Silicon-based X-ray photodetector based on titanium carbide nanofilm and preparation method thereof

The self-supported Ti3C2Tx nanofilm prepared by vacuum suction filtration using anodized aluminum substrate in an X-ray detector is combined with a single crystal silicon substrate to form a Schottky junction, which solves the problems of difficult materials and environmental pollution in the prior art. , realizes high sensitivity and stability X-ray detectors, suitable for large-scale production.

CN118156357BActive Publication Date: 2024-11-01ZHEJIANG UNIV
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410285887.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-13
Publication Date
2024-11-01
Estimated Expiration
2044-03-13

AI Technical Summary

Technical Problem

Most of the existing X-ray detector materials have high requirements for internal defects, are difficult to prepare, and have environmental pollution problems, resulting in low imaging resolution and inapplicable large-scale preparation.

Method used

The self-supported Ti3C2Tx nanofilm is prepared by vacuum suction filtration of anodized aluminum substrate and combined with a single crystal silicon substrate to form a vertical structure of silicon/Ti3C2Tx Schottky junction. The built-in electric field and the applied low-voltage electric field are used to separate the photogenerated electron holes, and By assisting the thermal electron transition by polarons, the sensitivity and stability of the detector are improved.

Benefits of technology

X-ray detectors with high sensitivity, high working stability and high light absorption are suitable for large-scale preparation, and avoid pollution from heavy metals and organic matters, and are environmentally friendly.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118156357B_ABST
    Figure CN118156357B_ABST
Patent Text Reader

Abstract

The present invention discloses a silicon-based X-ray photoelectric detector based on titanium carbide nanofilm and a preparation method thereof. The photoelectric detector comprises a silicon substrate, a self-supporting titanium carbide nanofilm, and a metal electrode. 3 C 2 T x The nanofilm is transferred to a silicon substrate to prepare an X-ray photodetector. 3 C 2 T x Absorption of X-rays by nanofilms and combined with silicon / Ti 3 C 2 T x The built-in electric field formed by the Schottky junction and the external low electric field separate the photogenerated electron-hole pairs generated by radiation. 3 C 2 T x The Schottky junction can excite Ti under X-ray irradiation. 3 C 2 T x Polarons are generated in the nanofilm, and a large number of polarons can assist hot electrons in transitioning through the Schottky barrier, ultimately resulting in an X-ray photodetector with high sensitivity, extremely low dark current, and high operating stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of photoelectric detectors, and in particular relates to a photoelectric detector based on titanium carbide (Ti3C2T x ) Nano-film silicon-based X-ray photodetector and its preparation method. Background Art

[0002] Since Roentgen first revealed the existence of X-rays in 1895, X-ray detectors have been continuously updated and iterated, and now play an important role in medical diagnosis, non-destructive testing, radiation monitoring, security inspection and security. According to the working mechanism, X-ray detectors can be divided into indirect and direct types. Indirect X-ray detectors mainly convert high-energy X-ray photons into visible fluorescence based on scintillator materials, and then convert optical signals into electrical signals through photodiodes. This type of detector often presents low-resolution imaging results due to the scattering effect of the scintillator. Direct X-ray detectors usually use traditional semiconductor materials as absorption layers (such as amorphous silicon and selenium), directly converting X-ray photons into electrons, thereby having higher conversion efficiency and imaging resolution. At present, new X-ray detection materials mainly include metal halide perovskites, lead-free perovskites, organic and inorganic materials, etc. Most of these materials have high requirements for internal defect concentrations, so they are often difficult to prepare or require high costs to prepare. In addition, the intervention of heavy metals and organic matter can easily cause environmental pollution problems, making such materials unsuitable for large-scale preparation of X-ray detectors.

[0003] The present invention proposes a method for obtaining a self-supporting Ti3C2T3 by vacuum filtration of an anodic aluminum oxide substrate (AAO). x( T x The method of forming a nanofilm of a silicon / Ti3C2T3 nanostructured film by combining the nanostructured film with a single crystal silicon substrate is shown in FIG. x The built-in electric field formed by the Schottky junction and the external low-voltage electric field separate the photogenerated electron-hole pairs generated by X-ray radiation. x Schottky junction can excite Ti3C2T under X-ray irradiation x Polarons are generated in the nanofilm, and a large number of polarons can assist hot electrons in transitioning through the Schottky barrier, making the X-ray detector highly sensitive and highly stable. x Nanofilms make large-scale and large-scale preparation feasible, and Ti3C2T x The thickness of the nanofilm can be adjusted by changing the dosage and concentration of the solution. In addition, the composition without heavy metals and organic matter makes this invention able to prevent harm and pollution to the human body and the environment. Summary of the invention

[0004] In view of the shortcomings of the prior art, the present invention provides a Ti3C2T x A nano-membrane silicon-based X-ray photodetector and a preparation method thereof, wherein the photodetector can effectively detect X-rays with a photon energy of 10-30keV, and the overall device has the advantages of high light absorption, high sensitivity, high working stability, etc.

[0005] The objective of the present invention is achieved through the following technical solutions:

[0006] In a first aspect, the present invention provides a silicon-based X-ray photodetector, comprising: a silicon substrate, a self-supporting Ti3C2T x Nano film, metal electrode; the silicon substrate has a silicon window, which promotes silicon and self-supporting Ti3C2T x Nanofilm forms Schottky junction and self-supporting Ti3C2T x The nanofilm forms an atomically flat interface with the silicon in the silicon window; the metal electrode is located at the periphery of the silicon window; the self-supporting Ti3C2T x The nanofilm forms an ohmic contact with the metal electrode, and the signal generated at the Schottky junction is led out to the PCB board through the metal electrode and the back side of the silicon substrate.

[0007] The self-supporting Ti3C2T x Nanofilm preparation process:

[0008] (1) The precursor titanium carbide aluminum powder is added to a mixed solution of lithium fluoride and dilute hydrochloric acid and stirred to etch the aluminum element of the precursor, and then centrifuged, washed with deionized water, and finally subjected to ultrasonic treatment in a cold water bath under an argon atmosphere to obtain a weakly acidic Ti3C2T x Solution;

[0009] (2) Ti3C2T x The solution was placed in a suction flask with anodized aluminum oxide (AAO) membrane as the substrate and vacuum filtered for 30-60 min at room temperature to obtain a self-supporting Ti3C2T x Nano membrane.

[0010] Preferably, the self-supporting Ti3C2T x The thickness of the nano film is 30-500nm, the thickness of the metal electrode is 60-100nm; the silicon substrate adopts single crystal silicon with high conductivity, electron mobility and high absorption coefficient.

[0011] Preferably, the concentration of the dilute hydrochloric acid is 9 mol / L, Ti3C2T x The concentration of the solution was 5 mg / mL.

[0012] Preferably, the metal electrode consists of Ti or Cr and Au.

[0013] In the second aspect, the present invention provides a Ti3C2T x A method for preparing a nanofilm silicon-based X-ray photoelectric detector, the method specifically comprising the following steps:

[0014] S1: cleaning and pre-treating the silicon substrate;

[0015] S2: Photolithography the silicon window pattern on the cleaned and pre-treated silicon substrate, etch the silicon dioxide in the silicon window, and clean the residual photoresist to obtain a photoresist that can be bonded to Ti3C2T x The nanofilm forms a silicon window for Schottky junction;

[0016] S3: photolithography and developing a metal electrode pattern on the periphery of the silicon window pattern of the silicon substrate processed in step S2, and magnetron sputtering a metal layer onto the metal electrode pattern to form a metal electrode;

[0017] S4: Direct transfer of self-supporting Ti3C2T x Nanofilm to the silicon window of the silicon substrate after step S3 treatment, add 1-2 drops of deionized water to make Ti3C2T x The nanofilm forms an ohmic contact with the metal electrode, and nitrogen purge makes Ti3C2T x The nanofilm and the silicon substrate fit tightly together to form an atomically flat interface;

[0018] The Ti3C2T x The size of the nanofilm is just right to cover the silicon window and the metal electrode;

[0019] S5: Photolithography and developing the desired Ti3C2T on the silicon substrate after processing in step S4 x Nanofilm patterning, Ti3C2T etched using inductively coupled plasma x Nanofilm patterning, washing away residual photoresist, and drying the device surface;

[0020] S6: Gallium indium alloy (GaIn) is coated on the back of the silicon substrate, and copper tape is adhered to the portion coated with GaIn to form an ohmic contact between the silicon substrate and the copper tape, and an X-ray photoelectric detector is obtained by electrically connecting the copper tape to the PCB board.

[0021] Preferably, in step S3, after magnetron sputtering the metal layer to the metal electrode pattern, the metal layer in other areas is stripped by soaking in acetone, and the residual photoresist on the metal electrode is washed away by acetone and isopropanol;

[0022] Preferably, during magnetron sputtering in step S3, Ti or Cr is sputtered first, and then Au is sputtered.

[0023] Preferably, the etching gas used in the inductively coupled plasma in step S5 is CF4 or SF6.

[0024] The beneficial effects of the present invention are as follows:

[0025] Ti3C2T x The nanofilm is self-supporting and thus easy to transfer. Its X-ray absorption capacity gradually increases with the thickness, thereby improving the device's X-ray sensitivity. x The nanofilm forms an atomically flat interface with silicon, so that the Schottky junction has an efficient electron-hole transmission channel. With the help of the built-in electric field of the Schottky junction and by applying a low voltage on both sides of the Schottky junction, the photogenerated carriers can be effectively separated, the recombination of electron-hole pairs can be avoided, and the quantum efficiency of the device can be further improved. x Schottky junction can excite Ti3C2T under X-ray irradiation x Polarons are generated in the nanofilm, and a large number of polarons can assist hot electrons in transitioning across the Schottky barrier, thereby improving the photoelectric conversion efficiency and increasing the photoresponse current of the device. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 Ti3C2T x High-resolution transmission electron microscopy image of the nanosheet.

[0027] Figure 2 Ti3C2T x Actual image of the nanomembrane, showing its self-supporting nature.

[0028] Figure 3 Ti3C2T x Scanning electron microscope image of the nanofilm.

[0029] Figure 4 Ti3C2T x Raman characterization results of nanofilms. The peaks marked in the figure are Ti3C2T x Characteristic peak.

[0030] Figure 5 It is a process flow chart of the preparation method of the present invention.

[0031] Figure 6 Based on Ti3C2T x Schematic diagram of a three-dimensional nanomembrane silicon-based X-ray photodetector.

[0032] Figure 7 Based on Ti3C2T x Schematic diagram of the cross section of a nanomembrane silicon-based X-ray photodetector.

[0033] Figure 8 Ti3C2T x High-resolution transmission electron microscopy image of a cross-section of a Ti3C2T / Si heterojunction, where the left area represents the silicon substrate and the middle area represents the Ti3C2T x Nanofilm, the right area represents the Pt (platinum) layer (covered on the Ti3C2T when the sample is processed by focused ion beam) x Nano film surface as a protective layer).

[0034] Fig. 9 , Fig.10 , Fig.11 It is based on Ti3C2T x Photocurrent response curves of the nanofilm silicon-based X-ray photodetector under X-ray irradiation with photon energies of 10keV, 20keV, and 30keV, respectively.

[0035] In the figure: 1. Ti3C2T x 1. Nanofilm; 2. Gallium-Indium alloy; 3. Metal electrode; 4. Silicon substrate; 5. Silicon dioxide oxide layer. DETAILED DESCRIPTION

[0036] The following is a complete description of the technical solutions in the embodiments of the present invention in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0037] The implementation method is described in detail below with reference to the accompanying drawings:

[0038] Example 1: Preparation of Ti3C2T x Nanofilm (thickness 30-500nm).

[0039] S1: First, add 2g lithium fluoride to 40ml dilute hydrochloric acid with a concentration of 9M, stir and mix well, then slowly add 1g titanium aluminum carbide, stir at 35°C for 24h, and after etching the aluminum layer, centrifuge the mixed solution at 3500rpm for 15min. Take the supernatant and wash it seven times with deionized water until the pH of the mixed solution reaches 6. Then, ultrasonically treat the mixed solution in a cold water bath under argon atmosphere for 1h, and finally obtain 5mg / mL Ti3C2T x The solution was stored in a refrigerator at 4 °C under argon atmosphere.

[0040] The prepared Ti3C2T xTwo drops of the solution were taken out with a dropper and added to a 20 ml test tube. After dilution with deionized water, the solution was added dropwise onto a molybdenum mesh. After drying, high-resolution transmission electron microscopy was used to characterize Ti3C2T x Nanosheets, such as Figure 1 The image shown here proves that the aluminum layer in titanium carbide is etched to obtain a single layer of Ti3C2T x Nanosheets.

[0041] S2: Take out a certain amount of Ti3C2T with a pipette x The solution was placed in a test tube, a small amount of deionized water was added, and the diluted solution was placed in a suction flask with anodized aluminum substrate (AAO) membrane as the substrate. The solution was vacuum filtered for 30-60 minutes at room temperature to finally obtain an independent self-supporting Ti3C2T x Nanofilms, such as Figure 2 As shown. Further, the Ti3C2T x Nanofilm surfaces, such as Figure 3 The results show a uniform and smooth effect. Furthermore, the Raman spectrometer was used to characterize the Ti3C2T x Raman spectra of nanofilms, such as Figure 4 As shown, the peaks marked in the figure are Ti3C2T x Characteristic peaks;

[0042] Example 2: Based on Ti3C2T x The preparation process of nanofilm silicon-based X-ray photodetectors, such as Figure 5 shown.

[0043] S1: Purchase a 4-inch n-type lightly doped single-crystal silicon wafer (silicon oxide thickness is 300nm) with a thickness of 500μm and a resistivity of 1-10Ω·cm, and place it in acetone and isopropanol for ultrasonic cleaning to remove impurity particles on the surface of the substrate.

[0044] S2: After the substrate is cleaned, use 5350 photoresist to make a silicon window pattern. The spin coating process parameters are: 500rpm pre-spin coating for 10s, 4000rpm spin coating for 60s, forming a photoresist covering layer of about 1μm thick, and place it on a heating plate at 105℃ for 5min. Use a photolithography machine to photolithography the silicon wafer with uniform photoresist. The light source of the photolithography machine is a 365nm DC mercury lamp, and the exposure time is 2s. After the exposure is completed, the silicon wafer is placed in the developer for about 30s, and it is removed with tweezers, washed with deionized water and blown dry with nitrogen to obtain a device with a 3×3mm silicon window pattern. It is placed on a heating plate at 110℃ and then baked for 5min to improve the photoresist's anti-etching ability. Then use BOE etching solution (ratio of NH4F:HF:H2O=60g:30ml:100ml) to etch the silicon dioxide in the silicon window for 180s. The device is removed and washed with deionized water. The surface is dried with nitrogen to obtain a device that can be used with Ti3C2T x The nanofilm forms a silicon window for Schottky junction;

[0045] S3: Photolithography and development of metal electrode patterns. The specific parameters are as described in S2. Use a magnetron sputtering system to first sputter 10nm Ti (or Cr) as an adhesion layer, and then sputter 80nm Au as an electrode onto the metal electrode pattern. Immerse the silicon wafer with electrodes in acetone, use the lift-off process to peel off the metal layer in other areas, use acetone and isopropanol to wash away the residual photoresist on the metal electrode, and blow dry the interface with nitrogen to obtain the device;

[0046] S4: Use pointed tweezers to tear off the desired area of ​​the self-supporting Ti3C2T in Example 1. x The nanofilm gently covers the silicon window and makes the self-supporting Ti3C2T x The nanofilm is in contact with the metal electrode and a syringe is used to x One or two drops of deionized water were dripped onto the edge of the nanomembrane, and finally nitrogen gas was blown gently across the interface to make it fit tightly;

[0047] S5: Photolithography develops the required Ti3C2T x The nanofilm pattern was etched with the parameters described in S2 using an inductively coupled plasma dry etching system (with CF4 and SF6 as etching gases) at an etching rate of 2 nm / s to etch the excess Ti3C2T x For the nanofilm, the etching time depends on Ti3C2T x The thickness of the nanofilm depends on the thickness of the nanofilm. After the etching is completed, the residual photoresist is washed away with acetone and isopropanol, and the interface is gently blown dry with nitrogen to obtain a Ti3C2T x Nano-film silicon-based X-ray detector devices;

[0048] S6: Back electrode fabrication. xThe back side of the silicon substrate of the nanofilm silicon-based X-ray detector device is coated with a gallium-indium alloy (GaIn), such as Figure 6 and Figure 7 Copper tape is glued to the part coated with GaIn to form an ohmic contact between the silicon substrate and the copper tape, and then the copper tape is connected to the corresponding PCB board. The preparation is completed by wire bonding, and finally a complete Ti3C2T based x Nanofilm's silicon-based X-ray detectors enable X-ray photoelectric response testing to be performed safely in a lead box.

[0049] Furthermore, Ti3C2T x Nanofilm silicon-based X-ray detector devices can be characterized using focused ion beam technology and high-resolution transmission electron microscopy to obtain Ti3C2T x High-resolution transmission electron microscopy images of the cross-section of a / Si heterojunction, such as Figure 8 The left area represents the silicon substrate, and the middle area represents the Ti3C2T x Nanofilm, the right area represents the Pt (platinum) layer (covered on the Ti3C2T when the sample is processed by focused ion beam) x The nanofilm surface is used as a protective layer). This image proves that Ti3C2T x The nanomembrane and the silicon substrate achieve an atomically flat interface, which helps improve the photoelectric conversion efficiency of the X-ray detector and further enhance its sensitivity.

[0050] Furthermore, Ti3C2T x The photocurrent response test of the nanofilm silicon-based X-ray photodetector was carried out under X-ray irradiation with photon energies of 10keV, 20keV, and 30keV, and the results were as follows: Fig. 9 , 10 From the results shown in Figures 1 and 11, it can be found that the X-ray detector can obtain a higher photoresponse current under the irradiation of X-rays with these three photon energies.

[0051] The above is only a preferred embodiment of the present invention. Although the present invention has been disclosed as a preferred embodiment, it is not intended to limit the present invention. Any technician familiar with the art can make many possible changes and modifications to the technical solution of the present invention by using the above disclosed methods and technical contents without departing from the scope of the technical solution of the present invention, or modify it into an equivalent embodiment of equivalent changes. Therefore, any simple modification, equivalent change and modification made to the above embodiments according to the technical essence of the present invention without departing from the content of the technical solution of the present invention still falls within the scope of protection of the technical solution of the present invention.

Claims

1. A silicon-based X-ray photodetector based on titanium carbide nanofilm, characterized in that include: Silicon substrate, self-supporting titanium carbide nanofilm, metal electrode; the silicon substrate has a silicon window, the self-supporting titanium carbide nanofilm and the silicon in the silicon window form an atomically flat interface, which promotes the formation of a Schottky junction between silicon and the self-supporting titanium carbide nanofilm; The metal electrode is located at the periphery of the silicon window; The self-supporting titanium carbide nanofilm forms an ohmic contact with the metal electrode, and the signal generated at the Schottky junction is led out to the PCB board through the metal electrode and the back of the silicon substrate; The preparation process of the self-supporting titanium carbide nanofilm: (1) The precursor titanium carbide aluminum powder is added to a mixed solution of lithium fluoride and dilute hydrochloric acid and stirred to etch the aluminum element of the precursor, and then centrifuged, washed with deionized water, and finally subjected to ultrasonic treatment in a cold water bath under an argon atmosphere to obtain a weakly acidic Ti3C2T x Solution, Ti3C2T x The concentration of the solution is 5 mg / mL; (2) Ti3C2T x The solution is placed in a suction filtration bottle with an anodic aluminum oxide substrate membrane as a substrate, and a self-supporting titanium carbide nanofilm is obtained after vacuum filtration.

2. The photodetector according to claim 1, characterized in that The thickness of the self-supporting titanium carbide nanofilm is 30-500nm.

3. The photoelectric detector according to claim 1, characterized in that The thickness of the metal electrode is 60-100 nm.

4. The photodetector according to claim 1, characterized in that The concentration of dilute hydrochloric acid in the preparation process of the self-supporting titanium carbide nanofilm is 9 mol / L.

5. The photodetector according to claim 1, characterized in that The vacuum filtration condition in the preparation process of the self-supporting titanium carbide nanofilm is vacuum filtration for 30-60 minutes at room temperature.

6. The photodetector according to claim 1, characterized in that The silicon substrate is made of single crystal silicon.

7. The photodetector according to claim 1, characterized in that The metal electrode consists of Ti and Au, or consists of Cr and Au.

8. The method for preparing the photoelectric detector according to any one of claims 1 to 7, characterized in that The method specifically comprises the following steps: S1: cleaning and pre-treating the silicon substrate; S2: Photolithography and developing a silicon window pattern on the cleaned and pre-treated silicon substrate, etching silicon dioxide in the silicon window, and cleaning the residual photoresist to obtain a silicon window that can form a Schottky junction with the titanium carbide nanofilm; S3: photolithography and developing a metal electrode pattern on the periphery of the silicon window pattern of the silicon substrate processed in step S2, and magnetron sputtering a metal layer onto the metal electrode pattern to form a metal electrode; S4: directly transferring the self-supporting titanium carbide nanofilm to the silicon window of the silicon substrate after the treatment in step S3, so that the titanium carbide nanofilm forms an ohmic contact with the metal electrode, and nitrogen purges the titanium carbide nanofilm to closely fit the silicon substrate to form an atomic-level flat interface; the size of the titanium carbide nanofilm is just enough to cover the silicon window and the metal electrode; S5: photolithographically developing the desired titanium carbide nanofilm pattern on the silicon substrate after the treatment in step S4, etching the titanium carbide nanofilm pattern using inductively coupled plasma, washing away the residual photoresist, and drying the device surface; S6: Gallium-indium alloy is coated on the back of the silicon substrate, and copper tape is adhered to the part coated with the gallium-indium alloy to form an ohmic contact between the silicon substrate and the copper tape, and an X-ray photoelectric detector is obtained by electrically connecting the copper tape to the PCB board.

9. The method according to claim 8, characterized in that In step S3, after magnetron sputtering the metal layer to the metal electrode pattern, the metal layer in other areas is stripped by soaking in acetone, and the residual photoresist on the metal electrode is washed away by acetone and isopropyl alcohol.

10. The method according to claim 8, characterized in that The etching gas used in the inductively coupled plasma in step S5 is CF4 or SF6.

Citation Information

Patent Citations

  • Silicon / graphene nanofilm / germanium-based vertical photoelectric detector and preparation method thereof

    CN114583003A

  • Semiconductor device and method of manufacturing the same

    CN115939194A

  • High-speed optical detector based on self-passivation MXene / Si Van der Waals Schottky junction

    CN116230782A

  • Preparation and application of ionic liquid / novel two-dimensional nanosheet gas separation membrane

    CN116474563A

  • X-ray detector

    US20040217295A1