A composite inhibitor and method for defluorination and upgrading of copper concentrate
By using a composite inhibitor for defluorination and upgrading of copper concentrate, and through wet grinding and multiple flotation processes, the problem of controlling the fluoride content in high-fluoride copper concentrate during smelting was solved, achieving efficient defluorination and quality improvement of copper concentrate.
Patent Information
- Application Number
- CN202410415428.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-08
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2044-04-08
AI Technical Summary
In existing technologies, it is difficult to effectively control the fluoride content in high-fluoride copper concentrate during the smelting process, which leads to equipment corrosion and a decline in the quality of copper concentrate, and there is a lack of effective defluorination methods.
A composite inhibitor for defluorination and upgrading of copper concentrate is used, which consists of hydroxypropyl guar gum, sodium hexametaphosphate, guar gum and sodium citrate. Through wet grinding defluorination, slurry conditioning inhibition and multiple flotation processes, the selective separation of copper minerals and impurity minerals is achieved, thereby reducing the fluoride content.
It achieves efficient, low-cost, and environmentally friendly defluorination of copper concentrate, improves the quality and recovery rate of copper concentrate, avoids secondary fluoride pollution, and fills a technological gap in the field of mineral processing.
Abstract
Description
Technical Field
[0001] This invention belongs to the field of mineral processing technology, and particularly relates to a composite inhibitor and method for defluorination and upgrading of copper concentrate. Background Technology
[0002] Copper is an important non-ferrous metal widely used in machinery, medical, and chemical industries. Some copper deposits contain associated fluorine-bearing minerals, which can easily lead to excessive fluorine content in copper concentrate. During smelting, most of the fluorine in the copper concentrate enters the furnace gas as hydrogen fluoride. After passing through the preheating boiler and electrostatic precipitator, it enters the acid production system, exacerbating corrosion of equipment in the sulfuric acid purification system, reducing the activity of some catalysts in the conversion process, and corroding the ceramic tiles inside the dry absorption tower. The fluorine content in the waste acid solution increases, further corroding metal equipment such as filter presses and centrifuges. Smelters can only rely on strengthening incoming inspection, improving batching management, and enhancing fluorine fixation during the smelting process. Currently, there is no effective method for defluorinating high-fluorine copper concentrate. Therefore, research on controlling the fluorine content in copper concentrate entering the furnace and on copper concentrate defluorination is essential and of great significance. Summary of the Invention
[0003] The purpose of this invention is to provide a composite inhibitor and method for defluorination and upgrading of copper concentrate, thereby reducing the fluoride content in copper concentrate and solving the problem of difficulty in smelting copper concentrate with excessive fluoride content.
[0004] The technical solution adopted in this invention is as follows: A composite inhibitor for defluorination and upgrading of copper concentrate, comprising hydroxypropyl guar gum, sodium hexametaphosphate, guar gum and sodium citrate.
[0005] A further technical solution is that the weight ratio of hydroxypropyl guar gum, sodium hexametaphosphate, baking gum, and sodium citrate is: hydroxypropyl guar gum: sodium hexametaphosphate: baking gum: sodium citrate = (5~10): (1~2): (2~5): (5~10).
[0006] A method for defluorinating and upgrading copper concentrate using the aforementioned composite inhibitor for copper concentrate defluorination and upgrading includes the following steps: a: Wet grinding de-refining involves feeding copper concentrate and water into a mill for grinding. Mechanical de-refining removes residual reagents adsorbed on the mineral surface, resulting in a fresh mineral surface. This improves the selectivity of copper mineral components and fluorine-containing and gangue components in the copper concentrate. The liquid-to-solid ratio for wet grinding de-refining is 1:3 to 1:1. b: Slurry conditioning and inhibition. Add water to the grinding slurry to achieve a liquid-to-solid ratio of 3:1 to 5:1. Add 1200 to 2500 grams of compound inhibitor Tyf-16 per ton of defluorinated and upgraded copper concentrate to condition the slurry and inhibit fluoride-containing and gangue components. The conditioning and inhibition process takes 3 to 5 minutes. c: Copper roughing. Roughing is completed in two steps. After the slurry is prepared, a traditional frothing collector is added to perform copper roughing I, producing copper roughing I concentrate and copper roughing I tailings. Collectors are added to the copper roughing I tailings to enhance copper mineral collection and flotation, producing roughing II concentrate and roughing tailings. The copper roughing I concentrate and copper roughing II concentrate are combined as the roughing concentrate. d: Copper scavenging, using rougher tailings as scavenging feed, with the addition of a foaming collector before scavenging operations, producing scavenged concentrate and defluorinated tailings. e: Copper beneficiation, using rougher concentrate as beneficiation feed, adding 100-800 grams of compound inhibitor Tyf-16 to adjust the slurry for 3 minutes to produce copper concentrate.
[0007] A further technical solution involves returning the tailings from the first copper beneficiation process (BBE) and the concentrate from the first copper scavenging process (BBE) to step a (wet grinding and reagent removal) or step b (slurry conditioning and inhibition) for further slurry conditioning, inhibition, and subsequent steps.
[0008] A further technical solution involves two copper beneficiation processes, with the tailings from the second copper beneficiation process being returned to the feed from the first copper beneficiation process.
[0009] A further technical solution involves two copper scavenging cycles, with the concentrate from the second copper scavenging cycle being returned to the scavenging feed for the second copper scavenging cycle.
[0010] In summary, due to the adoption of the above technical solution, the beneficial effects of the present invention are: 1. Impurities in high-fluoride copper concentrate mainly consist of fluoride-containing minerals such as fluorite, fluorapatite, and cryolite, as well as calcium-magnesium-aluminum silicate minerals such as talc, chlorite, and serpentine that have adsorbed fluoride during weathering and alteration. These minerals, due to their unique layered crystal structure, have naturally good floatability, making them difficult to suppress. Conventional inhibitors have poor selective inhibition effects on these impurity minerals and copper minerals, often resulting in difficulties in suppressing impurity minerals and copper minerals together or simultaneously without inhibition. This is also a reason for the occurrence of high-fluoride copper concentrate. A composite inhibitor with a reasonable distribution of organic matter... The ratio of hydroxyl and carboxyl groups reacts with calcium, magnesium, and aluminum on the surface of impurity mineral crystals to produce precipitates and slightly soluble substances with very low solubility. This forms a hydrophilic organic coating layer on the surface, preventing the reaction of sulfide mineral flotation agents. At the same time, it has a good dispersing effect on these minerals, preventing them from agglomerating into larger particles and floating. However, it has a weaker effect on sulfide copper ores with relatively stable crystal structures, such as chalcopyrite, chalcocite, and bornite. This results in a strong selective inhibition effect of the composite inhibitor, achieving effective separation of impurity minerals from copper minerals and achieving the effect of reducing impurities and improving the quality of high-fluorine copper concentrate.
[0011] 2. Through wet grinding and reagent removal, and slurry conditioning and inhibition operations, fresh surfaces are created between impurity minerals and copper minerals in the high-fluoride copper concentrate. This reduces the proportion of hydrophobic surfaces formed by the interaction of minerals and reagents during the production of the high-fluoride copper concentrate, achieving mechanical reagent removal. Further addition of composite inhibitors provides selective inhibition. Copper roughing achieves basic separation of copper minerals from impurity minerals. Due to mechanical inclusions during flotation, some impurities float to the surface. The purpose of cleaning I is to further separate copper minerals from impurity minerals during flotation, achieving the desired copper concentrate quality. Further cleaning reduces the content of impurity minerals and improves concentrate quality. Simultaneously, during flotation, some target minerals exhibit differences in floatability due to collision probability with bubbles and the degree of dissociation between target and impurity minerals. Target minerals are lost in the tailings during roughing and scavenging. Further scavenging reduces this loss. For copper concentrate upgrading and impurity reduction flotation, the number of cleaning and scavenging operations is 2-3 times to achieve the goals of copper upgrading, impurity reduction, and reduced copper mineral loss.
[0012] 3. The overall beneficial effects of this invention are: (1) The inhibitor has the advantages of being low in toxicity, non-toxic, green and environmentally friendly, highly selective, effective in defluorination and quality improvement, and low in reagent cost.
[0013] (2) The process method is stable and reliable, with advantages such as low copper loss rate, low cost, easy process control, and less risk of secondary fluorine pollution.
[0014] (3) Compared with the control of fluorine-containing feed in smelting and the removal of fluorine during smelting, the mineral processing method is a technological gap in this field. This invention fills the gap in the defluorination and upgrading technology of fluorine-containing copper concentrate in the mineral processing field by studying the mineral processing inhibitor of fluorine components and developing the corresponding process. Detailed Implementation
[0015] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to embodiments.
[0016] Example 1: A copper mine in Kyrgyzstan produces copper concentrate with a copper grade of 17.80% and a fluorine content of 0.16%. Due to the excessive fluorine content, it is difficult to import into China. A defluorination and upgrading test was conducted. The compound inhibitor Tyf-16 was prepared in the following ratio: hydroxypropyl guar gum: sodium hexametaphosphate: guar gum: sodium citrate = 10:1:2:5. One unit of water was added to the mixer, followed by 1% sodium hexametaphosphate, 5% sodium citrate, and 2% tannin. After dissolving, 10% hydroxypropyl guar gum was added and dissolved. The mixture was then added to various processing steps.
[0017] First, wet milling with a liquid-to-solid ratio of 1:3 to remove reagents and mill the ore to a fineness of -0.074mm, achieving a 80% purity. The grinding product was adjusted to a liquid-to-solid ratio of 5:1, and 2500g / t of compound inhibitor was added for 5 minutes of adjustment. Conventional frothing agent Z-200 20g / t was used to condition the slurry for 2 minutes; roughing flotation I was then performed for 5 minutes. Roughing | After adding Z-200 10g / t to the flotation tailings for 2 minutes to adjust the slurry, roughing II operation is carried out, followed by flotation for 3 minutes; The roughing stage tailings were used as scavenging feed, with Z-200 added at 5 g / t, and scavenged for 3 minutes. The scavenged tailings were then used as defluorination tailings. The roughing concentrate I and roughing concentrate II are combined as feed for cleaning I, and 800g / t of compound inhibitor is added to adjust the slurry for 3 minutes before cleaning I operation is carried out. Fine I concentrate is treated with 200g / t of compound inhibitor and then processed for Fine II. Adding 100g / t of compound inhibitor to the II concentrate and then carrying out the III concentrate process produces defluorinated and upgraded copper concentrate. Tailings from the first and scavenging processes are returned to wet grinding for reagent removal, while tailings from the second and third processes are returned to the feed for the first and second processes, respectively. The final product is a high-quality copper concentrate with a copper grade of 22.67%, a fluorine content of 0.072%, and a copper recovery rate of 96.39%.
[0018] Example 2: A copper concentrate has a copper grade of 18.28% and a fluorine content of 0.13%. The main impurities in the copper concentrate are fluorapatite, fluorinated talc, chlorite, and serpentine. A defluorination and upgrading test was conducted. The compound inhibitor Tyf-16 was prepared in the following ratio: hydroxypropyl guar gum: sodium hexametaphosphate: guar gum: sodium citrate = 5: 1: 2: 5, using the same method as in Example 1.
[0019] First, wet milling with 2000g / t of lime at a liquid-to-solid ratio of 1:1 was carried out to remove reagents and grind the ore to a fineness of -0.074mm with a content of 85%. Because the copper concentrate production time is relatively long, some copper sulfide is oxidized to produce sulfuric acid. After adjusting the slurry, it is acidic, so lime is added to neutralize it. The grinding product was adjusted to a liquid-to-solid ratio of 3:1, and 1200g / t of compound inhibitor was added for 4 minutes of adjustment. Using conventional collector SN-43# 30g / t to adjust the slurry for 2 minutes, roughing flotation I was performed for 8 minutes; After adding SN-43# 10g / t to the roughing stage flotation tailings for 2 minutes, roughing stage II flotation was carried out for 5 minutes. The tailings from roughing stage II were used as feed for scavenging stage I, with SN-43# added at 10 g / t, and scavenged for 3 minutes. Tailings from scavenging stage I are used as feed for scavenging stage II, with SN-43# added at 5 g / t, and scavenged for 3 minutes. The tailings from the second scavenging stage are used as the final defluorination tailings. The roughing concentrate I and roughing concentrate II are combined as feed for cleaning I, and 600g / t of compound inhibitor is added to adjust the slurry for 3 minutes before cleaning I operation is carried out. Fine I concentrate is treated with 300g / t of compound inhibitor and then treated as Fine II concentrate. Adding 100g / t of compound inhibitor to the II concentrate and then performing the III concentrate process yields high-quality defluorinated copper concentrate.
[0020] Tailings from Selected Cement I and Scavenged Cement I are returned to the slurry conditioning and suppression operation. Tailings from Selected Cement II and Selected Cement III are returned to the feed for Selected Cement I and Selected Cement II, respectively. The concentrate from Scavenged Cement II is returned to the feed for Scavenged Cement I. The final product is a high-quality copper concentrate with a copper grade of 21.97%, a fluorine content of 0.091%, and a copper recovery rate of 97.39%.
[0021] Example 3: A copper concentrate has a copper grade of 23.28% and a fluorine content of 0.21%. The main impurities in the copper concentrate are cryolite, fluorite, talc, chlorite, and serpentine. A defluorination test was conducted on it. The compound inhibitor ratio was: hydroxypropyl guar gum: sodium hexametaphosphate: guar gum: sodium citrate = 10: 2: 5: 10, prepared as in Example 1.
[0022] First, wet milling with a liquid-to-solid ratio of 1:2 was performed to remove the reagents and grind the ore to a fineness of -0.074 mm with a content of 70%. The grinding product was adjusted to a liquid-to-solid ratio of 4:1, and 2000g / t of compound inhibitor was added for 5 minutes of adjustment. Conventional collector ester-105 20g / t, slurry preparation for 2min; Perform roughing flotation I for 4 minutes; After adding 10g / t of ester-105 to the flotation tailings for 2 minutes to adjust the slurry, roughing II operation was carried out, followed by flotation for 2 minutes. The tailings from roughing stage II were used as feed for scavenging stage I, with ester-105 added at 5 g / t, and scavenged for 2 min. Tailings from scavenging stage I were used as feed for scavenging stage II, with ester-105 added at 3 g / t, and scavenged for 2 minutes. The tailings from the second scavenging stage are used as the final defluorination and upgrading tailings. The roughing concentrate I and roughing concentrate II are combined as feed for cleaning I, and 600g / t of compound inhibitor is added to adjust the slurry for 3 minutes before cleaning I operation is carried out. Fine I concentrate is treated with 300g / t of compound inhibitor and then treated as Fine II concentrate. Adding 200g / t of compound inhibitor to the II concentrate and then carrying out the III concentrate process yields high-quality copper concentrate. Tailings from Selected I and Scavenged I are returned to the pulp conditioning and suppression process. Tailings from Selected II and Selected III are returned to the feed for Selected I and Selected II, respectively. The concentrate from Scavenged II is returned to the feed for Scavenged I. The final product is a high-quality copper concentrate with a copper grade of 25.43%, a fluorine content of 0.089%, and a copper recovery rate of 97.31%.
[0023] Examples show that the composite inhibitor has good inhibitory effect and adaptability on impurity minerals such as fluorite, fluorapatite, talc, chlorite, and serpentine. The above are only preferred embodiments of the present invention.
Claims
1. A composite inhibitor for defluorination and upgrading of copper concentrate, characterized in that, The inhibitor contains hydroxypropyl guar gum, sodium hexametaphosphate, guar gum and sodium citrate. The weight ratio of hydroxypropyl guar gum, sodium hexametaphosphate, guar gum and sodium citrate is: hydroxypropyl guar gum: sodium hexametaphosphate: guar gum: sodium citrate = (5~10): (1~2): (2~5): (5~10).
2. A method for defluorinating and upgrading copper concentrate using the composite inhibitor for defluorination and upgrading as described in claim 1, comprising the following steps: a: Wet grinding de-refining involves feeding copper concentrate and water into a mill for grinding. Mechanical de-refining removes residual reagents adsorbed on the mineral surface, resulting in a fresh mineral surface. This improves the selectivity of copper mineral components and fluorine-containing and gangue components in the copper concentrate. The liquid-to-solid ratio for wet grinding de-refining is 1:3 to 1:
1. b: Slurry conditioning and inhibition. Add water to the grinding slurry product from step a to achieve a liquid-to-solid ratio of 3:1 to 5:
1. Add 1200 to 2500 grams of compound inhibitor per ton of defluorinated and upgraded copper concentrate feed to condition the slurry and inhibit fluoride-containing and gangue components. The conditioning and inhibitor operation time is 3 to 5 minutes. c: Copper roughing. Roughing is completed in two steps. After the pulp is prepared, a foaming collector is added to perform copper roughing I operation, producing copper roughing I concentrate and copper roughing I tailings. Collector is added to the copper roughing I tailings to enhance copper mineral collection and flotation, producing roughing II concentrate and roughing tailings. The copper roughing I concentrate and copper roughing II concentrate are combined as the roughing concentrate. d: Copper scavenging, using the roughing tailings from step c as scavenging feed, supplemented with a foaming collector before scavenging operations, producing scavenged concentrate and defluorinated tailings. e: Copper beneficiation, using rougher concentrate as beneficiation feed, adding 100-800 grams of compound inhibitor to adjust the slurry for 3 minutes to produce copper concentrate.
3. The method for defluorination and upgrading of copper concentrate according to claim 2, characterized in that, The tailings from the first copper beneficiation and the concentrate from the first copper scavenging are returned to step a (wet milling and reagent removal) or step b (slurry conditioning and inhibition) for further slurry conditioning, inhibition, and subsequent steps.
4. The method for defluorination and upgrading of copper concentrate according to claim 3, characterized in that, The copper beneficiation process is repeated twice. The tailings from the second copper beneficiation are returned to the feed from the first copper beneficiation.
5. The method for defluorinating and upgrading copper concentrate according to claim 4, characterized in that, The copper scavenging process is repeated twice. The concentrate from the second copper scavenging process is returned to the scavenging feed for the second copper scavenging process.
Citation Information
Patent Citations
Mineral separation process capable of separating copper, lead, zinc polymetal sulphide ore
CN101507951A
Gangue inhibitor and beneficiation method of copper sulfide ore containing easily floated gangue minerals
CN110653073A