and fireproof sealing adhesive according to claim 1, characterized in that: In step S5, the plasticizer includes one of dioctyl phthalate, diisononyl phthalate, and dimethyl phthalate.

6. The method for preparing the marine flame retardant and fireproof sealing adhesive according to claim 1, characterized in that: In step S5, the smoke suppressant is one or more of molybdenum trioxide, ammonium octamolybdate, and ferrocene.

7. The method for preparing the marine flame retardant and fireproof sealing adhesive according to claim 1, characterized in that: In step S6, the catalyst is one of dibutyltin diacetate, stannous octoate, and alkyne bistriphenylphosphine platinum complex.

Citation Information

Patent Citations

  • Modified graphene-containing heat-conducting master batches and preparation method thereof

    CN106700520A

  • Modified silane polyether sealant and preparation method thereof

    CN109504333A

  • Degradable composite foam material with high mechanical property and preparation method thereof

    CN114437447A

  • Low-smoke-amount silicone flame-retardant sealant and preparation method thereof

    CN114774070A

  • Flame-retardant silane modified polyether sealant as well as preparation method and application thereof

    CN115449328A