Lithium-containing compound-coated lithium-rich manganese-based cathode materials, their preparation methods and applications
By using a high-temperature coating machine to perform stepwise high-temperature melting coating under mechanical stirring, the problem of uneven coating of lithium-rich manganese-based cathode materials is solved, the cycle performance and first coulombic efficiency of lithium-ion batteries are improved, the process flow is simplified, and it is suitable for mass production.
Patent Information
- Application Number
- CN202410378755.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-29
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2044-03-29
AI Technical Summary
Existing technologies struggle to achieve uniform coating of lithium-rich manganese-based cathode materials without increasing process complexity and cost, and existing methods may affect the material's cycle performance and energy density.
A high-temperature coating machine is used to perform stepwise high-temperature melting under mechanical stirring. The lithium-containing compound is coated at different temperatures by utilizing its melting point to construct a uniform lithium-containing compound coating layer, thus avoiding secondary heat treatment.
Uniform coating of lithium-rich manganese-based cathode materials was achieved, improving the cycle performance and first coulombic efficiency of lithium-ion batteries, simplifying the process, and making it suitable for mass production.
Smart Images

Figure CN118198322B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of lithium-ion battery cathode material technology, specifically relating to a lithium-containing compound-coated lithium-rich manganese-based cathode material, its preparation method, and its application. Background Technology
[0002] Lithium-rich manganese-based cathode materials (xLi2MnO3·(1-x)LiMO2, M=Fe, Co, Ni, etc.) have attracted widespread attention from researchers worldwide due to their advantages such as high energy density, high reversible specific capacity, and low cost. They have shown great application potential in the new energy battery market and are regarded as one of the most promising cathode materials for the next generation of high-energy lithium-ion batteries. However, research on lithium-rich manganese-based cathode materials is mainly concentrated in the laboratory stage and is difficult to commercialize. The main reasons are: (1) Due to the irreversible presence of some Li in the lithium-rich phase structure during the first activation process, the initial coulombic efficiency of the lithium-rich material is low; (2) During the cycling process, the layered phase of Li2MnO3 in the lithium-rich phase structure will gradually transform into the spinel phase of LiMn2O4, resulting in severe voltage decay; (3) During the cycling process, the lithium-rich material will undergo phase transition and interfacial side reactions, resulting in poor cycling stability and rate performance. Therefore, it is of great significance to improve lithium-rich materials, maintain their advantages of high capacity and high energy, and at the same time enable them to have good cycle stability and rate performance.
[0003] Currently, improving the performance of lithium-rich manganese-based cathode materials mainly involves surface coating and elemental doping. These methods can improve the cycle stability and rate performance of lithium-rich materials to a certain extent, while suppressing voltage decay. Common coatings include metal oxides (Al2O3, TiO2), phosphates (Li3PO4, AlPO4), vanadates (Li3VO4), zirconates (Li2ZrO3), and fluorides (AlF3, CaF2). These coatings can effectively improve the interfacial stability and surface ionic / electronic conductivity of lithium-rich materials. Currently, the commonly used coating methods are solid-phase and liquid-phase methods. The solid-phase method is relatively simple, but it is difficult to obtain a uniform and ordered coating layer. Compared to the solid-phase method, the liquid-phase method can obtain a more uniform and ordered coating layer, but it generally requires secondary heat treatment, making the process cumbersome, and it involves the addition of solvents such as water. Prolonged contact between lithium-rich materials and water can cause structural changes, affecting their cycle performance.
[0004] Lithium-containing compounds, such as lithium zirconate, lithium vanadate, and lithium borate, generally possess good thermal stability and excellent lithium-ion transport properties. Coating these compounds onto the surface of lithium-rich materials can effectively prevent direct contact between the electrolyte and the cathode material surface, thus preventing decomposition reactions. Simultaneously, it can accelerate lithium-ion transport and improve the cycle performance and rate capability of lithium-ion batteries. Currently, industrial methods for coating lithium-containing compounds mainly include liquid-phase and solid-phase methods. However, existing methods suffer from problems such as uneven coating or cumbersome processes.
[0005] Patent CN 109103423 A discloses a solid-phase method for preparing lithium vanadate-coated lithium-rich manganese-based cathode materials. The method involves first mixing a synthesized carbonate precursor with a lithium source and then calcining it to obtain a lithium-rich manganese-based cathode material. After crushing, the precursor is mixed uniformly with lithium vanadate powder, and then calcined again to obtain lithium vanadate-coated lithium-rich manganese-based cathode material. This method has a simple process flow and can effectively improve the cycle stability of the material. However, uneven coating may reduce the specific capacity and energy density of the material.
[0006] Patent CN 113078316 A discloses a liquid-phase method for preparing lithium molybdate-coated lithium-rich manganese-based cathode materials. The method involves first ball-milling and dispersing MnO2 balls with at least two of a Li, Ni, Co, Al, or Mg source along with a ball-milling aid. After evaporating the solvent, a dry powder is obtained. This powder is then pre-sintered to obtain a lithium-rich manganese-based precursor. The precursor is then dispersed with a Mo source, a Li source, and the ball-milling aid, followed by a second sintering process to obtain the lithium molybdate-coated lithium-rich manganese-based cathode material. While this method improves the cycle stability of the material, it requires a secondary heat treatment, making the process cumbersome.
[0007] Therefore, it is necessary to provide a coating method that can achieve uniform coating without requiring secondary heat treatment. Summary of the Invention
[0008] One of the objectives of this invention is to provide a method for preparing lithium-rich manganese-based cathode materials coated with lithium-containing compounds. The method involves solid-phase melting of the coating material at different temperatures based on the melting points of different lithium-containing compounds, thereby constructing a coating layer of one or more lithium-containing compounds on the surface of the lithium-rich material. The coating layer has uniform thickness and stable properties, resulting in a significant improvement in the cycle performance of the lithium-ion battery and a significant increase in the first coulombic efficiency.
[0009] The second objective of this invention is to provide a lithium-containing compound-coated lithium-rich manganese-based cathode material prepared by this method.
[0010] The third objective of this invention is to provide an application of the lithium-containing compound-coated lithium-rich manganese-based cathode material in the preparation of lithium-ion battery cathodes.
[0011] In order to achieve the above-mentioned objectives of the present invention, the following technical solution is adopted:
[0012] In a first aspect, the present invention provides a method for preparing a lithium-rich manganese-based cathode material coated with a lithium-containing compound, comprising the following steps:
[0013] After uniformly mixing the lithium-containing compound and the lithium-rich manganese-based cathode material, the mixture is heated to the melting point of the lithium-containing compound. Under the combined action of mechanical mixing and high-temperature melting, the lithium-containing compound coats the lithium-rich manganese-based cathode material, resulting in a lithium-containing compound-coated lithium-rich manganese-based cathode material.
[0014] The above process can be repeated once or multiple times to achieve one or more coatings.
[0015] The above process can be carried out in a high-temperature coating machine, such as an example of a high-temperature coating machine. Figure 1 As shown, the equipment is a conical mixing drum with a central rotating shaft. The centrifugal force generated by the high-speed rotation of the shaft pushes the product against the inner wall of the drum. The blades on the surface of the drum rotate at high speed, causing the material to rise and then fall to the bottom of the drum. During the mixing process, the heating plate covering the drum wall can heat the drum wall.
[0016] The coated lithium-rich material has a uniform and orderly coating layer on its surface.
[0017] In some embodiments, the mass of the lithium-containing compound is 0.1%-10% of the mass of the lithium-rich manganese-based cathode material, such as 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, but not limited thereto.
[0018] In some embodiments, the lithium-containing compound is, for example, lithium zirconate, lithium vanadate, lithium borate, lithium molybdate, lithium tungstate, or lithium phosphate, but is not limited thereto.
[0019] In some implementations, the method includes the following steps:
[0020] S1: After the first lithium-containing compound and the lithium-rich manganese-based cathode material are stirred evenly in a high-temperature coating machine, the temperature is raised to the melting point temperature t1 of the first lithium-containing compound under an air atmosphere for high-temperature melting. After stirring and keeping warm for a period of time, the heating is stopped to obtain the first lithium-containing compound coated with the lithium-rich manganese-based cathode material.
[0021] Further preferably, the method further includes the following steps:
[0022] S2: A second lithium-containing compound is added to the first lithium-containing compound coating lithium-rich manganese-based cathode material. After stirring evenly in a high-temperature coating machine, the mixture is heated to the melting point temperature t2 of the second lithium-containing compound in an air atmosphere. After stirring and keeping warm for a period of time, the heating is stopped and the mixture is cooled to room temperature to obtain the first and second lithium-containing compound composite coated lithium-rich manganese-based cathode material.
[0023] Similarly, the Nth lithium-containing compound can be coated using the same method. The number of high-temperature melting and heat preservation sections corresponds to the number of types of coating materials.
[0024] In one specific implementation, the method includes the following steps:
[0025] S1: The first lithium-containing compound and the lithium-rich manganese-based cathode material are first stirred and premixed evenly in a high-temperature coating machine at a speed of 800-1000 rpm, and then stirred at a speed of 1500-1600 rpm. At the same time, the temperature of the coating chamber is heated to the melting point temperature t1 of the first lithium-containing compound at a heating rate of 5℃ / min. Stirring and heat preservation are maintained for 5-6 hours to obtain the first lithium-containing compound coated lithium-rich manganese-based cathode material.
[0026] S2: Preferably, based on step S1, a second lithium-containing compound is added, and after mixing evenly, it is first stirred and premixed at a speed of 800-1000 rpm, and then stirred at a speed of 1500-1600 rpm. At the same time, the temperature of the coating chamber is heated to the melting point temperature t2 of the second lithium-containing compound at a heating rate of 5℃ / min. After stirring and keeping warm for 8-10 hours, stirring is stopped, and the mixture is cooled to room temperature to obtain the first and second lithium-containing compound composite coated lithium-rich manganese-based cathode material.
[0027] This invention improves upon the traditional solid-state method by conducting the entire process in a high-temperature coating machine. The lithium-containing compound is heated to its melting point to achieve coating. This combines the advantages of the traditional solid-state method, which is simple and requires no secondary heat treatment, and the traditional liquid-state method, which provides uniform coating. At the same time, it avoids the disadvantages of the traditional solid-state method, which results in uneven coating, and the traditional liquid-state method, which is complex and requires secondary heat treatment.
[0028] Secondly, the present invention provides a method for preparing a lithium-containing compound-coated lithium-rich manganese-based cathode material. The prepared lithium-containing compound-coated lithium-rich manganese-based cathode material includes a lithium-rich manganese-based cathode material (substrate material) and at least one layer of uniformly distributed lithium-containing compound coating layer.
[0029] Preferably, the lithium-containing compound-coated lithium-rich manganese-based cathode material comprises, from the inside out, a lithium-rich manganese-based cathode material (substrate material), a first lithium-containing compound coating layer, and a second lithium-containing compound coating layer.
[0030] Preferably, the coating layer accounts for 0.1%-10 wt% of the base material by mass.
[0031] The lithium-rich material coated with lithium compounds of the present invention can melt the lithium compounds during the coating process through simple mechanical mixing and auxiliary high temperature action, achieving the effect of liquid phase coating and successfully constructing a uniform lithium compound coating layer on the material surface, which can effectively improve the cycle performance of the electrode material.
[0032] Thirdly, the present invention provides an application of the lithium-containing compound-coated lithium-rich manganese-based cathode material in the preparation of lithium-ion battery cathodes.
[0033] Beneficial effects:
[0034] (1) This invention utilizes a high-temperature coating machine to achieve liquid-phase coating by heating and melting while mechanically stirring. A lithium-containing compound coating layer is successfully constructed on the surface of lithium-rich materials using a stepwise high-temperature melting method, achieving the coating effect of the liquid-phase method, and the coating layer is stable and uniform.
[0035] (2) The synthesis method of the present invention is simple, the reaction conditions are easy to control, secondary heat treatment is avoided, the raw materials are cheap and readily available, and it is suitable for large-scale production.
[0036] (3) The lithium-rich materials coated with lithium compounds prepared in this invention have significantly improved cycle stability and initial coulombic efficiency compared with uncoated lithium-rich materials and lithium-rich materials coated by other coating methods.
[0037] The present invention has been described in detail above; however, the above embodiments are merely illustrative in nature and are not intended to limit the invention. Furthermore, this document is not limited to the foregoing prior art or the invention itself, or to any theory described in the following embodiments. Attached Figure Description
[0038] Figure 1 This is a schematic diagram of a high-temperature coating machine. Detailed Implementation
[0039] The present invention will be further described below with reference to the embodiments. It should be noted that the following embodiments are provided for illustrative purposes only and do not constitute a limitation on the scope of protection of the present invention.
[0040] Unless otherwise specified, the raw materials, reagents, and methods used in the embodiments are all conventional raw materials, reagents, and methods in the art.
[0041] Lithium-rich manganese-based cathode material Li was obtained using conventional co-precipitation and high-temperature lithiation. 1.2 Mn 0.54 Ni 0.13 Co 0.13 O2.
[0042] Lithium molybdate, lithium tungstate, and lithium borate were purchased commercially.
[0043] The lithium-containing compounds in the examples include lithium molybdate, lithium tungstate, and lithium borate, etc., and the melting points of each lithium-containing compound are shown in Table 1:
[0044] Table 1 Melting points of lithium-containing compounds
[0045] lithium compounds Melting point / °C Lithium molybdate 705 Lithium tungstate 742 Lithium borate 760
[0046] Example 1
[0047] 3g of lithium molybdate and 100g of lithium-rich manganese-based cathode material Li 1.2 Mn 0.54 Ni 0.13 Co 0.13 O2 is premixed evenly in a high-temperature coating machine at a speed of 800 rpm, and then stirred at a speed of 1500 rpm. At the same time, the temperature is raised to 705°C in an air atmosphere at a heating rate of 5°C / min and then stirred and kept at this temperature for 5 hours to obtain lithium-rich manganese-based cathode material coated with lithium molybdate.
[0048] Example 2
[0049] 3g of lithium tungstate and 100g of lithium-rich manganese-based cathode material Li 1.2 Mn 0.54 Ni 0.13 Co 0.13 O2 is premixed evenly in a high-temperature coating machine at a speed of 800 rpm, and then stirred at a speed of 1500 rpm. Simultaneously, the temperature is increased to 742°C in an air atmosphere at a heating rate of 5°C / min, and then stirred and kept at this temperature for 5 hours to obtain lithium-rich manganese-based cathode material coated with lithium tungstate.
[0050] Example 3
[0051] 3g of lithium borate and 100g of lithium-rich manganese-based cathode material Li 1.2 Mn 0.54 Ni 0.13 Co 0.13 O2 is premixed evenly in a high-temperature coating machine at a speed of 800 rpm, and then stirred at a speed of 1500 rpm. At the same time, the temperature is raised to 760°C in an air atmosphere at a heating rate of 5°C / min and then stirred and kept at this temperature for 5 hours to obtain lithium borate-coated lithium-rich manganese-based cathode material.
[0052] Example 4
[0053] 5g of lithium molybdate and 100g of lithium-rich manganese-based cathode material Li 1.2 Mn 0.54 Ni 0.13 Co 0.13O2 is premixed evenly in a high-temperature coating machine at a speed of 800 rpm, and then stirred at a speed of 1500 rpm. At the same time, the temperature is raised to 705°C in an air atmosphere at a heating rate of 5°C / min and then stirred and kept at this temperature for 5 hours to obtain lithium-rich manganese-based cathode material coated with lithium molybdate.
[0054] Example 5
[0055] Step 1: Mix 3g of lithium molybdate and 100g of lithium-rich manganese-based cathode material Li 1.2 Mn 0.54 Ni 0.13 Co 0.13 O2 is premixed evenly in a high-temperature coating machine at a speed of 800 rpm, and then stirred at a speed of 1500 rpm. At the same time, it is heated to 705°C in an air atmosphere at a heating rate of 5°C / min and then stirred and kept at the temperature for 5 hours.
[0056] Step 2: Add 3g of lithium tungstate to the high-temperature coating machine, premix it evenly at 800rpm, and then stir it at 1500rpm. At the same time, heat it to 742℃ in air at a heating rate of 5℃ / min and keep stirring and holding it at that temperature for 8 hours.
[0057] Example 6
[0058] Step 1: Mix 3g of lithium molybdate and 100g of lithium-rich manganese-based cathode material Li 1.2 Mn 0.54 Ni 0.13 Co 0.13 O2 is premixed evenly in a high-temperature coating machine at a speed of 800 rpm, and then stirred at a speed of 1500 rpm. At the same time, it is heated to 705°C in an air atmosphere at a heating rate of 5°C / min and then stirred and kept at the temperature for 5 hours.
[0059] Step 2: Add 3g of lithium borate to the high-temperature coating machine, premix it evenly at 800rpm, and then stir it at 1500rpm. At the same time, heat it to 760℃ in air at a heating rate of 5℃ / min and keep stirring and heat for 8 hours.
[0060] Example 7
[0061] Step 1: Mix 3g of lithium tungstate and 100g of lithium-rich manganese-based cathode material Li 1.2 Mn 0.54 Ni 0.13 Co 0.13 O2 is premixed evenly in a high-temperature coating machine at a speed of 800 rpm, and then stirred at a speed of 1500 rpm. At the same time, it is heated to 742°C in an air atmosphere at a heating rate of 5°C / min and then stirred and kept at the temperature for 5 hours.
[0062] Step 2: Add 3g of lithium borate to the high-temperature coating machine, premix it evenly at 800rpm, and then stir it at 1500rpm. At the same time, heat it to 760℃ in air at a heating rate of 5℃ / min and keep stirring and heat for 8 hours.
[0063] Example 8
[0064] Step 1: Mix 5g of lithium molybdate and 100g of lithium-rich manganese-based cathode material Li 1.2 Mn 0.54 Ni 0.13 Co 0.13 O2 is premixed evenly in a high-temperature coating machine at a speed of 800 rpm, and then stirred at a speed of 1500 rpm. At the same time, it is heated to 705°C in an air atmosphere at a heating rate of 5°C / min and then stirred and kept at the temperature for 5 hours.
[0065] Step 2: Add 5g of lithium borate to the high-temperature coating machine, premix it evenly at 800rpm, and then stir it at 1500rpm. At the same time, heat it to 760℃ in air at a heating rate of 5℃ / min and keep stirring and heat for 8 hours.
[0066] Example 9
[0067] Step 1: Mix 3g of lithium molybdate and 100g of lithium-rich manganese-based cathode material Li 1.2 Mn 0.54 Ni 0.13 Co 0.13 O2 is premixed evenly in a high-temperature coating machine at a speed of 800 rpm, and then stirred at a speed of 1500 rpm. At the same time, it is heated to 705°C in an air atmosphere at a heating rate of 5°C / min and then stirred and kept at the temperature for 5 hours.
[0068] Step 2: Add 3g of lithium tungstate to the high-temperature coating machine, premix it evenly at 800rpm, and then stir it at 1500rpm. At the same time, heat it to 742℃ in air at a heating rate of 5℃ / min and keep stirring and holding it at that temperature for 8 hours.
[0069] Step 3: Add 3g of lithium borate to the high-temperature coating machine, premix it evenly at 800rpm, and then stir it at 1500rpm. At the same time, heat it to 760℃ in air at a heating rate of 5℃ / min and keep stirring and heat for 8 hours.
[0070] To better illustrate the effects of this invention, the lithium-rich manganese-based cathode material Li, which has not undergone any treatment, is used. 1.2 Mn 0.54 Ni0.13 Co 0.13 O2 was used as comparative example 1.
[0071] Comparative Example 2
[0072] 3g of lithium molybdate, 3g of lithium borate, and 100g of lithium-rich manganese-based cathode material Li 1.2 Mn 0.54 Ni 0.13 Co 0.13 O2 is premixed at 800 rpm in a high-temperature coating machine, then mixed evenly at 1500 rpm, and finally heated to 500°C in an air atmosphere at a heating rate of 5°C / min and held for 5 hours to obtain lithium-rich manganese-based cathode material coated with lithium-containing compounds by the traditional solid-phase method.
[0073] Comparative Example 3
[0074] 3g of lithium molybdate was added to a high-temperature coating machine and heated to 705°C at a rate of 5°C / min in air, then stirred and held at this temperature for 2 hours. Next, 3g of lithium borate was added and premixed at 800 rpm until homogeneous. Then, the mixture was stirred at 1500 rpm and heated to 760°C at a rate of 5°C / min in air, then stirred and held at this temperature for 2 hours. Finally, 100g of lithium-rich manganese-based cathode material Li was added. 1.2 Mn 0.54 Ni 0.13 Co 0.13 O2 was premixed at 800 rpm and then stirred at 1500 rpm for 8 hours to obtain the coated lithium-rich manganese-based cathode material.
[0075] Table 2 lists the first cycle discharge specific capacity and coulombic efficiency of coin cells (with lithium anode) made of lithium-rich manganese-based cathode materials in Examples 1-9 and Comparative Examples 1, 2, and 3 at room temperature, 2-4.8V, and 0.1C (1C = 250mAh / g) current density, as well as the 200-cycle capacity retention at room temperature, 2-4.8V, and 1C (1C = 250mAh / g) current density.
[0076] Table 2 Comparison of Initial Charge and Discharge Performance
[0077]
[0078] As can be seen from the data in the table, the lithium-rich manganese-based cathode material coated with lithium molybdate / lithium borate obtained by the stepwise coating method of this invention can achieve an initial discharge specific capacity of 268.33 mAh / g, which is significantly higher than that of the uncoated lithium-rich manganese-based cathode material (250.54 mAh / g), the lithium-rich manganese-based cathode material coated by the traditional solid-state method (254.32 mAh / g), and the lithium-rich manganese-based cathode material coated by first melting lithium molybdate and lithium borate (258.78 mAh / g). At the same time, the initial coulombic efficiency can reach more than 87%, while the initial coulombic efficiency of the uncoated lithium-rich manganese-based cathode material is only 73.21%.
[0079] As can be seen from the data in the table, the capacity retention rate of the coated lithium-rich manganese-based cathode material prepared by the present invention can reach more than 85% after 200 cycles, with a maximum of 88.93%, which is higher than that of the uncoated lithium-rich manganese-based cathode material and the lithium-rich manganese-based cathode material coated by the traditional solid-state method.
[0080] The above embodiments are merely illustrative of the technical solutions of the present invention and are not intended to limit it. Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features therein, without departing from the spirit and substance defined by the claims of the present invention; and such modifications or substitutions are still within the scope defined by the claims of the present invention.
Claims
1. A method for preparing a lithium-rich manganese-based cathode material coated with a lithium-containing compound, characterized in that, The method includes the following steps: S1: After the first lithium-containing compound and the lithium-rich manganese-based cathode material are stirred evenly in a high-temperature coating machine, the temperature is raised to the melting point temperature t1 of the first lithium-containing compound under an air atmosphere for high-temperature melting. After stirring and keeping warm for a period of time, the heating is stopped to obtain the first lithium-containing compound coated with the lithium-rich manganese-based cathode material. The mass of the lithium-containing compound is 0.1%-10% of the mass of the lithium-rich manganese-based cathode material; The lithium-containing compound is selected from at least one of lithium zirconate, lithium vanadate, lithium borate, lithium molybdate, lithium tungstate, and lithium phosphate.
2. The preparation method according to claim 1, characterized in that, The method further includes the following steps: S2: Add a second lithium-containing compound to the first lithium-containing compound coating lithium-rich manganese-based cathode material, stir evenly in a high-temperature coating machine, heat to the melting point temperature t2 of the second lithium-containing compound in an air atmosphere, keep stirring and heat for a period of time, and then stop heating to obtain the first and second lithium-containing compound composite coating lithium-rich manganese-based cathode material. Similarly, the Nth lithium-containing compound is added, and after being stirred evenly in a high-temperature coating machine, it is heated to the melting point t of the Nth lithium-containing compound under an air atmosphere. N After stirring and keeping warm for a period of time, heating is stopped, and the mixture is cooled to room temperature to obtain a lithium-containing compound composite coated lithium-rich manganese-based cathode material, where N=3,4,5,6.
3. The preparation method according to claim 1, characterized in that, The method includes the following steps: S1: The first lithium-containing compound and the lithium-rich manganese-based cathode material are first stirred and premixed evenly in a high-temperature coating machine at a speed of 800-1000 rpm, and then coated and fused at a speed of 1500-1600 rpm. At the same time, the temperature of the coating chamber is heated to the melting point temperature t1 of the first lithium-containing compound at a heating rate of 5℃ / min. Stirring and heat preservation are maintained for 5-6 hours to obtain the first lithium-containing compound coated with lithium-rich manganese-based cathode material. S2: Based on step S1, add a second lithium-containing compound, mix evenly, and continue to stir and premix evenly at a speed of 800-1000 rpm. Then, coat and fuse at a speed of 1500-1600 rpm. At the same time, heat the coating chamber temperature to the melting point temperature t2 of the second lithium-containing compound at a heating rate of 5℃ / min. Keep stirring and holding at the temperature for 8-10 hours, then stop stirring and cool to room temperature to obtain the first and second lithium-containing compound composite coated lithium-rich manganese-based cathode material.
4. A lithium-containing compound-coated lithium-rich manganese-based cathode material, characterized in that, Prepared by the preparation method according to any one of claims 1-3, comprising a lithium-rich manganese-based cathode material and at least one layer of uniformly distributed lithium-containing compound coating.
5. The application of the lithium-containing compound-coated lithium-rich manganese-based cathode material as described in claim 4 in the preparation of a lithium-ion battery cathode.
Citation Information
Patent Citations
A preparation method of lithium vanadate coated lithium-rich oxide solid solution material
CN109103423A
Lithium molybdate coated lithium-rich manganese-based positive electrode material as well as preparation method and application thereof
CN113078316A
Coating modification method of lithium-rich manganese-based positive electrode material
CN111740085A
Lithium ion battery electrode material and preparation method therefor
WO2021109965A1