A transparent glass-ceramic with high scratch resistance
By using zinc-magnesium spinel solid solution as the main crystal phase in glass-ceramics, adjusting the oxide composition and performing heat treatment, the problem of insufficient scratch resistance of glass-ceramics is solved and efficient scratch resistance improvement is achieved. , suitable for protective covers of high-end electronic products.
Patent Information
- Application Number
- CN202211666110.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-23
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2042-12-23
AI Technical Summary
The scratch resistance of existing glass-ceramics is insufficient to meet the requirements of high-end product applications, especially in protective covers for electronic equipment.
Zinc-magnesium spinel solid solution glass-ceramics whose main crystal phase is (Zn, Mg)Al2O4 is used. By adjusting the proportion of oxide components and heat treatment conditions, the glass formula is optimized to improve scratch resistance. Specifically, it includes 30.00% ≤ SiO2 < 35.00%, Al2O3 30.00% ~ 40.00%, ZnO 10.00% ~ 12.00%, MgO 2.00% ~ 4.00%, The composition of ZrO2 is 5.00% to 7.00%, Na2O is 2.00% to 9.00%, Li2O is 0 to 2.00%, and B2O3 is 0 to 8.00%, and is nucleated and crystallized to form high-strength glass-ceramics.
The scratch resistance of glass-ceramics is significantly improved, making its scratch resistance close to that of sapphire glass, which can meet the needs of high-end electronic product covers and reduce production difficulty and cost.
Smart Images

Figure CN118164677B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of glass materials, and in particular to a transparent microcrystalline glass with high scratch resistance. Background Art
[0002] Due to its excellent optical properties, glass has gradually replaced plastic as the protective cover of portable electronic devices. As the protective cover and shell material of portable electronic products such as smartphones, smart watches, and tablets, it is required to have excellent scratch resistance. At present, sapphire glass is a material with excellent compression resistance and scratch resistance. However, sapphire glass is difficult to produce and process, with high processing costs. In addition, it has low tolerance for defects and is very easy to break. Ordinary glass has low scratch resistance. Even microcrystalline glass obtained by precipitating crystalline phases such as lithium disilicate and petalite in glass has limited improvement in scratch resistance and is difficult to meet the performance requirements of higher-end products.
[0003] Based on its high Young's modulus and shear modulus, zinc-magnesium spinel crystal has become the preferred crystal phase for improving the scratch resistance of glass.
[0004] Patent CN 111615500A discloses a transparent zinc spinel-spinel glass ceramic with spinel as the main crystal phase, which has a Young's modulus greater than or equal to about 98.0 GPa to less than or equal to about 114.0 GPa, and a hardness greater than or equal to about 9.0 GPa to less than or equal to about 11.2 GPa. Although the scratch resistance of the glass ceramic in this patent is greatly improved compared to the existing microcrystalline glass, its scratch resistance, Young's modulus and hardness still cannot meet the use requirements of higher-end products. Summary of the invention
[0005] In view of the above-mentioned deficiencies in the prior art, an object of the present invention is to provide a transparent microcrystalline glass with high scratch resistance, so as to solve the problem that the scratch resistance of microcrystalline glass in the prior art is not sufficient to meet the application requirements of high-end products.
[0006] In order to solve the above technical problems, the present invention adopts the following technical solutions:
[0007] In the first aspect, the present invention provides a transparent microcrystalline glass with high scratch resistance, wherein the microcrystalline glass contains crystal grains, the main crystal phase of the microcrystalline glass is (Zn, Mg)Al2O4, and (Zn, Mg)Al2O4 is a zinc-magnesium spinel solid solution; according to the mass percentage of the oxides, the microcrystalline glass includes the following components: 30.00%≤SiO2<35.00%; Al2O3 is 30.00%-40.00%; ZnO is 10.00%-12.00%; MgO is 2.00%-4.00%; ZrO2 is 5.00%-7.00%; Na2O is 2.00%-9.00%; Li2O is 0-2.00%; B2O3 is 0-8.00%; at the same time, the content of each oxide in the microcrystalline glass also satisfies the following conditions:
[0008] ①X=((Na2O+B2O3) / ZrO2) / Al2O3, X≥2.00;
[0009] ②Y=ln[(Na2O+B2O3) / ZrO2], Y≥0;
[0010] ③Z=(SiO2+Al2O3-MgO-ZnO) / (Li2O+Na2O+B2O3), 4.00≤Z≤10.00;
[0011] In formulae ① to ③, oxide represents the mass percentage of the oxide component.
[0012] Preferably, the content of each oxide in the microcrystalline glass also satisfies the following conditions:
[0013] ④W=(0.8×(Al2O3-SiO2)+1.5×(ZnO-MgO)) / ZrO2, 0≤W≤3.00; In formula ④, oxide represents the mass percentage of the oxide component.
[0014] Preferably, in terms of the molar percentage of oxides, the microcrystalline glass satisfies the following conditions: the molar percentage of Al2O3 is greater than the sum of the molar percentages of MgO and ZnO; the theoretical crystallinity of the microcrystalline glass is at least 30.00wt%, preferably 30.00wt% to 50.00wt%.
[0015] Preferably, when the microcrystalline glass meets the theoretical crystallinity, the dissociation energy per unit volume of the residual glass phase in the microcrystalline glass is not less than 71.00 kJ·cm -3 , preferably 71.00 kJ·cm -3 ~134.00kJ·cm -3 .
[0016] Preferably, the secondary crystalline phase of the microcrystalline glass includes one or more of tetragonal ZrO2, Zn2SiO4 (zinc silicate), and Mg2SiO4 (magnesium silicate).
[0017] Preferably, in the microcrystalline glass, the mass percentage of SiO2 is 32.00% to 34.95%; and / or the mass percentage of Al2O3 is 32.00% to 38.00%; and / or ZnO is 10.00% to 11.48%; and / or MgO is 2.50% to 3.50%; and / or ZrO2 is 5.40% to 6.50%; and / or Na2O is 2.50% to 8.50%; and / or B2O3 is 2.50 to 8.00%.
[0018] Preferably, the glass-ceramics further comprises 0-3.00wt% of BaO and / or 0-2.00wt% of Y2O3.
[0019] Preferably, the microcrystalline glass is substantially free of TiO2 and / or P2O5. Here, "substantially free of" means that TiO2 and / or P2O5 are not actively added or dosed into the glass, but may exist in very small amounts as contaminants.
[0020] Preferably, in the glass-ceramics, the average grain size is ≤15.00 nm, preferably 1.00 to 10.00 nm, and more preferably 4.50 to 8.00 nm.
[0021] Preferably, in the glass-ceramics, the crystal content is 20.00 to 50.00 wt %, preferably 25.00 to 50.00 wt %, and more preferably 25.00 to 45.00 wt %.
[0022] Preferably, the Young's modulus of the glass-ceramics is not less than 110 GPa, preferably 110 to 130 GPa, more preferably greater than 114 GPa and less than or equal to 140 GPa.
[0023] Preferably, a gem mineral hardness pen with a Mohs hardness rating of 7 is fixed at an angle of 45° using an automatic pencil hardness tester, and the surface of the microcrystalline glass is scratched under a load of 500g, and the scratched microcrystalline glass is placed under a 400x microscope for observation, and there are no scratches on the surface of the microcrystalline glass;
[0024] and / or
[0025] Using an automatic pencil hardness tester and a gem mineral hardness pen with a Mohs hardness rating of 6 fixed at an angle of 45°, the surface of the microcrystalline glass was scratched under a load of 750g, and the scratched microcrystalline glass was observed under a 400x microscope. The surface of the microcrystalline glass had no scratches.
[0026] Preferably, at a thickness of 0.7 mm, for light with a wavelength of 550 nm, the transmittance of the microcrystalline glass is greater than or equal to 85.00%, and preferably the transmittance is greater than or equal to 89.00%.
[0027] Preferably, at a thickness of 0.7 mm, the optical b value of the glass-ceramics is 0.20 to 1.50, preferably 0.35 to 1.20.
[0028] Preferably, the glass-ceramics is prepared by the following method:
[0029] Step 1: Obtain substrate glass, which includes the following components in terms of mass percentage of oxides: 30.00%≤SiO2<35.00%; Al2O3 is 30.00%-40.00%; ZnO is 10.00%-12.00%; MgO is 2.00%-4.00%; ZrO2 is 5.00%-7.00%; Na2O is 2.00%-9.00%; Li2O is 0-2.00%; B2O3 is 0-8.00%; and the content of each oxide in the substrate glass also satisfies the following conditions:
[0030] ①X=((Na2O+B2O3) / ZrO2) / Al2O3, X≥2.00;
[0031] ②Y=ln[(Na2O+B2O3) / ZrO2], Y≥0;
[0032] ③Z=(SiO2+Al2O3-MgO-ZnO) / (Li2O+Na2O+B2O3), 4.00≤Z≤10.00;
[0033] In formulas ① to ③, oxide represents the mass percentage of the oxide component;
[0034] Step 2: heat-treating the substrate glass to obtain the microcrystalline glass; the heat treatment includes nucleation treatment and / or crystallization treatment.
[0035] Preferably, in step 2, when the nucleation treatment is performed, the nucleation temperature is 650° C. to 850° C., preferably 650° C. to 750° C., and the nucleation treatment time is 0 to 72 hours, preferably 0 to 24 hours.
[0036] Preferably, in step 2, when the crystallization treatment is performed, the crystallization temperature is 700° C. to 1000° C., preferably 700° C. to 850° C., and the crystallization treatment time is 0.1 to 72 h, preferably 0.1 to 24 h.
[0037] Preferably, in step 2, when heat treatment is performed, the heating rate is controlled to be 5 to 30° C. / min, preferably 5 to 15° C. / min.
[0038] Preferably, the content of each oxide in the substrate glass also satisfies the following conditions:
[0039] ④W=(0.8×(Al2O3-SiO2)+1.5×(ZnO-MgO)) / ZrO2, 0≤W≤3.00; In formula ④, oxide represents the mass percentage of the oxide component.
[0040] Preferably, the substrate glass further comprises 0-3.00wt% of BaO and / or 0-2.00wt% of Y2O3.
[0041] Preferably, the substrate glass contains substantially no TiO2 and / or P2O5.
[0042] In a second aspect, the present invention further provides a substrate glass, which can obtain the microcrystalline glass as described in the first aspect after heat treatment and crystallization.
[0043] According to the mass percentage of oxides, the substrate glass includes the following components: 30.00%≤SiO2<35.00%; Al2O3 is 30.00%~40.00%; ZnO is 10.00%~12.00%; MgO is 2.00%~4.00%; ZrO2 is 5.00%~7.00%; Na2O is 2.00%~9.00%; Li2O is 0~2.00%; B2O3 is 0~8.00%; at the same time, the content of each oxide in the microcrystalline glass also meets the following conditions:
[0044] ①X=((Na2O+B2O3) / ZrO2) / Al2O3, X≥2.00;
[0045] ②Y=ln[(Na2O+B2O3) / ZrO2], Y≥0;
[0046] ③Z=(SiO2+Al2O3-MgO-ZnO) / (Li2O+Na2O+B2O3), 4.00≤Z≤10.00;
[0047] In formulae ① to ③, oxide represents the mass percentage of the oxide component.
[0048] Preferably, the content of each oxide in the substrate glass also satisfies the following conditions:
[0049] ④W=(0.8×(Al2O3-SiO2)+1.5×(ZnO-MgO)) / ZrO2, 0≤W≤3.00; In formula ④, oxide represents the mass percentage of the oxide component.
[0050] Preferably, the substrate glass further comprises 0-3.00wt% of BaO and / or 0-2.00wt% of Y2O3.
[0051] Preferably, the substrate glass contains substantially no TiO2 and / or P2O5.
[0052] In a third aspect, the present invention further provides a chemically strengthened glass obtained by subjecting the above-mentioned glass-ceramics or substrate glass to chemical strengthening treatment, wherein the chemically strengthened glass comprises a compressive stress layer and a tensile stress layer.
[0053] The chemically strengthened glass provided by the present invention includes strengthened glass obtained by chemically strengthening substrate glass and strengthened microcrystalline glass obtained by chemically strengthening microcrystalline glass.
[0054] In a fourth aspect, the present invention further provides a glass device, which is made of the above-mentioned microcrystalline glass, or made of the above-mentioned substrate glass, or made of the above-mentioned chemically strengthened glass.
[0055] In a fifth aspect, the present invention further provides an electronic device, which comprises the above-mentioned microcrystalline glass or the above-mentioned substrate glass or the above-mentioned chemically strengthened glass.
[0056] Compared with the prior art, the present invention has the following beneficial effects:
[0057] The present invention has conducted an in-depth study on the component system of microcrystalline glass, and optimized the glass formula by adjusting the oxides in the glass system and the content relationship of each oxide. On the one hand, the difficulty of melting the substrate glass and the heat treatment temperature of preparing the target microcrystalline glass using the substrate glass are reduced, and the difficulty of mass production of microcrystalline glass is reduced. The glass formula provided by the present invention can be mass-produced by conventional continuous melting, rolling and other methods to obtain substrate glass, ensuring the formability of the substrate glass; and the substrate glass corresponding to the glass formula of the present invention can obtain a transparent microcrystalline glass with a main crystal phase of zinc-magnesium spinel solid solution and good optical properties when the heat treatment temperature does not exceed 800°C. Compared with the prior art, the formula system provided by the present invention can significantly reduce the heat treatment temperature, thereby reducing the difficulty of mass production of spinel microcrystalline glass and improving the mass production performance of spinel microcrystalline glass. On the other hand, by utilizing the synergistic coordination of each oxide component with a specific content, while obtaining the required content of the target main crystal phase (Zn, Mg)Al2O4, the intrinsic strength of the residual glass phase in the microcrystalline glass is improved. By combining the main crystal phase (Zn, Mg) Al2O4) with high Young's modulus and shear modulus with the residual glass phase with high intrinsic strength, the obtained microcrystalline glass has high intrinsic strength and has better scratch resistance than the existing spinel system microcrystalline glass. The scratch resistance of the strengthened microcrystalline glass strengthened by the microcrystalline glass of the present invention is comparable to that of sapphire glass, and can meet the demand for cover glass of high-end electronic products. BRIEF DESCRIPTION OF THE DRAWINGS
[0058] Figure 1 This is the TGA curve of the substrate glass of Example S4.
[0059] Figure 2 This is the XRD spectrum of the glass-ceramic sample of Example S1.
[0060] Figure 3 This is the transmittance curve of the microcrystalline glass sample of Example S1.
[0061] Figure 4 The scratch effect diagram of the microcrystalline glass of Example S1 subjected to scratch experiments under different conditions, wherein:
[0062] (a) The corresponding experimental conditions are R1: gem mineral hardness pen with Mohs hardness level 7, load 250g;
[0063] (b) The corresponding experimental conditions are R2: gem mineral hardness pen with Mohs hardness level 7, load 500 g;
[0064] (c) The corresponding experimental condition is R3: gem mineral hardness pen with Mohs hardness grade of 6 and load of 750 g.
[0065] Figure 5 The scratch effect diagram of the glass-ceramics of Examples S2 and S8 subjected to a scratch test under experimental condition R4, wherein:
[0066] Experimental conditions R4 are: gem mineral hardness pen with Mohs hardness rating of 7, load 750g;
[0067] (d) corresponds to the strengthened glass-ceramics of Example S2, and (e) corresponds to the strengthened glass-ceramics of Example S8.
[0068] Figure 6 The figure is a scratch effect diagram of the strengthened microcrystalline glass of Example S1 subjected to a scratch test under the experimental condition R4, wherein:
[0069] Experimental condition R4 is: gem mineral hardness pen with Mohs hardness level 7 and load 750g.
[0070] Figure 7 The figure is a scratch effect diagram of the strengthened micro-ceramic glass and sapphire glass of Examples S2 and S8 subjected to a scratch test under the experimental condition R5, wherein:
[0071] Experimental conditions R5 are: gem mineral hardness pen with Mohs hardness rating of 8, load 750g;
[0072] (g) corresponds to the strengthened microcrystalline glass of Example S2, (h) corresponds to the strengthened microcrystalline glass of Example S8, and (i) corresponds to sapphire glass.
[0073] Figure 8 The figure is a scratch effect diagram of the strengthened micro-ceramic glass of comparative examples D1 and D2 subjected to a scratch test under experimental condition R4, wherein the experimental condition R4 is: a gem mineral hardness pen with a Mohs hardness rating of 7 and a load of 750g;
[0074] (j) corresponds to the strengthened microcrystalline glass of the corresponding ratio D1, and (k) corresponds to the strengthened microcrystalline glass of the corresponding ratio D2.
[0075] Fig. 9 It is a scratch effect diagram of the microcrystalline glass of comparative example D6 subjected to a scratch test under experimental condition R3, wherein the experimental condition R3 is: a gem mineral hardness pen with a Mohs hardness rating of 6 and a load of 750g.
[0076] Fig.10 It is a scratch effect diagram of the strengthened microcrystalline glass of comparative example D6 subjected to a scratch test under experimental condition R3, wherein the experimental condition R3 is: a gem mineral hardness pen with a Mohs hardness grade of 6 and a load of 750g.
[0077] Fig.11 This is the SEM image of the glass-ceramics of Example S3 of the present invention.
[0078] Fig.12 This is a functional relationship diagram of Na2O and K2O concentrations in the strengthened microcrystalline glass of Example S1 measured by thickness cross-section electron probe.
[0079] Fig.13 This is a graph showing the functional relationship between the Na2O and K2O concentrations in the strengthened glass-ceramics of Example S2 as measured by the thickness cross-section electron probe.
[0080] Fig.14 This is a functional relationship diagram of Na2O and K2O concentrations in the strengthened microcrystalline glass of Example D2 measured by thickness cross-section electron probe. DETAILED DESCRIPTION
[0081] 1. The relevant special names and relevant measurement methods involved in the present invention are explained as follows.
[0082] Base glass: glass that has not been subjected to nucleation, crystallization or strengthening treatment.
[0083] Glass-ceramics: also known as glass ceramics, is a type of solid composite material that is prepared by targeted and controlled crystallization of the base glass and contains both glass phase and crystal phase (microcrystalline phase, crystalline phase, and crystalline phase).
[0084] Strengthened glass-ceramics: It is a solid composite material obtained after chemical strengthening of glass-ceramics. During high-temperature chemical strengthening, the alkali metal ions with large ionic radius (such as potassium ions and sodium ions) in the salt bath / molten salt will replace the alkali metal ions with small ionic radius (such as sodium ions and lithium ions) in the glass-ceramics, thereby generating a volume difference of exchange ions and generating compressive stress on the surface of the glass-ceramics.
[0085] Residual glass phase: The amorphous phase in the glass-ceramic system; glass-ceramic contains crystalline phase and residual glass phase.
[0086] Dissociation energy: generally refers to dissociation energy, which is the minimum energy absorbed from the outside world when a molecule in the lowest energy state decomposes into completely independent atoms, and is also the energy required to break a bond.
[0087] Nucleation: Through heat treatment, the nucleating material in the glass grows small crystal nuclei.
[0088] Crystallization: Growing a certain crystal based on the crystal nucleus through heat treatment.
[0089] Crystalline phase: The crystallographic phase is the microscopic structure of the crystal, which is determined by the conformation and arrangement of the polymer chains in the crystal.
[0090] Theoretical crystallinity: The theoretical maximum degree of crystallinity under this glass-ceramic formula system.
[0091] Average grain size: The microcrystalline glass sample was tested by an X-ray diffractometer. The Scherrer formula D = Kλ / (βcosθ) was used for the result data obtained from the XRD test. λ is the X-ray wavelength of 0.154056nm, β is the peak half-height width, and K = 0.89 to obtain the average grain size.
[0092] Crystal content: the percentage of the total mass of crystals / crystalline phases / grains in the total mass of microcrystalline glass, also known as actual crystallinity. It should be understood that both crystal phases and grains refer to crystals precipitated in microcrystalline glass, but are described in different ways.
[0093] Transmittance: The ratio of the radiant energy projected and transmitted through an object to the total radiant energy projected onto the object during the process of the incident light flux leaving from the illuminated surface or the incident surface of the medium to the other surface. In the embodiments and comparative examples of the present invention, the transmittance of microcrystalline glass at a wavelength of 550nm refers to the average transmittance of multiple glass samples of the same batch measured at a wavelength of 550nm. At least 5 microcrystalline glass samples are taken from each batch for testing.
[0094] Refractive index: the ratio of the propagation speed of light in a vacuum to the propagation speed of light in the medium. The present invention uses a monocular Abbe refractometer (WYA-2WAJ, Bell Analytical Instruments Co., Ltd.) with a wavelength set to 589 nm to test the refractive index of the microcrystalline glass sheet.
[0095] b value: represents the yellow-blue value of the material. The b value in the embodiment of the present invention is the b value of the transmitted light. A positive b value indicates that the material is blue. It is measured using a Konica Minolta spectrophotometer CM-3600A.
[0096] Vickers hardness: A standard for expressing the hardness of materials proposed by Robert L. Smith and George E. Sandland of the United Kingdom at Vickers Ltd in 1921.
[0097] Sample thickness test: determined by micrometer test. It should be understood that in the thickness direction, the degree of ion exchange changes gradually from the surface to the center, and the total Na-K and / or Li-Na exchange amount generally does not exceed 1% of the total mass of the sample, and the difference in ion radius is at the pm level, so the expansion effect in the thickness direction is very slight, and it can be approximately considered that the thickness has basically not changed. That is, the thickness change of the microcrystalline glass sheet before and after chemical strengthening is very small and can be ignored.
[0098] Optical performance test: According to the standard of GB / T 7962.12-2010 Test method for colorless optical glass Part 12: Spectral transmittance, professional testing instruments are used to test the haze, b value and transmittance of microcrystalline glass. The present invention uses the spectrophotometer CM-3600A of Konica Minolta of Japan to test the haze and b value; the present invention uses the UV-2000 ultraviolet visible spectrophotometer of Shimadzu to test the transmittance and its curve.
[0099] The test method of crystal content is as follows: the microcrystalline glass sample is tested by an X-ray diffractometer to obtain an XRD diffraction peak curve, and then the X-ray diffractometer test result file (RAW format) is imported into the X-ray diffraction data Rietveld refinement software (such as Gsas, Fullprof, Maud), and the fitting and calculation are performed. The ratio of the fitted crystal phase peak area to the fitted total peak area is the crystal content. The X-ray diffractometer used in the present invention is Shimadzu's XRD-6100, the target material is copper, the diffraction angle range used in the test is 2θ=10-80°, the scanning speed is 0.2° / min, the operating voltage is 40kV, and the operating current is 30mA.
[0100] Density measurement: The density of the glass-ceramic sample was tested according to the principle of “Archimedes drainage method”, and the testing instrument was ALFA MIRAGE electronic density balance SD-200L.
[0101] Test of Young's modulus: The testing instrument is UMS-100 ultrasonic material characterization system.
[0102] Differential Scanning Calorimetry (DSC) test: The test instrument is Mettler-Toledo's TGA / DSC3+ thermogravimetric and synchronous thermal analyzer. During the test, the sample was ground and passed through a 200-mesh sieve; the test conditions were: room temperature to 1100°C, and the heating rate was 10°C / min;
[0103] Single rod static pressure: Place the strengthened microcrystalline glass on the bottom ring of the tensile testing machine (LT-850A), start the test software, and set the moving speed of the extrusion rod (rod diameter 8mm, indenter arc radius 10mm) to 50mm / min. Click to start the test. The extrusion rod will apply force to the center of the microcrystalline glass sheet to be tested at the set moving speed until the microcrystalline glass cracks and breaks. The test software will automatically read the force (N) when the glass breaks as the test result. Take 10 microcrystalline glass samples in the same state for testing, and take the average value of the test results as the single rod static pressure strength of the microcrystalline glass.
[0104] Scratch test: The testing instrument is an automatic pencil hardness tester (ZIPANG MOTOR). Test method: Use an automatic pencil hardness tester to fix the Mohs hardness pen at an angle of 45° so that the pen tip contacts the surface of the glass sample. Under a predetermined load, move the glass placement table at a moving rate of 60 mm / min to perform a scratch test. A clean glass sample to be tested is placed on the glass placement table, and the predetermined load is set by placing weights of corresponding weights. The gem mineral hardness pens No. 6-8 used in the present invention correspond to Mohs hardness levels 6-8, respectively. After the scratch experiment is completed, the scratched glass sample is placed under a 400x microscope to observe the scratch state and take photos for record. The hardness of the glass sample to be tested is judged based on whether scratches are left and the state of the scratches. If scratches are left, it means that the hardness of the glass sample to be tested is lower than that of the test hardness pen. If there are no scratches, it means that the hardness of the glass sample to be tested is higher than that of the test hardness pen.
[0105] Electron probe test: The test instrument is Shimadzu electron probe EPMA-1720. The characteristic X-rays generated by the electron beam acting on the sample are used to perform micro-area composition analysis. In the present invention, the depth of the compressive stress layer formed by potassium-sodium exchange in the strengthened microcrystalline glass obtained after chemical strengthening is obtained by electron probe testing.
[0106] Surface K2O concentration test: Surface K2O concentration is equal to K2O mass / total oxide mass, where the total oxide mass includes SiO2, Al2O3, P2O5, ZrO2, Na2O, K2O and other oxides that can be accurately tested by XRF, but does not include Li2O, B2O3 and other oxides that cannot be accurately tested by XRF. The surface K2O concentration of the strengthened microcrystalline glass of the present invention is measured by X-ray fluorescence spectrometer (XRF), and the test equipment used is Thermo Scientific ARL TM PERFORM'X. The target material is Rh (rhodium), the light tube voltage is 40kW, the current is 60mA, the collimator is 0.15, the crystal is LiF200, the detector is FPC, the test range is 29mm circle, and the analysis software is UniQuant standardless analysis. Standardless testing is used during XRF testing, and the concentration of elements with atomic numbers 6 and below or their oxides in the glass is not tested. That is, when calculating the K2O concentration obtained by XRF testing in the present invention, the total mass of the oxide does not include the mass of elements with atomic numbers 6 and below or their oxides in the glass.
[0107] Vickers hardness (HV) test: The chemically strengthened strengthened microcrystalline glass sheet is made into a small piece with a length, width and thickness of 50mm*50mm*0.7mm, and a glass sample with a clean surface and no visible scratches, pits, cracks and other damage is selected as a test sample, and then the Vickers hardness of the strengthened microcrystalline glass is measured using a Vickers hardness tester. Test conditions: load 300gf, load time 10s, the validity of the indentation complies with GB / T 16534. Select 3 different positions on the surface of the same sample for measurement, and select the average value as the final test result. The Vickers hardness tester used in the present invention is a digital display small load Vickers hardness tester (Beijing Kewei Technology Co., Ltd., VTD405).
[0108] 2. The present invention provides a transparent microcrystalline glass with high scratch resistance.
[0109] After studying the components of existing microcrystalline glass, the present invention found that although zinc-magnesium spinel crystals have become the preferred crystal phase for improving the scratch resistance of glass due to their high Young's modulus and shear modulus, the scratch resistance of existing transparent spinel microcrystalline glass is still insufficient to meet the application requirements of protective cover plates of high-end products and needs to be further improved.
[0110] The transparent microcrystalline glass provided by the present invention contains crystal grains, the main crystal phase is (Zn, Mg)Al2O4, and (Zn, Mg)Al2O4 is a zinc-magnesium spinel solid solution; according to the mass percentage of oxides, the microcrystalline glass includes the following components: 30.00%≤SiO2<35.00%; Al2O3 is 30.00%-40.00%; ZnO is 10.00%-12.00%; MgO is 2.00%-4.00%; ZrO2 is 5.00%-7.00%; Na2O is 2.00%-9.00%; Li2O is 0-2.00%; B2O3 is 0-8.00%; at the same time, the content of each oxide in the microcrystalline glass also meets the following conditions:
[0111] ①X=((Na2O+B2O3) / ZrO2) / Al2O3, X≥2.00;
[0112] ②Y=ln[(Na2O+B2O3) / ZrO2], Y≥0;
[0113] ③Z=(SiO2+Al2O3-MgO-ZnO) / (Li2O+Na2O+B2O3), 4.00≤Z≤10.00;
[0114] In formulae ① to ③, oxide represents the mass percentage of the oxide component.
[0115] In the study of the various oxide components of microcrystalline glass, the present invention found that there is a certain correlation between the various oxide components, and this correlation affects the structure and properties of the microcrystalline glass, which is related to both the scratch resistance of the microcrystalline glass required by the present invention and other properties of the microcrystalline glass.
[0116] The inventors found that due to the extremely high dissociation energy of aluminum oxide G = 134 kJ cm -3 Increasing the content of Al2O3 in the spinel glass-ceramic formula system can, on the one hand, improve the aluminum saturation of the crystal phase, and on the other hand, help to increase the dissociation energy in the residual glass phase and the intrinsic strength of the residual glass phase. Moreover, the atomic packing density of the glass increases with the coordination number of aluminum. Increasing the content of Al2O3 is also beneficial to improve the compactness of the glass-ceramic system. However, replacing silicon oxide with aluminum oxide will increase the difficulty of glass melting and molding, and it is necessary to add components with fluxing effects, such as alkali metal oxides, alkaline earth metal oxides, boron oxide, etc. Alkali metal oxides can provide alkali metal ions to achieve chemical strengthening and toughening of glass-ceramics, and at the same time provide free oxygen, affecting the network structure of the glass. Boron oxide has a good fluxing effect, but the coordination structure of boron oxide will be affected by the free oxygen provided by alkali metals and / or alkaline earth metals. If the content of boron oxide is too much, the ratio of boron-oxygen tetrahedron to boron-oxygen triangle in the glass phase will decrease, causing part of the glass phase to change from the original three-dimensional space frame structure to a two-dimensional space layered structure, weakening the glass network structure; at the same time, excessive boron oxide content will have a negative impact on the optical properties of the glass. Zinc oxide, magnesium oxide and aluminum oxide are components of the target main crystal phase (Zn, Mg) Al2O4), and ZrO2 is a nucleating agent. The content relationship of these oxides not only determines the content of the main crystal phase in the microcrystalline glass, but also determines the structure and intrinsic strength of the residual glass phase in the microcrystalline glass.
[0117] On this basis, the present invention unexpectedly discovered that, based on the range of the amount of each oxide, the microcrystalline glass formula system is adjusted in three aspects. On the one hand, it can reduce the difficulty of melting the substrate glass and the heat treatment temperature of preparing the target microcrystalline glass using the substrate glass. The glass formula provided by the present invention can be mass-produced by conventional continuous melting, rolling and other methods to obtain the substrate glass, thereby ensuring the formability of the glass; and the substrate glass corresponding to the glass formula of the present invention can obtain a transparent microcrystalline glass with a main crystal phase of zinc-magnesium spinel solid solution and good optical properties when the heat treatment temperature does not exceed 800°C. Compared with the prior art, the formula system provided by the present invention can significantly reduce the heat treatment temperature, thereby reducing the difficulty of mass production of spinel microcrystalline glass and improving the mass production performance of spinel microcrystalline glass. On the other hand, by utilizing the synergistic coordination of each oxide component with a specific content, while obtaining the required content of the target main crystal phase (Zn, Mg)Al2O4, the intrinsic strength of the residual glass phase in the microcrystalline glass is improved. By combining the main crystal phase (Zn, Mg)Al2O4 with high Young's modulus and shear modulus with the residual glass phase with high intrinsic strength, the obtained microcrystalline glass has high intrinsic strength and has better scratch resistance than the existing spinel system microcrystalline glass. The scratch resistance of the strengthened microcrystalline glass strengthened by the microcrystalline glass of the present invention is comparable to that of sapphire glass, and can meet the demand for cover glass of high-end electronic products.
[0118] SiO2 is a glass network forming oxide and an indispensable component of the glass network structure. Properly increasing the content of SiO2 can increase the stability and mechanical strength of the glass, but excessive SiO2 will increase the viscosity of the base glass, making it more difficult to melt the glass, thereby reducing the formability of the base glass. In the present invention, the mass percentage of SiO2 is between 30.00% and 35.00%, which is conducive to better balancing the contradiction between the stability, formability and mechanical strength of the glass. In some embodiments, the content of SiO2 can be 30.00% to 31.00%, 30.00% to 32.00%, 30.00% to 33.00%, 32.00% to 34.95%, 31.00% to 34.95%, 31.00% to 34.00%, 30.00%, 30.50%, 31.00%, 31.50%, 32.00%, 32.50%, 33.00%, 33.50%, 34.00%, 34.50%, 34.95%, etc., and all ranges and sub-ranges between the above values. It should be understood that in embodiments, any of the above ranges can be combined with any other ranges.
[0119] Al2O3 is an intermediate oxide in the formation of glass, which can improve the chemical stability of glass. Al2O3 is one of the components that form the zinc-magnesium spinel-spinel crystal phase after the substrate glass is crystallized, and will directly affect the content of the main crystalline phase (Zn, Mg) Al2O4. At the same time, since [AlO4] is larger in volume than [SiO4], it can provide a larger space for ion exchange and promote chemical strengthening. Moreover, Al2O3, with its extremely high dissociation energy, has a greater influence on the intrinsic strength of the residual glass phase. However, excessive Al2O3 will increase the viscosity of the substrate glass, causing the formability of the substrate glass to decrease. In the present invention, the mass percentage of Al2O3 is between 30.00 and 40.00%. In some embodiments, the content of Al2O3 can be 30.00% to 31.00%, 30.00% to 32.00%, 30.00% to 33.00%, 32.00% to 35.00%, 31.00% to 35.00%, 31.00% to 34.00%, 33.00% to 36.00%, 32.00% to 38.00%, 30.00% to 39.00% %, 34.00% to 39.00%, 35.00% to 40.00%, 36.00% to 40.00%, 30.00%, 31.00%, 32.00%, 33.00%, 34.00%, 35.00%, 37.00%, 38.00%, 39.00%, 40.00%, etc., and all ranges and subranges between the above values. It should be understood that in embodiments, any of the above ranges can be combined with any other ranges.
[0120] ZnO provides the zinc necessary for the formation of zinc-magnesium spinel-spinel crystalline phase after the substrate glass is crystallized. ZnO can reduce the thermal expansion coefficient of glass and improve the chemical stability, thermal stability and refractive index of glass. In the present invention, the mass percentage of ZnO is between 10% and 12%. In some embodiments, the content of ZnO can be 10.00% to 11.00%, 10.00% to 11.40%, 11.00% to 12.00%, 11.50% to 12.00%, 10.00%, 10.50%, 11.00%, 11.48%, 11.50%, 12.00%, etc., and all ranges and sub-ranges between the above values. It should be understood that in the embodiment, any of the above ranges can be combined with any other ranges.
[0121] MgO provides the magnesium necessary for the crystallization of the substrate glass to form a zinc-magnesium spinel-spinel crystal phase. MgO can slow down the hardening speed of the glass and improve the forming properties of the glass; MgO can also reduce the crystallization tendency and crystallization speed, increase the high temperature viscosity of the glass, and improve the chemical stability and mechanical strength of the glass. In the present invention, the mass percentage of MgO is between 2% and 4%. In some embodiments, the content of MgO can be 2.00% to 3.00%, 3.00% to 4.00%, 2.00% to 2.50%, 2.50% to 3.00%, 2.50% to 4.00%, 3.50% to 4.00%, 2.00%, 2.50%, 3.00%, 3.50%, 4.00%, etc., and all ranges and sub-ranges between the above values. It should be understood that in the embodiment, any of the above ranges can be combined with any other ranges.
[0122] ZrO2 has a large accumulation effect on the glass structure due to its high cationic charge and strong field, and acts as a nucleating agent in the substrate glass; at the same time, ZrO2 can also increase the strength and toughness of the microcrystalline glass and improve its acid and alkali corrosion resistance. In addition, ZrO2 is also the second crystalline phase of the microcrystalline glass of this system. However, it is extremely difficult to melt ZrO2, and excessive ZrO2 cannot be evenly dispersed in the substrate glass, which easily produces melting defects such as unmelted materials or precipitation. In the present invention, the mass percentage of ZrO2 is between 5% and 7%. In some embodiments, the content of ZrO2 can be 5.00% to 6.00%, 5.50% to 6.00%, 5.50% to 7.00%, 6.00% to 7.00%, 6.50% to 7.00%, 5.00%, 5.40%, 5.50%, 6.00%, 6.50%, 7.00%, etc., and all ranges and sub-ranges between the above values. It should be understood that in embodiments, any of the above ranges can be combined with any other ranges.
[0123] The microcrystalline glass of the present invention also contains one or more alkali metal oxides, such as Li2O and Na2O, which can promote the ion exchange process to chemically strengthen the microcrystalline glass and improve the mechanical strength of the microcrystalline glass. At the same time, the alkali metal oxides, as the external oxides of the network formed by the glass, will provide free oxygen, destroy the network structure of the glass, and further affect the intrinsic strength of the glass. However, destroying the network structure of the glass is beneficial to reducing the high-temperature viscosity of the glass and promoting the melting and clarification of the glass liquid.
[0124] In the present invention, the mass percentage of Na2O is between 2.00% and 9.00%. + The ion exchange component required for the chemical strengthening process is obtained by + Compared with the Na+ ions with small ionic radius in glass-ceramics +The exchange reaction can generate surface compressive stress on the surface of the microcrystalline glass, further improving the monomer strength and scratch resistance of the microcrystalline glass. In some embodiments, the content of Na2O can be 2.00% to 3.00%, 2.00% to 5.00%, 2.00% to 8.00%, 2.50% to 8.50%, 3.00% to 6.00%, 4.00% to 9.00%, 2.00% to 7.00%, 5.00% to 8.00%, 6.00% to 9.00%, 2.00%, 2.50%, 3.00%, 4.00%, 5.00%, 6.00%, 7.00%, 8.00%, 8.50%, 9.00%, etc., and all ranges and sub-ranges between the above values. It should be understood that in the embodiment, any of the above ranges can be combined with any other ranges.
[0125] In the present invention, the mass percentage of Li2O is between 0.00% and 2.00%. + Compared with the Li ions with small ionic radius in glass-ceramics + The exchange reaction can form deep stress in the microcrystalline glass, which improves the strength and scratch resistance of the microcrystalline glass monomer while improving the impact resistance of the microcrystalline glass. In some embodiments, the content of Li2O can be 0.00-1.00%, 0.00-1.50%, 1.00%-1.50%, 1.00%-2.00%, 1.50%-2.00%, 0.00%, 1.00%, 1.50%, 2.00%, etc., and all ranges and sub-ranges between the above values. It should be understood that in the embodiment, any of the above ranges can be combined with any other ranges.
[0126] B2O3 acts as a flux in the glass formation process. The free oxygen provided by alkali metals or alkaline earth metals will affect the coordination of boron oxide, causing it to transform from a boron-oxygen triangle to a boron-oxygen tetrahedron composed of bridging oxygen, causing part of the glass phase to transform from the original two-dimensional layered structure to a three-dimensional frame structure, thereby enhancing the glass network structure. B2O3 can reduce the high-temperature viscosity of the glass, accelerate the clarification of the glass, and reduce the crystallization ability of the glass; it can effectively alleviate the problem of difficulty in melting the base glass due to high content of alumina, but excessive B2O3 will reduce the chemical stability and mechanical strength of the glass, and affect the optical properties of the glass. In the present invention, the mass percentage of B2O3 is 0 to 8%. In some embodiments, the content of B2O3 can be 1.00% to 6.00%, 2.00% to 3.00%, 1.00% to 4.00%, 1.00% to 5.00%, 2.00% to 5.00%, 2.50% to 8.00%, 3.00% to 6.00%, 4.00% to 9.00%, 2.00% to 7.00%, 5.00% to 8.00%, 6.00% to 9.00%, 0.00%, 1.00%, 2.00%, 2.50%, 3.00%, 4.00%, 5.00%, 6.00%, 7.00%, 8.00%, etc., and all ranges and sub-ranges between the above values. It should be understood that in embodiments, any of the above ranges can be combined with any other ranges.
[0127] In some embodiments, the value of X=((Na2O+B2O3) / ZrO2) / Al2O3 can be 2.00-3.00, 2.00-4.00, 2.00-5.00, 2.00-6.00, 2.00-7.00, 2.00-8.00, 2.00-9.00, 2.00-10.00, 3.00-4.00, 3.00-6.00, 3.00-9.00, 5.00-9.00, 6.00-9.00, 8.00-9.00, 2.00, 3.00, 4.00, 5.00, 6.00, 7.00, 8.00, 9.00, 10.00, etc., and all ranges and sub-ranges between the above values. It should be understood that in embodiments, any of the above ranges may be combined with any other ranges.
[0128] In some embodiments, the value of Y=ln[(Na2O+B2O3) / ZrO2] can be 0.00-0.10, 0.00-1.00, 0.00-0.30, 0.00-0.60, 0.00-0.90, 0.00-0.40, 0.10-0.90, 0.30-0.70, 0.30-0.90, 0.20-0.50, 0.40-0.80, 0.10, 0.20, 0.30, 0.40, 0.50, 0.60, 0.70, 0.80, 0.90, 1.00, 1.10, etc., and all ranges and sub-ranges between the above values. It should be understood that in embodiments, any of the above ranges can be combined with any other ranges.
[0129] In some embodiments, the value of Z=(SiO2+Al2O3-MgO-ZnO) / (Li2O+Na2O+B2O3) may be 4.00-10.00, 4.00-5.00, 4.00-6.00, 4.00-7.00, 4.00-8.00, 4.00-9.00, 5.00-6.00, 5.00-7.00, 5.00-8.00, 5.00-9.00, 5.00-10 00, 6.00, 7.00, 8.00, 9.00, 10 ...
[0130] In some embodiments of the present invention, the content of each oxide in the microcrystalline glass also satisfies the following conditions:
[0131] ④W=(0.8×(Al2O3-SiO2)+1.5×(ZnO-MgO)) / ZrO2, 0≤W≤3.00;In formula ④, oxide represents the mass percentage of the oxide component. By adjusting the content relationship of Al2O3, SiO2, ZnO, MgO, and ZrO2 to meet ④ on the basis of satisfying the range of each oxide and the requirements of formulas ① to ③, it can be ensured that the transparent microcrystalline glass has excellent optical properties.
[0132] In some embodiments, the value of W=(0.8×(Al2O3-SiO2)+1.5×(ZnO-MgO)) / ZrO2 can be 0.00-3.00, 0.00-1.00, 0.00-2.00, 1.00-2.00, 1.00-3.00, 2.00-3.00, 0.00-0.50, 0.00-1.50, 0.00-2.50, 1.00-1.50, 1.00-2.50, 2.00-2.50, 2.5.00-3.00, 0.00, 0.50, 1.00, 1.50, 2.00, 2.50, 3.00, etc., and all ranges and sub-ranges between the above values. It should be understood that in embodiments, any of the above ranges can be combined with any other ranges.
[0133] In some embodiments of the present invention, the microcrystalline glass satisfies the following conditions in terms of the molar percentage of oxides: the molar percentage of Al2O3 is greater than the sum of the molar percentages of MgO and ZnO; the theoretical crystallinity of the microcrystalline glass is at least 30.00wt%, preferably 30.00wt% to 50.00wt%. In some embodiments, the theoretical crystallinity can be 30.00wt% to 40.00wt%, 30.00wt% to 60.00wt%, 30.00wt% to 70.00wt%, 35.00wt% to 45.00wt%, 32.00wt% to 48.00wt%, 41.00wt% to 49.00wt%, 30.00wt%, 35.00wt%, 40.00wt%, 45.00wt%, 50.00wt%, etc., and all ranges and sub-ranges between the above values. It should be understood that in embodiments, any of the above ranges may be combined with any other ranges.
[0134] It should be understood that theoretical crystallinity refers to the theoretical maximum degree of crystallinity of a certain formula base glass when a specific crystal phase is formed. Theoretical crystallinity is the theoretical maximum crystallinity, which is the preliminary basic regulation of the core crystal phase components to ensure that there is a chance to obtain microcrystalline glass with the desired target crystal phase content in the end.
[0135] For glass-ceramics of different systems, the calculation of their theoretical crystallinity is different due to the differences in their crystal phases and degrees of crystallization. The theoretical crystallinity in different glass-ceramics systems is determined by two parts: the nucleating agent in the component, such as ZrO2, and the oxide that constitutes the specific crystal phase. In the present invention, the main crystal phase of the glass-ceramics is zinc-magnesium spinel solid solution (Zn, Mg)Al2O4, and the secondary crystal phase includes one or more of tetragonal ZrO2, Zn2SiO4, and Mg2SiO4. Therefore, the theoretical crystallinity of the glass-ceramics of the present invention is determined by two parts: the nucleating agent in the component, such as ZrO2, and the oxides Al2O3, MgO and ZnO that constitute the crystal phase.
[0136] The main crystalline phase of the microcrystalline glass of the present invention is zinc-magnesium spinel solid solution (Zn, Mg)Al2O4. The crystalline phase composition is calculated by the oxide molar ratio, MgO / Al2O3=1 in MgAl2O4, and ZnO / Al2O3=1 in ZnAl2O4. In order to obtain a higher crystallinity and a better strengthening effect, it is required that after ZnAl2O4 and / or MgAl2O4 are completely formed, a portion of Al2O3 can still remain in the residual glass phase. Because the volume of [AlO4] tetrahedron is larger than that of [SiO4] tetrahedron, the remaining amount of Al2O3 in the residual glass phase can provide a larger space for ion exchange during the chemical strengthening process and promote the ion exchange. On this basis, in the microcrystalline glass of the present invention, the molar percentage of Al2O3 is greater than the sum of the molar percentages of ZnO and MgO.
[0137] In some embodiments of the present invention, when the microcrystalline glass meets the theoretical crystallinity, the residual glass phase unit volume dissociation energy U in the microcrystalline glass is not less than 71.00 kJ·cm -3 , preferably 71.00 kJ·cm -3 ~134.00kJ·cm -3 In some embodiments, the dissociation energy per unit volume of the residual glass phase in the glass-ceramics may be 71.00 kJ·cm -3 ~75.00kJ·cm -3 、71.00kJ·cm -3 ~80.00kJ·cm -3 , 7.00 kJ·cm -3 1~90.00kJ·cm -3 、71.00kJ·cm -3 ~100.00kJ·cm -3 、71.00kJ·cm -3 ~110.00kJ·cm -3 、71.00kJ·cm -3 ~120.00kJ·cm -3 、71.00kJ·cm -3 ~130.00kJ·cm -3 、80.00kJ·cm -3 ~90.00kJ·cm -3 、80.00kJ·cm -3 ~100.00kJ·cm -3 、80.00kJ·cm -3 ~110.00kJ·cm -3 、80.00kJ·cm -3~120.00kJ·cm -3 、80.00kJ·cm -3 ~130.00kJ·cm -3 、90.00kJ·cm -3 ~100.00kJ·cm -3 、90.00kJ·cm -3 ~110.00kJ·cm -3 、90.00kJ·cm -3 ~120.00kJ·cm -3 、90.00kJ·cm -3 ~130.00kJ·cm -3 、100.00kJ·cm -3 ~110.00kJ·cm -3 、100.00kJ·cm -3 ~120.00kJ·cm -3 、100.00kJ·cm -3 ~130.00kJ·cm -3 、71.00kJ·cm -3 、80.00kJ·cm -3 、90.00kJ·cm -3 、100.00kJ·cm -3 、110.00kJ·cm -3 、120.00kJ·cm -3 、134.00kJ·cm -3 Etc., and all ranges and subranges between the above values. It should be understood that in embodiments, any of the above ranges can be combined with any other ranges.
[0138] Regarding the calculation of the unit volume dissociation energy U of the residual glass phase, taking the spinel system glass-ceramics of the present invention as an example:
[0139] Assuming that in the glass formula: the molar percentage of Al2O3 is a, the molar percentage of ZnO is b, and the molar percentage of MgO is c, then a>b+c. Calculate the unit volume dissociation energy U of the residual glass phase after the substrate glass of this formula is used to prepare zinc-magnesium spinel micro-ceramics with theoretical crystallinity:
[0140] 1. Determine the molar percentages of ZnO, MgO, and Al2O3 in the residual glass phase.
[0141] Since it is a theoretical crystallinity, that is, the crystallinity achieved when both ZnO and MgO participate in the precipitation of spinel, ZnO and MgO will all exist in the crystal phase, that is, the content of ZnO and MgO in the residual glass phase is 0. Since a>b+c, a-(b+c) Al2O3 will remain in the residual glass phase, and the molar percentage of Al2O3 in the residual glass phase is calculated based on the content of each oxide in the residual glass phase.
[0142] 2. Determine the molar percentage of other oxides in the residual glass phase except Al2O3, ZnO and MgO.
[0143] (1) Nucleating agents usually precipitate before crystals. For example, the nucleating agent ZrO2 precipitates tiny grains with a size of less than 1 nm in the nucleation step of microcrystalline glass, and the crystals grow on them; the nucleating agent TiO2 forms titanate nuclei in the nucleation step of microcrystalline glass, and the crystals grow under its induction and cover it. Nucleating agents are generally located in the center of the crystal. Therefore, in theory, the nucleating agent will all exist in the crystal phase, and the content of nucleating agent in the residual glass phase is 0.
[0144] (2) In addition to the oxides and nucleating agents that constitute the crystalline phase, other oxides in the substrate glass are theoretically present in the residual glass phase. According to the content of each oxide in the residual glass phase, the molar percentage of each other oxide in the residual glass phase is calculated.
[0145] 3. Define the molar percentage of a certain oxide i in the residual glass phase as n i , the dissociation energy coefficient of the oxide is defined as U i According to Makishima and Mackenzie, U i The values are shown in the following table.
[0146] The dissociation energy per unit volume of the residual glass phase is defined as U:
[0147] U=∑U i ×n i
[0148] U i is the dissociation energy coefficient, in kJ cm -3 , n i It is the molar percentage of a certain oxide in the residual glass phase.
[0149] Table 1 U of common oxides i value
[0150] Oxide <![CDATA[U i / kJ·cm -3 ]]> Oxide <![CDATA[U i / kJ·cm -3 ]]> <![CDATA[SiO2]]> 64.50 CaO 64.90 <![CDATA[Al2O3]]> 134.00 BaO 40.60 <![CDATA[B2O3]]> 77.80 <![CDATA[Li2O]]> 80.40 <![CDATA[P2O5]]> 62.80 <![CDATA[Na2O]]> 37.30 <![CDATA[As2O3]]> 54.80 <![CDATA[K2O]]> 23.40 <![CDATA[Y2O3]]> 74.30 <![CDATA[TiO2]]> 86.70 MgO 83.70 <![CDATA[ZrO2]]> 97.10 ZnO 41.50
[0151] In some embodiments of the present invention, the glass-ceramics further includes 0 to 3.00 wt % of BaO and / or 0 to 2.00 wt % of Y2O3.
[0152] Y2O3, as a high field strength cation, works synergistically with Al2O3, which is beneficial to enhancing the atomic packing density of glass and improving the hardness and Young's modulus of microcrystalline glass. In the present invention, the mass percentage of Y2O3 is between 0.00 and 2.00%. In some embodiments, the content of Y2O3 can be 0.00-1.00%, 0.00-1.50%, 1.00%-1.50%, 1.00%-2.00%, 1.50%-2.00%, 0.00, 1.00%, 1.50%, 2.00%, etc., and all ranges and sub-ranges between the above values. It should be understood that in the embodiment, any of the above ranges can be combined with any other ranges.
[0153] BaO has a good fluxing effect in microcrystalline glass, especially in this system. At the same time, it can increase the refractive index of the glass phase and improve the optical properties of the glass. In the present invention, the mass percentage of BaO is between 0 and 3.00%. In some embodiments, the content of BaO can be 0.00-3.00, 0.00-1.00, 0.00-2.00, 1.00-2.00, 1.00-3.00, 2.00-3.00, 0.00-0.50, 0.00-1.50, 0.00-2.50, 1.00-1.50, 1.00-2.50, 2.00-2.50, 2.5.00-3.00, 0.00, 0.50, 1.00, 1.50, 2.00, 2.50, 3.00, etc., and all ranges and sub-ranges between the above values. It should be understood that in embodiments, any of the above ranges may be combined with any other ranges.
[0154] In some embodiments of the present invention, the microcrystalline glass is substantially free of TiO2 and / or P2O5. Here, "substantially free of" means that TiO2 and / or P2O5 are not actively added or compounded into the glass, but may exist in very small amounts as contaminants. The inventors have found that in the formulation system of the present invention, the addition of TiO2 can cause undesirable color. In order to obtain the desired transparent microcrystalline glass, it is preferably free of TiO2.
[0155] In some embodiments of the present invention, in the glass-ceramics, the average grain size is ≤15.00nm. In some embodiments, the average grain size may be 1.00nm to 4.00nm, 1.00nm to 9.00nm, 1.00nm to 13.00nm, 3.00nm to 5.00nm, 6.00nm to 10.00nm, 7.00nm to 9.00nm, 5.00nm to 6.00nm, 5.00nm to 7.00nm, 5.00nm to 8.00nm, 6.00nm to 8.00nm, 8.00nm to 10.00nm, 7.00nm to 9.00nm, 5.00nm to 6.00nm, 5.00nm to 7.00nm, 5.00nm to 8.00nm, 8.00nm to 10.00nm, 7.00nm to 10.00nm, 8 ... 00nm, 1.00nm, 2.00nm, 3.00nm, 4.00nm, 5.00nm, 6.00nm, 7.00nm, 8.00nm, 9.00nm, 10.00nm, 11.00nm, 12.00nm, 13.00nm, 14.00nm, 15.00nm, etc., preferably 1.00 to 10.00nm, more preferably 4.50 to 8.00nm, etc., and all ranges and sub-ranges between the above values. It should be understood that in an embodiment, any of the above ranges can be combined with any other ranges.
[0156] In some embodiments of the present invention, in the glass-ceramics, the crystal content is 20.00-50.00wt%, preferably 25.00-50.00wt%, and more preferably 25.00-45.00wt%. In some embodiments, in the glass-ceramics, the crystal content can be 20.00wt%, 25.00wt%, 28.00wt%, 30.00wt%, 33.00wt%, 35.00wt%, 38.00wt%, 40.00wt%, 43.00wt%, 45.00wt%, 48.00wt%, 50.00wt%, etc., and all ranges and sub-ranges between the above values. It should be understood that in the embodiments, any of the above ranges can be combined with any other ranges.
[0157] In some embodiments of the present invention, the Young's modulus of the glass-ceramics is not less than 110.00 GPa, preferably 110.00 GPa to 130.00 GPa, more preferably greater than 114 GPa and less than or equal to 140 GPa, and the Young's modulus may be 110.00 GPa to 140.00 GPa, 110.00 GPa to 115.00 GPa, 110.00 GPa to 120.00 GPa, 110.00 GPa to 125.00 GPa, 115.00 GPa to 14 ... GPa~120.00GPa, 115.00GPa~125.00GPa, 115.00GPa~130.00GPa, 120.00GPa~125.00GPa, 120.00GPa~130.00GPa, 114.00GPa, 115.00GPa, 120.00GPa, 125.00GPa, 130.00GPa, 135GPa, 140GPa, etc., and all ranges and sub-ranges between the above values. It should be understood that in embodiments, any of the above ranges can be combined with any other ranges.
[0158] In some embodiments of the present invention, a gem mineral hardness pen with a Mohs hardness rating of 7 is fixed at a 45° angle using an automatic pencil hardness tester, and the surface of the microcrystalline glass is scratched under a load of 500 g, and the scratched microcrystalline glass is placed under a 400x microscope for observation, and there are no scratches on the surface of the microcrystalline glass;
[0159] and / or
[0160] Using an automatic pencil hardness tester and a gem mineral hardness pen with a Mohs hardness rating of 6 fixed at an angle of 45°, the surface of the microcrystalline glass was scratched under a load of 750g, and the scratched microcrystalline glass was observed under a 400x microscope. The surface of the microcrystalline glass had no scratches.
[0161] In some embodiments of the present invention, at a thickness of 0.7 mm, for light of a wavelength of 550 nm, the transmittance of the microcrystalline glass is greater than or equal to 85.00%, preferably greater than or equal to 89.00%. In some embodiments, the transmittance can be 85.00% to 89.00%, 85.00% to 96.00%, 85.00% to 90.00%, 88.00% to 95.00%, 88.00% to 96.00%, 88.00% to 99.00%, 86.00%, 87.00%, 88.00%, 89.00%, 90.00%, 91.00%, 92.00%, 93.00%, 94.00%, 95.00%, 96.00%, etc., and all ranges and sub-ranges between the above values. It should be understood that in the embodiments, any of the above ranges can be combined with any other ranges.
[0162] In some embodiments of the present invention, at a thickness of 0.7 mm, the optical b value of the glass-ceramics is 0.20 to 1.50, preferably 0.35 to 1.20. In some embodiments, the optical b value can be 0.20 to 0.60, 0.30 to 0.90, 0.40 to 0.80, 0.30 to 1.20, 0.60 to 1.10, 0.50 to 1.50, 0.90 to 1.40, 0.80 to 1.30, 0.20, 0.30, 0.50, 0.80, 1.00, 1.10, 1.30, 1.40, 1.50, etc., and all ranges and sub-ranges between the above values. It should be understood that in embodiments, any of the above ranges can be combined with any other ranges.
[0163] The transparent microcrystalline glass with high scratch resistance of the present invention is prepared by the following method:
[0164] Step 1: Obtain substrate glass, which includes the following components in terms of mass percentage of oxides: 30.00%≤SiO2<35.00%; Al2O3 is 30.00%-40.00%; ZnO is 10.00%-12.00%; MgO is 2.00%-4.00%; ZrO2 is 5.00%-7.00%; Na2O is 2.00%-9.00%; Li2O is 0-2.00%; B2O3 is 0-8.00%; and the content of each oxide in the substrate glass also satisfies the following conditions:
[0165] ①X=((Na2O+B2O3) / ZrO2) / Al2O3, X≥2.00;
[0166] ②Y=ln[(Na2O+B2O3) / ZrO2], Y≥0;
[0167] ③Z=(SiO2+Al2O3-MgO-ZnO) / (Li2O+Na2O+B2O3), 4.00≤Z≤10.00;
[0168] In formulas ① to ③, oxide represents the mass percentage of the oxide component;
[0169] Step 2: heat-treating the substrate glass to obtain the microcrystalline glass. The heat treatment includes nucleation treatment and / or crystallization treatment. It should be understood that when heat-treating the substrate glass, one-step heat treatment or two-step or more-step heat treatment can be performed. If a one-step heat treatment is performed, it means that the nucleation treatment is not performed separately, and the nucleation and target crystal growth are directly performed in a one-step heating process, which can be understood as directly performing a crystallization treatment. If a two-step heat treatment is performed, it means that a two-step heating process is performed, first a nucleation treatment, i.e., a nucleation treatment, is performed, and then a target crystal growth treatment, i.e., a crystallization treatment, is performed.
[0170] In some embodiments of the present invention, in step 2, when the nucleation treatment is performed, the nucleation temperature is 650°C to 850°C, preferably 650°C to 750°C, and the nucleation treatment time is 0 to 72 hours, preferably 0 to 24 hours.
[0171] In some embodiments of the present invention, in step 2, when the crystallization treatment is performed, the crystallization temperature is 700°C to 1000°C, preferably 700°C to 850°C, and the crystallization treatment time is 0.1 to 72 hours, preferably 0.1 to 24 hours.
[0172] It should be understood that, in the present invention, the nucleation treatment time refers to the time for keeping the crystallization furnace warm to the set nucleation temperature at a set heating rate; the crystallization treatment time refers to the time for keeping the crystallization furnace warm to the set crystallization temperature at a set heating rate.
[0173] In some embodiments of the present invention, in step 2, during the heat treatment, the heating rate is controlled to be 5 to 30° C. / min, preferably 5 to 15° C. / min.
[0174] In some embodiments of the present invention, the content of each oxide in the substrate glass also satisfies the following conditions:
[0175] ④W=(0.8×(Al2O3-SiO2)+1.5×(ZnO-MgO)) / ZrO2, 0≤W≤3.00; In formula ④, oxide represents the mass percentage of the oxide component.
[0176] In some embodiments of the present invention, the substrate glass further includes 0 to 3.00 wt % of BaO and / or 0 to 2.00 wt % of Y2O3.
[0177] In some embodiments of the present invention, the substrate glass is substantially free of TiO2 and / or P2O5.
[0178] Finally, the microcrystalline glass obtained in the above step 2 can be cold processed as needed. The cold processing is to process the microcrystalline glass into the required microcrystalline glass sample. For example, the microcrystalline glass can be processed into a polished sheet of the required size by one or more of slicing, grinding, and polishing, such as a polished sheet with a length, width, and thickness of 50mm×50mm×0.7mm.
[0179] In the present invention, those skilled in the art can select the thickness of the microcrystalline glass according to the requirements. Exemplarily, the thickness of the microcrystalline glass is 0.2-5.0 mm.
[0180] Second, the present invention also provides a substrate glass, which can be used to obtain the above-mentioned microcrystalline glass after heat treatment and crystallization of the substrate glass; it should be understood that in the present invention, the composition of the substrate glass is the same as the composition of the microcrystalline glass in terms of the mass percentage of oxides;
[0181] According to the mass percentage of oxides, the substrate glass includes the following components: 30.00%≤SiO2<35.00%; Al2O3 is 30.00%~40.00%; ZnO is 10.00%~12.00%; MgO is 2.00%~4.00%; ZrO2 is 5.00%~7.00%; Na2O is 2.00%~9.00%; Li2O is 0~2.00%; B2O3 is 0~8.00%; at the same time, the content of each oxide in the microcrystalline glass also meets the following conditions:
[0182] ①X=((Na2O+B2O3) / ZrO2) / Al2O3, X≥2.00;
[0183] ②Y=ln[(Na2O+B2O3) / ZrO2], Y≥0;
[0184] ③Z=(SiO2+Al2O3-MgO-ZnO) / (Li2O+Na2O+B2O3), 4.00≤Z≤10.00;
[0185] In formulae ① to ③, oxide represents the mass percentage of the oxide component.
[0186] In some embodiments of the present invention, the content of each oxide in the substrate glass also satisfies the following conditions:
[0187] ④W=(0.8×(Al2O3-SiO2)+1.5×(ZnO-MgO)) / ZrO2, 0≤W≤3.00; In formula ④, oxide represents the mass percentage of the oxide component.
[0188] In some embodiments of the present invention, the substrate glass further includes 0 to 3.00 wt % of BaO and / or 0 to 2.00 wt % of Y2O3.
[0189] In some embodiments of the present invention, the substrate glass is substantially free of TiO2 and / or P2O5.
[0190] In some embodiments of the present invention, the molding method of the substrate glass includes but is not limited to float, overflow, rolling or casting processes. Exemplarily, the components are mixed evenly according to the formula, and after melting and molding, cooling and annealing are performed to obtain the substrate glass. For example, the substrate glass raw material can be melted at a melting temperature of 1480°C to 1650°C, the molten glass liquid can be molded, and after molding, cooling and annealing can be performed to obtain the substrate glass. The preferred annealing temperature is 500°C to 650°C, and the annealing is preferably kept warm for 12 to 48 hours.
[0191] In some embodiments of the present invention, when preparing the substrate glass, a clarifier may be added to the substrate glass. The clarifier includes but is not limited to SnO2, Sb2O3, and NaCl. Based on the total mass of the substrate glass, the amount of the clarifier added is 0.01wt% to 2.00wt%, preferably 0.01wt% to 1.50wt%.
[0192] 3. The present invention also provides a chemically strengthened glass, which is obtained by subjecting the above-mentioned glass-ceramics or substrate glass to chemical strengthening treatment, wherein the chemically strengthened glass comprises a compressive stress layer and a tensile stress layer.
[0193] The chemically strengthened glass provided by the present invention includes a strengthened glass product obtained by chemically strengthening a base glass and a strengthened microcrystalline glass obtained by chemically strengthening a microcrystalline glass.
[0194] It should be understood that after the chemical strengthening ion exchange process, the composition of the surface of the glass-ceramic or substrate glass may be different from the composition of the newly formed glass-ceramic or substrate glass (i.e., the glass-ceramic or substrate glass that has not undergone ion exchange). In other words, the composition of the compressive stress layer formed on the surface of the strengthened glass-ceramic / strengthened glass by ion exchange may be different from the composition of the glass-ceramic or substrate glass. This is because during ion exchange, one type of alkali metal ion (e.g., Li + Or Na + ) will be replaced by larger alkali metal ions (e.g., Na + or K + ) is replaced by, such as Na in glass + K in strengthening salt bath + Exchange, K +Replaced by, and / or, Li in glass + and Na in the strengthening salt bath + Exchange, by Na + However, in the embodiment, the composition of the glass-ceramics or substrate glass at the center of the depth of the glass product or near the center of the depth still has the composition of the glass-ceramics or substrate glass just formed. That is, the composition of the tensile stress layer in the strengthened glass-ceramics / strengthened glass that has not undergone ion exchange still has the composition of the glass-ceramics or substrate glass.
[0195] Since the chemical strengthening process involves the exchange of alkali metal ions, and the main crystalline phase of the microcrystalline glass of the present invention is (Zn, Mg)Al2O4, and the secondary crystalline phase includes one or more of tetragonal ZrO2, Zn2SiO4, and Mg2SiO4. It does not contain alkali metal ions and does not participate in ion exchange, so the crystalline phase composition does not change basically before and after strengthening. Therefore, the main crystalline phase of the strengthened microcrystalline glass obtained after chemical strengthening is still (Zn, Mg)Al2O4, and the secondary crystalline phase includes one or more of tetragonal ZrO2, Zn2SiO4, and Mg2SiO4.
[0196] In some embodiments of the present invention, the surface K2O concentration of the strengthened glass-ceramics is ≥7.00wt%, preferably 7.00-15.00wt%. In some embodiments, the surface K2O concentration may be 7.00wt%-8.00wt%, 7.00wt%-9.00wt%, 7.00wt%-10.00wt%, 7.00wt%-11.00wt%, 7.00wt%-12.00wt%, 7.00wt%-13.00wt%, 7.00wt%-14.00wt%, 7.00wt%-15.00wt%. %, 8.00wt% to 10.00wt%, 9.00wt% to 14.00wt%, 9.00wt% to 13.00wt%, 7.00wt%, 8.00wt%, 9.00wt%, 10.00wt%, 11.00wt%, 12.00wt%, 13.00wt%, 14.00wt%, 15.00wt%, etc. and all ranges and subranges between the above values;
[0197] In some embodiments of the present invention, in the strengthened glass-ceramics, along the thickness direction of the glass, the depth from any surface of the strengthened glass-ceramics to a position close to the surface and having the same potassium (K) concentration as that at the center of the strengthened glass-ceramics is ≥ 0.07t, preferably 0.07t to 0.10t, where t is the thickness of the strengthened glass-ceramics. In some embodiments, the depth from any surface of the strengthened glass-ceramics to a position close to the surface and having the same potassium (K) concentration as that at the center of the strengthened glass-ceramics can be 0.07t to 0.08t, 0.07t to 0.09t, 0.08t to 0.09t, 0.08t to 0.10t, 0.09t to 0.10t, 0.07t, 0.08t, 0.09t, 0.10t, etc. and all ranges and sub-ranges between the above values. For example, when the thickness of the strengthened glass-ceramics is 0.7 mm, along the thickness direction of the glass, the depth from any surface of the strengthened glass-ceramics to a position close to the surface and having the same potassium (K) concentration as that at the center of the strengthened glass-ceramics is ≥ 49.00 μm, more preferably 49.00 μm to 70.00 μm, and can also be 49.00 μm to 55.00 μm, 49.00 μm to 60.00 μm, 49.00 μm to 55 .00 μm, 50.00 μm to 60.00 μm, 50.00 μm to 70.00 μm, 60.00 μm to 70.00 μm, 55.00 μm to 70.00 μm, 65.00 μm to 70.00 μm, 49.00 μm, 50.00 μm, 55.00 μm, 60.00 μm, 65.00 μm, 70.00 μm, etc. and all ranges and sub-ranges between the above values. It should be understood that in embodiments, any of the above ranges can be combined with any other ranges. In the present invention, the greater the depth from any surface of the strengthened glass-ceramics to a position close to the surface and having the same potassium (K) concentration as that at the center of the strengthened glass-ceramics, the deeper the K ions in the salt bath enter the glass-ceramics during chemical strengthening. Thus, the depth of the compressive stress layer formed by potassium-sodium exchange (i.e., the exchange of potassium ions in the salt bath with Na ions in the glass-ceramics) in the strengthened glass-ceramics is greater.
[0198] In some embodiments of the present invention, at a thickness of 0.7 mm, the single rod static pressure strength of the strengthened glass-ceramics is greater than or equal to 450N, preferably 450N to 650N. In some embodiments, the single rod static pressure strength may be 450N to 500N, 450N to 600N, 450N to 490N, 480N to 570N, 470N to 610N, 520N to 650N, 540N to 630N, 450N, 500N, 550N, 600N, 650N, etc. and all ranges and sub-ranges between the above values. It should be understood that in embodiments, any of the above ranges may be combined with any other ranges.
[0199] It should be understood that after chemical strengthening treatment, the Young's modulus of the microcrystalline glass will increase appropriately. Therefore, in some embodiments of the present invention, the Young's modulus of the strengthened microcrystalline glass is not less than 110 GPa, and is preferably 110 to 140 GPa.
[0200] In some embodiments of the present invention, the Vickers hardness of the strengthened glass-ceramics is not less than 750 kgf / mm 2 , preferably 750~900kgf / mm 2 , more preferably 800 to 900 kgf / mm 2 In some embodiments, the Vickers hardness of the strengthened glass-ceramics may be 750 kgf / mm 2 、800kgf / mm 2 、810kgf / mm 2 、820kgf / mm 2 、830kgf / mm 2 、840kgf / mm 2 、850kgf / mm 2 HV, 860kgf / mm 2 、870kgf / mm 2 、880kgf / mm 2 、890kgf / mm 2 、900kgf / mm 2 Etc., and all ranges and subranges between the above values. It should be understood that in embodiments, any of the above ranges can be combined with any other ranges.
[0201] It should be understood that in the present invention, after chemical strengthening treatment, the transmittance of the microcrystalline glass does not change substantially. At a thickness of 0.7 mm, for light of a wavelength of 550 nm, the transmittance of the microcrystalline glass of the present invention is greater than or equal to 85.00%, and preferably the transmittance is greater than or equal to 89.00%. Therefore, in some embodiments of the present invention, the strengthened microcrystalline glass is transparent in the visible light range and has excellent transmittance.
[0202] It should be understood that the main crystalline phase of the microcrystalline glass of the present invention is (Zn, Mg)Al2O4, and the secondary crystalline phase includes one or more of tetragonal ZrO2, Zn2SiO4, and Mg2SiO4, and does not contain alkali metal ions, so it does not participate in ion exchange, so the crystalline phase composition does not change substantially before and after strengthening. Therefore, in some embodiments of the present invention, in the strengthened microcrystalline glass, the crystal content is still maintained between 20.00 and 50.00wt%. In some embodiments of the present invention, in the strengthened microcrystalline glass, the average grain size is ≤15.00nm.
[0203] In some embodiments of the present invention, a gem mineral hardness pen with a Mohs hardness rating of 7 is fixed at a 45° angle using an automatic pencil hardness tester, and the surface of the strengthened microcrystalline glass is scratched under a load of 750g. The scratched microcrystalline glass is then observed under a 400x microscope, and there are no scratches on the surface of the strengthened microcrystalline glass.
[0204] In some embodiments of the present invention, the glass-ceramics or substrate glass is placed in a salt bath containing potassium salt at 380°C to 550°C for chemical strengthening treatment. The strengthening treatment time is 1h to 96h, preferably 1h to 48h, to obtain the chemically strengthened glass.
[0205] In some embodiments of the present invention, the potassium salt includes one or more of potassium nitrate, potassium sulfate, and potassium carbonate, preferably potassium nitrate.
[0206] In some embodiments, the salt bath containing potassium salt can be 100wt% potassium salt, preferably 100wt% potassium nitrate, or a mixed salt of potassium salt and sodium salt, preferably a mixed salt of potassium nitrate and sodium nitrate. The salt bath can also contain 0-1wt% lithium salt, preferably 0-1wt% lithium nitrate. When performing chemical strengthening treatment, one-step strengthening can be performed, or two-step or more-step strengthening can be performed.
[0207] In some embodiments, the strengthening time can be 1.00h to 5.00h, 1.00h to 6.00h, 3.00h to 10.00h, 5.00h to 10.00h, 7.00h to 12.00h, 9.00h to 24.00h, 12.00h to 36.00h, 24.00h to 44.00h, 8.00h to 24.00h, 9.00h to 44.00h, 25.00h to 36.00h h, 22.00h-37.00h, 48h-96h, 6.00h, 8.00h, 12.00h, 14.00h, 24.00h, 32.00h, 36.00h, 22.00h, 18.00h, 28.00h, 42.00h, 48.00h, 60.00h, 70.00h, 80.00h, 90.00h, 96.00h, etc., and all ranges and sub-ranges between the above values.
[0208] In some embodiments, the strengthening salt bath temperature can be 380°C to 400°C, 400°C to 450°C, 450°C to 500°C, 500°C to 550°C, 400°C to 420°C, 450°C, 480°C, 500°C, 510°C, 530°C, 540°C, 550°C, etc., and all ranges and sub-ranges between the above values.
[0209] 4. The present invention also provides a glass device, which is made from the above-mentioned microcrystalline glass, or made from the above-mentioned substrate glass, or made from the above-mentioned chemically strengthened glass.
[0210] The glass device of the present invention may be regular or irregular, and those skilled in the art may manufacture it according to the requirements.
[0211] 5. The present invention also provides an electronic device, which includes the above-mentioned microcrystalline glass or the above-mentioned substrate glass or the above-mentioned chemically strengthened glass.
[0212] The electronic device described in the present invention includes but is not limited to at least one of a mobile phone, a display (such as a car display, an aircraft display, etc.), a tablet computer, an electronic watch, a smart wearable (such as a smart bracelet, a smart watch, smart glasses), and a television.
[0213] In the electronic device of the present invention, a layer may or may not be provided on the surface of the cover.
[0214] Illustratively, the electronic device provided by the present invention includes:
[0215] a housing including a front surface, a back surface, and a side surface;
[0216] an electronic assembly at least partially located within the housing, the electronic assembly comprising at least a controller, a memory, and a display, the display being located on or adjacent to the front surface of the housing; and a cover substrate disposed over the display;
[0217] Wherein, at least a portion of at least one of the outer shell or the covering substrate comprises the microcrystalline glass or reinforced microcrystalline glass as described in any one of the above.
[0218] The transparent glass-ceramics and strengthened glass-ceramics of the present invention have excellent properties and can be included / applied in other products, as well as any products requiring a certain degree of transparency, scratch resistance or other combinations.
[0219] 6. The present invention is described by specific embodiments
[0220] Table 2: Formula of Examples S1 to S10
[0221]
[0222] Table 3 Comparative Examples D1 to D7 Formulations
[0223]
[0224]
[0225] Table 4 Characteristic parameters of glass-ceramics of Examples S1 to S10 and characteristic parameters of strengthened glass-ceramics
[0226]
[0227]
[0228] Note: In the table, 1. DOL K It refers to the position along the thickness direction of the glass, from any surface of the strengthened microcrystalline glass to the position close to the surface and having the same potassium (K) concentration as the center of the strengthened microcrystalline glass; 2. First, heat up to the nucleation temperature at the heat treatment heating rate, and after the nucleation treatment for a certain period of time, heat up to the crystallization temperature at this heating rate and crystallize for a certain period of time.
[0229] Table 5 Characteristic parameters of glass-ceramics of comparative examples D1 to D7 and characteristic parameters of strengthened glass-ceramics
[0230]
[0231]
[0232] Note: In the table, 1. DOLK refers to the position from any surface of the strengthened microcrystalline glass to the position close to the surface and having the same potassium (K) concentration as the center of the strengthened microcrystalline glass along the thickness direction of the glass; 2. First, the temperature is raised to the nucleation temperature at the heat treatment heating rate, and after the nucleation treatment for a certain period of time, the temperature is raised to the crystallization temperature at this heating rate and the crystallization treatment is carried out for a certain period of time.
[0233] Table 6 Anti-scratch test plan
[0234]
[0235] Table 7 Scratch test results of glass-ceramics and strengthened glass-ceramics of Examples S1 to S10 and Comparative Examples D1 to D7
[0236]
[0237] Note: Unless otherwise specified, in the category, "before strengthening" corresponds to the microcrystalline glass sheet, and "after strengthening" corresponds to the strengthened microcrystalline glass sheet. In D6, "before strengthening" corresponds to the base glass sheet, and "after strengthening" corresponds to the strengthened glass sheet.
[0238] Taking Example S1 as an example,
[0239] (1) Preparation of substrate glass:
[0240] According to the formula, 1000g of raw materials are mixed, and after the materials are mixed evenly for 30 minutes, 5g of NaCl clarifier is added. The obtained mixture is placed in a platinum crucible, melted at 1650°C for 5 hours, and then poured into a mold for molding and cooling. After cooling to 900°C, it is placed in a 620°C annealing furnace, annealed for 12 hours, and then cooled to room temperature with the furnace to obtain the substrate glass. The preparation of the substrate glass of other embodiments S2 to S10 is the same as that of embodiment S1.
[0241] (2) Preparation of glass-ceramics:
[0242] The temperature is raised to a nucleation temperature of 690°C at a heating rate of 10°C / min, and the nucleation treatment time is 240 minutes; then, the temperature is raised to a crystallization temperature of 760°C at a heating rate of 10°C / min, and the crystallization treatment time is 240 minutes to obtain a microcrystalline glass brick. The nucleation treatment time here refers to the time for the crystallization furnace to be heated to the set nucleation temperature at a set heating rate and then kept warm; the crystallization treatment time here refers to the time for the crystallization furnace to be heated to the set crystallization temperature at a set heating rate and then kept warm.
[0243] (3) Cold processing: The above-mentioned microcrystalline glass bricks are subjected to cold processing, and the cold processing includes shaping and slicing to obtain microcrystalline glass sheets of required sizes, such as microcrystalline glass sheets with a length, width and thickness of 50 mm×50 mm×0.7 mm.
[0244] After the slicing process, CNC processing, grinding processing, and polishing processing can be performed in sequence, or after the slicing process, at least one of CNC processing, grinding processing, and polishing processing can be selected to perform glass sheet modification processing.
[0245] The microcrystalline glass sample used for testing the physical properties of microcrystalline glass and performing chemical strengthening in Example S1 is a polished sheet with a length, width and thickness of 50 mm×50 mm×0.7 mm.
[0246] (4) Preparation of strengthened glass-ceramics: The above glass-ceramics sheet was placed in 100 wt % KNO3 at 480°C for a one-step chemical strengthening ion exchange for 6 h (360 min) to obtain strengthened glass-ceramics.
[0247] Tables 2 to 7 are respectively the formula tables of the embodiments and comparative examples, the characteristic parameters of the microcrystalline glass of the embodiments and comparative examples and the characteristic parameters of the strengthened microcrystalline glass, the anti-scratch test scheme, and the scratch test results of the microcrystalline glass of the embodiments and comparative examples and the strengthened microcrystalline glass.
[0248] The present invention strictly controls the content of each oxide in Examples S1 to S10, and regulates the content of important oxides through X, Y and Z, so that the obtained microcrystalline glass has a higher residual glass phase dissociation energy, and the spinel crystals expected by the present invention are formed in the microcrystalline glass, while maintaining excellent optical properties. By combining the main crystal phase (Zn, Mg) Al2O4) with high Young's modulus and shear modulus with the residual glass phase with high intrinsic strength, the obtained microcrystalline glass finally has high intrinsic strength and has better scratch resistance than the existing spinel system microcrystalline glass. After strengthening the microcrystalline glass to meet specific stress characteristics, the strengthened microcrystalline glass is given excellent surface stress characteristics and deep stress characteristics, which ultimately greatly improves the mechanical properties of the strengthened microcrystalline glass of the present invention, so that the strengthened microcrystalline glass can achieve a scratch resistance comparable to that of sapphire glass.
[0249] Exemplary:
[0250] The microcrystalline glass of Example S1 of the present invention can pass the scratch verification with a load of 250g, 500g, gem mineral hardness pen No. 7 (Mohs hardness 7) and a load of 750g, gem mineral hardness pen No. 6 (Mohs hardness 6). There is no scratch on the surface of the microcrystalline glass after scratching, and the effect after scratching is obvious. Figure 4 .
[0251] The microcrystalline glass of Examples S2 and S8 of the present invention can pass the scratch test with a load of 750g and a gem mineral hardness pen No. 7 (Mohs hardness 7). There are no scratches on the surface of the microcrystalline glass after scratching. Figure 5 .
[0252] The scratch resistance of the strengthened micro-ceramic glass strengthened by the micro-ceramic glass of the present invention is further improved compared with that of the micro-ceramic glass. The scratch resistance of the strengthened micro-ceramic glass of the present invention is comparable to that of sapphire glass, and can meet the demand for cover glass of high-end electronic products.
[0253] Exemplary:
[0254] The strengthened microcrystalline glass of Example S1 of the present invention can pass the scratching test with a load of 750g, a gem mineral hardness pen No. 6 (Mohs hardness 6) and a load of 750g, a gem mineral hardness pen No. 7 (Mohs hardness 7). There is no scratch on the surface of the microcrystalline glass after scratching, and the effect after scratching is obvious. Figure 6 .
[0255] In the scratch test of the strengthened micro-ceramics of Examples S2 and S8 of the present invention with a load of 750g and a gem mineral hardness pen No. 8 (Mohs hardness 8), the scratch effect on the surface of the micro-ceramics after scratching is close to the scratch effect of the sapphire glass tested under the same conditions. Figure 7This indicates that the anti-scratch effect of the strengthened glass-ceramics of Examples S2 and S8 of the present invention is comparable to that of sapphire glass.
[0256] Comparative Examples D1 to D7 cannot fully meet the requirements of the glass formula scheme of the present invention, and the stress characteristics after strengthening do not meet the requirements of the scheme of the present invention. The finally obtained microcrystalline glass and strengthened microcrystalline glass are different from the present invention, and the scratch resistance is obviously inferior to the scheme of the embodiment of the present invention.
[0257] Exemplary:
[0258] The strengthened micro-ceramics of comparative examples D1 and D2 cannot pass the scratch test with a load of 750g and a gem mineral hardness pen No. 7 (Mohs hardness 7). After scratching, there are obvious scratches on the surface of the micro-ceramics. Figure 8 Comparing the strengthened microcrystalline glass of D1 and D2, the scratch resistance of the strengthened microcrystalline glass of D1 is better than that of D2.
[0259] The dissociation energy per unit volume of the residual glass phase in comparative example D5 is relatively high, which is 75.46 kJ·cm -3 However, the improvement of the dissociation energy of this scheme comes from the fact that the system contains a large amount of Li. The present invention has found through experiments that this scheme cannot obtain a transparent sample through heat treatment.
[0260] Comparative Example D6 is a mainstream microcrystalline glass product in the existing cover plate market. The microcrystalline glass of Comparative Example D6 cannot pass the scratch test with a load of 750g and a gem mineral hardness pen No. 6 (Mohs hardness 6). After scratching, there are obvious scratches on the surface of the microcrystalline glass. The scratches are deep and wide, accompanied by fish scale embossing or scratch debris. The effect after scratching is not obvious. Fig. 9 The strengthened micro-ceramic glass of comparative example D6 still cannot pass the scratch test with a load of 750g and a gem mineral hardness pen No. 6 (Mohs hardness 6). After scratching, there are obvious scratches on the surface of the micro-ceramic glass. Fig.10 .
[0261] In addition, the heat treatment temperature of all embodiments of the present invention is lower than that of comparative examples D1 to D5, indicating that the substrate glass obtained by the formula system of the present invention can obtain a transparent microcrystalline glass with a main crystal phase of zinc-magnesium spinel solid solution and good optical properties when the heat treatment temperature does not exceed 800°C. Compared with the prior art, the component system of microcrystalline glass provided by the present invention can obviously reduce the heat treatment temperature, thereby reducing the difficulty of mass production of spinel microcrystalline glass and improving the mass production performance of spinel microcrystalline glass, that is, the microcrystalline glass formula system of the present invention has high mass production feasibility. At the same time, the formula system of the present invention contains relatively low lithium, and the raw material cost is much lower than the mainstream lithium aluminum silicon microcrystalline glass in the market, which has good application prospects.
[0262] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the technical solution. Those skilled in the art should understand that those modifications or equivalent substitutions of the technical solution of the present invention that do not depart from the purpose and scope of the technical solution should be included in the scope of the claims of the present invention.
Claims
1. A transparent microcrystalline glass with high scratch resistance, wherein the microcrystalline glass contains crystal grains, characterized in that: The main crystalline phase of the microcrystalline glass is (Zn, Mg)Al2O4; according to the mass percentage of the oxides, the microcrystalline glass includes the following components: 30.00%≤SiO2<35.00%; Al2O3 is 30.00%-40.00%; ZnO is 10.00%-12.00%; MgO is 2.00%-4.00%; ZrO2 is 5.00%-7.00%; Na2O is 2.00%-9.00%; Li2O is 0-2.00%; B2O3 is 0-8.00%; at the same time, the content of each oxide in the microcrystalline glass also meets the following conditions: ①X=((Na2O+B2O3) / ZrO2) / Al2O3, X≥2.00; ②Y=ln[(Na2O+B2O3) / ZrO2], Y≥0; ③Z=(SiO2+Al2O3-MgO-ZnO) / (Li2O+Na2O+B2O3), 4.00≤Z≤10.00; ④W=(0.8×(Al2O3-SiO2)+1.5×(ZnO-MgO)) / ZrO2,0≤W≤3.00; In formulae ① to ④, oxide represents the mass percentage of the oxide component.
2. The transparent microcrystalline glass according to claim 1, characterized in that: The contents of each oxide in the microcrystalline glass also meet the following conditions: ④W=(0.8×(Al2O3-SiO2)+1.5×(ZnO-MgO)) / ZrO2 has a value of 1.00 to 3.00; and / or, ① The value of X=((Na2O+B2O3) / ZrO2) / Al2O3 is 3.00~9.00; and / or, ③The value of Z=(SiO2+Al2O3-MgO-ZnO) / (Li2O+Na2O+B2O3) is 4.00~9.
00.
3. The transparent microcrystalline glass according to claim 2, characterized in that: The W value is 1.00 to 2.
50.
4. The transparent microcrystalline glass according to claim 1, characterized in that: Calculated by molar percentage of oxides, the microcrystalline glass meets the following conditions: the molar percentage of Al2O3 is greater than the sum of the molar percentages of MgO and ZnO; and the theoretical crystallinity of the microcrystalline glass is above 30.00wt%.
5. The transparent microcrystalline glass according to claim 4, characterized in that: The theoretical crystallinity of the glass-ceramics is 30.00 wt % to 50.00 wt %.
6. The transparent microcrystalline glass according to claim 4, characterized in that: When the microcrystalline glass meets the theoretical crystallinity, the residual glass phase unit volume dissociation energy U in the microcrystalline glass is not less than 71.00 kJ·cm -3 .
7. The transparent microcrystalline glass according to claim 6, characterized in that: When the microcrystalline glass meets the theoretical crystallinity, the dissociation energy per unit volume of the residual glass phase in the microcrystalline glass is 71.00 kJ·cm -3 ~134.00kJ·cm -3 .
8. The transparent glass-ceramics according to claim 1, characterized in that: The secondary crystalline phase of the microcrystalline glass includes one or more of tetragonal ZrO2, Zn2SiO4, and Mg2SiO4.
9. The transparent microcrystalline glass according to claim 1, characterized in that: In the microcrystalline glass, the mass percentage of SiO2 is 32.00% to 34.95%; and / or the mass percentage of Al2O3 is 32.00% to 38.00%; and / or ZnO is 10.00% to 11.48%; and / or MgO is 2.50% to 3.50%; and / or ZrO2 is 5.40% to 6.50%; and / or Na2O is 2.50% to 8.50%; and / or B2O3 is 2.50 to 8.00%.
10. The transparent glass-ceramics according to claim 1, characterized in that: The microcrystalline glass also includes 0-3.00wt% of BaO and / or 0-2.00wt% of Y2O3.
11. The transparent microcrystalline glass according to claim 1, characterized in that: The microcrystalline glass basically does not contain TiO2 and / or P2O5.
12. The transparent microcrystalline glass according to claim 1, characterized in that: In the microcrystalline glass, the average grain size is ≤15.00nm.
13. The transparent microcrystalline glass according to claim 12, characterized in that: In the microcrystalline glass, the average grain size is 1.00 to 10.00 nm.
14. The transparent glass-ceramics according to claim 13, characterized in that: In the microcrystalline glass, the average grain size is 4.50 to 8.00 nm.
15. The transparent microcrystalline glass according to claim 1, characterized in that: The Young's modulus of the microcrystalline glass is not less than 110 GPa.
16. The transparent microcrystalline glass according to claim 15, characterized in that: The Young's modulus of the microcrystalline glass is 110 to 130 GPa.
17. The transparent microcrystalline glass according to claim 15, characterized in that: The Young's modulus of the microcrystalline glass is greater than 114 GPa and less than or equal to 140 GPa.
18. The transparent glass-ceramics according to any one of claims 1 to 17, characterized in that: In the microcrystalline glass, the crystal content is 20.00-50.00wt%.
19. The transparent microcrystalline glass according to claim 18, characterized in that: In the microcrystalline glass, the crystal content is 25.00-50.00wt%.
20. The transparent microcrystalline glass according to claim 19, characterized in that: In the microcrystalline glass, the crystal content is 25.00-45.00wt%.
21. The transparent glass-ceramics according to any one of claims 1 to 17, characterized in that: Using an automatic pencil hardness tester, a gem mineral hardness pen with a Mohs hardness rating of 7 is fixed at a 45° angle, and the surface of the microcrystalline glass is scratched under a load of 500g, and the scratched microcrystalline glass is placed under a 400x microscope for observation, and there are no scratches on the surface of the microcrystalline glass; and / or Using an automatic pencil hardness tester and a gem mineral hardness pen with a Mohs hardness rating of 6 fixed at an angle of 45°, the surface of the microcrystalline glass was scratched under a load of 750g, and the scratched microcrystalline glass was observed under a 400x microscope. The surface of the microcrystalline glass had no scratches.
22. The transparent microcrystalline glass according to any one of claims 1 to 17, characterized in that: At a thickness of 0.7 mm, for light with a wavelength of 550 nm, the transmittance of the microcrystalline glass is greater than or equal to 85.00%.
23. The transparent microcrystalline glass according to claim 22, characterized in that: At a thickness of 0.7 mm, for light with a wavelength of 550 nm, the transmittance of the microcrystalline glass is greater than or equal to 89.00%.
24. The transparent glass-ceramics according to any one of claims 1 to 17, characterized in that: At a thickness of 0.7 mm, the optical b value of the microcrystalline glass is 0.20 to 1.
50.
25. The transparent microcrystalline glass according to claim 24, characterized in that: At a thickness of 0.7 mm, the optical b value of the microcrystalline glass is 0.35 to 1.
20.
26. The transparent glass-ceramics according to any one of claims 1 to 17, characterized in that: The microcrystalline glass is prepared by the following method: Step 1: Obtain substrate glass, which includes the following components in terms of mass percentage of oxides: 30.00%≤SiO2<35.00%; Al2O3 is 30.00%-40.00%; ZnO is 10.00%-12.00%; MgO is 2.00%-4.00%; ZrO2 is 5.00%-7.00%; Na2O is 2.00%-9.00%; Li2O is 0-2.00%; B2O3 is 0-8.00%; and the content of each oxide in the substrate glass also meets the following conditions: ①X=((Na2O+B2O3) / ZrO2) / Al2O3, X≥2.00; ②Y=ln[(Na2O+B2O3) / ZrO2], Y≥0; ③Z=(SiO2+Al2O3-MgO-ZnO) / (Li2O+Na2O+B2O3), 4.00≤Z≤10.00; ④W=(0.8×(Al2O3-SiO2)+1.5×(ZnO-MgO)) / ZrO2,0≤W≤3.00; In formulas ① to ④, oxide represents the mass percentage of the oxide component; Step 2: heat-treating the substrate glass to obtain the microcrystalline glass; the heat treatment includes nucleation treatment and / or crystallization treatment.
27. The transparent microcrystalline glass according to claim 26, characterized in that: In step 2, when performing the nucleation treatment, the nucleation temperature is 650° C. to 850° C., and the nucleation treatment time is 0 to 72 hours; and / or In step 2, when the crystallization treatment is performed, the crystallization temperature is 700° C. to 1000° C., and the crystallization treatment time is 0.1 to 72 hours; and / or In step 2, when performing heat treatment, the heating rate is controlled to be 5 to 30° C. / min.
28. The transparent microcrystalline glass according to claim 27, characterized in that: In step 2, when the nucleation treatment is performed, the nucleation temperature is 650° C. to 750° C., and the nucleation treatment time is 0 to 24 hours; and / or In step 2, when the crystallization treatment is performed, the crystallization temperature is 700° C. to 850° C., and the crystallization treatment time is 0.1 to 24 hours; and / or In step 2, when performing heat treatment, the heating rate is controlled to be 5 to 15°C / min.
29. The transparent glass-ceramics according to claim 26, characterized in that: The content of each oxide in the substrate glass also meets the following conditions: ④W=(0.8×(Al2O3-SiO2)+1.5×(ZnO-MgO)) / ZrO2 has a value of 1.00 to 3.00; and / or, ① The value of X=((Na2O+B2O3) / ZrO2) / Al2O3 is 3.00~9.00; and / or, ③ The value of Z=(SiO2+Al2O3-MgO-ZnO) / (Li2O+Na2O+B2O3) is 4.00~9.00; and / or The substrate glass further comprises 0-3.00 wt% of BaO and / or 0-2.00 wt% of Y2O3; and / or The substrate glass contains substantially no TiO2 and / or P2O5.
30. The transparent glass-ceramics according to claim 29, characterized in that: The value of W is 1.00 to 2.
50.
31. A substrate glass, characterized in that: The substrate glass can be heat-treated and crystallized to obtain the glass-ceramics as described in any one of claims 1 to 30; According to the mass percentage of oxides, the substrate glass includes the following components: 30.00%≤SiO2<35.00%; Al2O3 is 30.00%~40.00%; ZnO is 10.00%~12.00%; MgO is 2.00%~4.00%; ZrO2 is 5.00%~7.00%; Na2O is 2.00%~9.00%; Li2O is 0~2.00%; B2O3 is 0~8.00%; at the same time, the content of each oxide in the microcrystalline glass also meets the following conditions: ①X=((Na2O+B2O3) / ZrO2) / Al2O3, X≥2.00; ②Y=ln[(Na2O+B2O3) / ZrO2], Y≥0; ③Z=(SiO2+Al2O3-MgO-ZnO) / (Li2O+Na2O+B2O3), 4.00≤Z≤10.00; ④W=(0.8×(Al2O3-SiO2)+1.5×(ZnO-MgO)) / ZrO2,0≤W≤3.00; In formulae ① to ④, oxide represents the mass percentage of the oxide component.
32. The substrate glass according to claim 31, characterized in that: The content of each oxide in the substrate glass also meets the following conditions: ④W=(0.8×(Al2O3-SiO2)+1.5×(ZnO-MgO)) / ZrO2 has a value of 1.00 to 3.00; and / or, ① The value of X=((Na2O+B2O3) / ZrO2) / Al2O3 is 3.00~9.00; and / or, ③ The value of Z=(SiO2+Al2O3-MgO-ZnO) / (Li2O+Na2O+B2O3) is 4.00~9.00; and / or The substrate glass further comprises 0-3.00 wt% of BaO and / or 0-2.00 wt% of Y2O3; and / or The substrate glass contains substantially no TiO2 and / or P2O5.
33. The substrate glass according to claim 32, characterized in that: The value of W is 1.00 to 2.
50.
34. A chemically strengthened glass, characterized in that: The glass-ceramic material is obtained by subjecting the microcrystalline glass described in any one of claims 1 to 30 or the substrate glass described in any one of claims 31 to 33 to chemical strengthening treatment.
35. The chemically strengthened glass according to claim 34, wherein: The chemically strengthened glass can be obtained by placing the microcrystalline glass or substrate glass into a salt bath containing potassium salt at 380° C. to 550° C. for chemical strengthening treatment for 1 hour to 96 hours; the potassium salt includes one or more of potassium nitrate, potassium sulfate, and potassium carbonate.
36. The chemically strengthened glass according to claim 35, wherein: The strengthening treatment time is 1h to 48h.
37. The chemically strengthened glass according to claim 35, wherein: The potassium salt is potassium nitrate.
38. A glass device, which is made of the glass-ceramics according to any one of claims 1 to 30, or made of the substrate glass according to any one of claims 31 to 33, or made of the chemically strengthened glass according to any one of claims 34 to 37.
39. An electronic device comprising the glass-ceramics according to any one of claims 1 to 30, the substrate glass according to any one of claims 31 to 33, or the chemically strengthened glass according to any one of claims 34 to 37.
Citation Information
Patent Citations
Ion exchangeable, transparent gahnite-spinel glass ceramics with high hardness and modulus
CN111615500A
Spinel transparent microcrystalline glass with low melting temperature, preparation method and performance enhancing method thereof
CN111018354A
Tempered glass, microcrystalline glass and preparation method and application thereof
CN115286251A
Reinforced microcrystalline glass with high scratch resistance
CN118164678A
High rigidity glass-ceramic substrate
US20020032113A1
Cited By
Chemically strengthened microcrystalline glass and preparation thereof
CN121672942A
Chemically strengthened microcrystalline glass and preparation thereof
CN121672942B
Precursor glass for preparing spinel glass ceramics
CN121698567A
Spinel glass ceramic and preparation method thereof
CN121698570A
Spinel microcrystalline glass and preparation method thereof
CN121698570B