A laser sealing welding method and system
By constructing a laser power-oscillation amplitude-fitted axis speed curve and implementing closed-loop control, the problems of weld consistency and low efficiency in metal bipolar plate welding were solved, achieving efficient two-dimensional planar welding of thin metal plates. In particular, the weld width and penetration depth were consistent in both straight and non-straight paths, thus improving welding efficiency.
Patent Information
- Application Number
- CN202410272517.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-11
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2044-03-11
AI Technical Summary
Existing laser welding technology suffers from poor weld consistency and low efficiency in metal bipolar plate sealing welding. In particular, the weld width and penetration depth are inconsistent on straight and non-straight paths, and weld overlap and heat accumulation at corners can easily lead to poor welding.
By constructing a laser power-oscillation amplitude-fitted shaft speed curve, the fitted shaft speed is monitored in real time, and the laser power and oscillation amplitude are quickly adjusted to achieve stable welding of welds with different geometric paths. The laser generation module, welding head and motion module are synchronously controlled by a closed-loop connection.
It achieves consistent welding results for different geometric paths on a two-dimensional plane of thin metal sheets, improves welding efficiency by more than 50%, avoids weld overlap and heat accumulation at corner welds, and meets the needs of mass production.
Smart Images

Figure CN118204628B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of laser welding, and more particularly to a highly efficient and reliable method for sealing and welding metal bipolar plates, specifically a laser sealing and welding method and system. Background Technology
[0002] Metal bipolar plates, as one of the core components of fuel cells, play a role in distributing reactant gases, collecting current, and supporting electrode materials. They form the skeleton of the entire fuel cell stack and account for approximately 30% of the total cost. Metal bipolar plates are mainly composed of anode and cathode metal plates made of stainless steel or titanium alloy, with a thickness ranging from 0.05 to 0.15 mm. The anode and cathode metal plates are arranged in flow channels with different geometric paths (…). Figure 1 To prevent the reaction gas and coolant from mixing or even leaking, a sealing weld is performed.
[0003] Metal bipolar plates are relatively large (length × width = 450 × 150 mm), and there are currently two technical approaches for their sealing welding: high-speed laser scanning sealing welding and laser oscillating sealing welding. High-speed laser scanning welding uses a field lens with a large focal length to achieve sealing welding of large-sized bipolar plates, resulting in high welding efficiency. However, this welding method cannot provide inert gas protection for the weld, resulting in a yellowish weld with weld slag, and a low yield rate in the critical airtightness test. In contrast, laser oscillating sealing welding can integrate a coaxial gas nozzle directly below the high-speed scanning component, resulting in a white and smooth weld with a high pass rate in airtightness tests.
[0004] In current laser oscillating welding sealing welding, the bipolar plate welding channel is divided into multiple small segments for welding. To achieve better consistency, a section of idle lead wire needs to be added before and after welding so that the motion axis reaches the set welding speed before laser welding. Furthermore, two segments are used at the corners to achieve a sealing effect. Figure 2 This method avoids the increase in overlap and heat accumulation in the oscillating weld due to the reduced shaft speed at corner welds, which can lead to weld widening and burn-through defects, resulting in poor overall weld consistency and failure to pass the airtightness test. However, this method of welding after the moving shaft reaches speed means that the idle time of the moving shaft accounts for more than 50% of the total welding process time, resulting in welding efficiency that is 4 to 5 times lower than that of the laser high-speed scanning method. Summary of the Invention
[0005] The purpose of this invention is to address the problems existing in the prior art by providing a laser sealing welding method and system. By rapidly adapting the laser power and oscillation amplitude to the motion axis speed, the problem of consistency in weld width and penetration depth for both straight and non-straight paths is solved.
[0006] According to one aspect of the present invention, a laser sealing welding method is provided for laser sealing welding of ultrathin metal bipolar plates, the method comprising:
[0007] Confirm the power output linearity and welding focus of the laser welding system;
[0008] The fitted shaft speed is acquired in real time during the welding process;
[0009] Based on the fitted shaft speed, combined with the current weld path and the pre-constructed laser power-oscillation amplitude-fitted shaft speed curve, the laser power and oscillation amplitude corresponding to the current fitted shaft speed are determined.
[0010] A laser beam is generated based on a determined laser power and transmitted to the welding head, which then performs motion welding according to a set welding trajectory, oscillation mode, and determined oscillation amplitude.
[0011] The above technical solution constructs a laser power-oscillation amplitude-fitted axis speed curve, which enables rapid adjustment of laser power and oscillation amplitude when the speed of the moving axis changes, thereby achieving smooth and rapid welding of weld paths with different geometric paths and ensuring the consistency of welding effect for different geometric paths on the two-dimensional plane of thin metal plates.
[0012] As a further technical solution, the pre-construction of the laser power-oscillation amplitude-fitted axial velocity curve includes:
[0013] Under a straight weld path, the laser power and oscillation amplitude corresponding to different fitted axis speeds are measured for the same weld width and penetration depth, forming a laser power-oscillation amplitude-fitted axis speed curve;
[0014] Under non-linear weld seam paths, the fitted axis speed corresponding to different non-linear weld seams is measured. Based on the fitted axis speed and the laser power-oscillation amplitude-fitted axis speed curve, the laser power and oscillation amplitude corresponding to the current non-linear weld seam are determined.
[0015] As a further technical solution, the straight weld seam includes straight weld seams of different lengths; the non-straight weld seam includes corner weld seams of different sizes.
[0016] As a further technical solution, after forming the laser power-oscillation amplitude-fitted axis speed curve, the method further includes: determining the initial fitted axis speed; and based on the laser power and oscillation amplitude corresponding to the initial fitted axis speed, determining the correction coefficients of the laser power and oscillation amplitude of each fitted axis speed relative to the laser power and oscillation amplitude of the initial fitted axis speed.
[0017] As a further technical solution, the real-time acquisition of the fitted axis speed during the welding process also includes: dividing the motion trajectory into multiple small line segments, performing vector fitting on the two sets of monitored X-axis speed and Y-axis speed according to the Pythagorean theorem to obtain the fitted axis speed of each small segment, and obtaining the fitted axis speed of the motion trajectory based on the fitted axis speed of each small segment, which is used as the fitted axis speed of the current weld path.
[0018] As a further technical solution, the method also includes: enabling closed-loop communication between the laser, welding head, and motion axis via a circuit board.
[0019] According to one aspect of the present invention, a laser sealing welding system is provided, comprising: a laser generating module for generating a laser beam; a laser optics module for transmitting, oscillating, focusing, and real-time imaging of the welding area of the laser beam; a motion module for driving a motion axis to perform precise and rapid welding according to a preset trajectory; and a control module for real-time control of laser output power, fitting speed control, and monitoring of the fitting axis speed of the motion module, determining the laser power of the laser generating module and the oscillation amplitude of the laser optics module based on the fitting axis speed, and controlling the welding head to perform high-speed welding according to a set welding trajectory and oscillation mode.
[0020] The above technical solution establishes a closed-loop communication between the laser generation module, the welding head of the laser optics module, and the motion axis of the motion module, achieving millisecond-level synchronous control of laser welding power, oscillation amplitude, and axis speed. For sealing welding of bipolar plate flow channels with complex geometries, by monitoring and fitting the axis speed and rapidly adjusting the laser welding power and oscillation amplitude in synergy, it achieves stable and rapid welding of both straight and non-straight weld seams. This eliminates the need for inefficient welding procedures involving idle acceleration, reaching speed and switching on the laser, welding completion and switching off the laser, and deceleration. Furthermore, it avoids weld overlap and heat accumulation at corner weld seams due to reduced axis speed, which can lead to welding defects.
[0021] As a further technical solution, the control module includes a laser control unit, a swing control unit, a motion control unit, and a fitted axis speed monitoring unit. The fitted axis speed monitoring unit is used to monitor the fitted axis speed of the motion axis and send the monitored fitted axis speed to the laser control unit and the swing control unit. The laser control unit is used to determine the appropriate laser power based on the fitted axis speed and send it to the laser generating module. The swing control unit is used to determine the appropriate swing amplitude based on the fitted axis speed and send it to the welding head. The motion control unit is used to control the movement of the welding head according to the set welding trajectory and swing mode.
[0022] As a further technical solution, both the laser control unit and the swing control unit store a pre-constructed laser power-swing amplitude-fitted axis speed curve.
[0023] As a further technical solution, the fitted axis speed monitoring unit includes an X-axis encoder, a Y-axis encoder, and a fitter. The fitter is used to fit the X-axis and Y-axis motion speeds obtained by the X-axis encoder and the Y-axis encoder to obtain the fitted axis speed.
[0024] Compared with the prior art, the beneficial effects of the present invention are:
[0025] This invention constructs a laser power-oscillation amplitude-fitted shaft speed curve and monitors the fitted shaft speed in real time during the welding process. This allows for rapid adjustment of laser power and oscillation amplitude in response to changes in the shaft speed, enabling stable welding of welds along different paths. This solves the problem of consistent welding results for ultra-thin (thickness less than 0.15mm) metal sheets with different geometric shapes on a two-dimensional plane, and in particular, it solves the problem of consistent weld width and penetration depth for straight and non-straight welding paths.
[0026] This invention eliminates the need for an inefficient welding process involving idling, speed-up, speed-up, welding completion, and speed-down. It avoids the problem of increased weld overlap and heat accumulation at corner welds due to reduced shaft speed, which can lead to poor welding. While meeting the requirements for mass production, the welding efficiency is increased by more than 50% compared to existing processing methods. Attached Figure Description
[0027] Figure 1 This is a schematic diagram of the welding trajectory of an existing metal bipolar plate;
[0028] Figure 2 This is a schematic diagram of the welding path and corner welding before and after optimization according to an embodiment of the present invention;
[0029] Figure 3 This is a schematic diagram of welding trajectory optimization according to an embodiment of the present invention;
[0030] Figure 4 This is a schematic diagram illustrating the welding effect of straight lines and corners according to an embodiment of the present invention.
[0031] Figure 5 This is a schematic diagram of the welding trajectory according to an embodiment of the present invention.
[0032] Figure 6 This is a schematic diagram illustrating laser power-oscillation amplitude adaptation according to an embodiment of the present invention.
[0033] Figure 7 This is a schematic diagram of the system structure according to an embodiment of the present invention.
[0034] Figure 8 This is a schematic diagram of closed-loop communication according to an embodiment of the present invention.
[0035] Figure 9This is a schematic diagram of the laser power-oscillation amplitude-fitted shaft speed curve according to an embodiment of the present invention.
[0036] In the diagram: 1. Laser; 2. Transmission fiber; 3. Fiber optic connector; 4. Collimating lens; 5. 45° folding mirror; 6. Scanning galvanometer; 7. 45° folding mirror; 8. CCD module; 9. Focusing lens; 10. Illumination source; 11. Coaxial nozzle; 12. Workpiece to be welded; 13. Motion module; 14. Industrial computer; 15. Fitting axis speed monitoring; 16. Swing control; 17. Laser control; 18. Motion control. Detailed Implementation
[0037] To address the limitations of inert gas protection for weld seams in bipolar plate sealing welding, and the low welding efficiency caused by idle movement of the motion axis, this invention provides a laser sealing welding method. This method establishes a closed-loop communication connection between the laser, scanning galvanometer, and motion axis, achieving millisecond-level synchronous control of welding power, oscillation amplitude, and axis speed. Furthermore, for sealing welding of bipolar plate flow channels with complex geometries, this method optimizes corner running speed and coordinates various methods to rapidly adjust welding power and oscillation amplitude, achieving smooth and rapid welding of both straight and corner weld seams. This eliminates the need for inefficient welding procedures involving idle movement for speed increase, reaching speed and switching on the laser, welding completion and switching off the laser and decelerating. It also avoids weld seam overlap and heat accumulation at corner weld seams caused by reduced axis speed, thus preventing welding defects.
[0038] The welding method of this invention efficiently achieves consistent welding results for ultra-thin (thickness less than 0.15mm) metal sheets with different geometric paths in a two-dimensional plane. In particular, it solves the problem of consistent weld width and penetration depth for straight and corner paths. While meeting the requirements of mass production, the welding efficiency is increased by more than 50% compared with the original processing method.
[0039] The technical solution of the present invention will now be clearly and completely described with reference to the accompanying drawings. Obviously, the described embodiments are merely some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0040] This invention provides a laser sealing welding method for ultrathin metal bipolar plates, comprising:
[0041] Step 1: Confirm the power output linearity and welding focus of the laser welding system;
[0042] Step 2: Obtain the fitted shaft speed in real time during the welding process;
[0043] Step 3: Based on the fitted shaft speed, combined with the current weld path and the pre-constructed laser power-oscillation amplitude-fitted shaft speed curve, determine the laser power and oscillation amplitude corresponding to the current fitted shaft speed;
[0044] Step 4: A laser beam is generated according to the determined laser power and transmitted to the welding head. The welding head performs high-speed welding according to the set welding trajectory, oscillation mode, and determined oscillation amplitude. The welding head is an oscillating welding head with a coaxial air nozzle.
[0045] Furthermore, a protective gas, including but not limited to inert gases such as nitrogen and argon, can be introduced during the welding process.
[0046] Before welding begins, the following is also included:
[0047] Step 1.1: Assemble the anode metal plate and cathode metal plate by overlapping them and placing them horizontally on the contour pressing fixture. Make the upper and lower areas to be welded of the anode metal plate and cathode metal plate fit together and ensure that the surface of the workpiece is flat. Then fix the contour fixture containing the metal bipolar plate sample on the welding platform.
[0048] Step 1.2: Install the coaxial nozzle, adjust the optical path system and the origin correction function of the welding software to ensure that the laser beam is in the exact center of the coaxial nozzle; at the same time, confirm that the actual size of the laser beam oscillation circle differs from the set size by less than 0.02mm.
[0049] Step 1.3: Connect the laser, scanning galvanometer, and motion axis to a closed-loop communication circuit via a board. Use the power correction function of the laser control software to ensure the linearity of the laser power output. The laser, scanning galvanometer, and motion axis communicate in a closed loop and exchange signals via an industrial control computer.
[0050] Step 1.4: Under the straight weld path, measure the laser power and oscillation amplitude corresponding to different fitting axis speeds under the same welding width and penetration depth, and establish the laser power-oscillation amplitude-fitting axis speed curve (Table 1).
[0051] Table 1. Laser Power - Oscillation Amplitude - Fitted Axis Velocity Table
[0052]
[0053] Fitted axis speed refers to the real-time motion speed of the X and Y axes monitored by the encoders of the X and Y axes respectively under a specified weld seam trajectory. The fitted axis speed of the XY dual-axis motion is obtained by fitting the monitored speed values. It should be noted that the measurement operation interface has only one fitted axis speed input field. By inputting different fitted axis speeds, different laser power and oscillation amplitude can be measured under the same line width and weld depth requirements.
[0054] Furthermore, the fitted axial velocity of straight welds remains constant within the same straight segment. The fitted axial velocity of corner welds is related to the number of chamfers.
[0055] Specifically, if a corner weld has only one chamfer, there will be only one fitted axis speed. However, if there is a welding trajectory like an S-shaped curve, there will be multiple fitted axis speeds, requiring multiple measurements of the corresponding laser power and oscillation amplitude.
[0056] like Figure 5 As shown, the welding trajectory includes straight weld segments and corner welds. The corner welds have only one chamfer, and the dimensions of all four corners are identical. Therefore, the fitted axial velocity of the straight weld remains constant within the same straight segment, and the fitted axial velocity of the corner weld remains constant within the same corner. The correspondence between the laser power and the oscillation amplitude of this welding trajectory is as follows: Figure 6 As shown.
[0057] Furthermore, when multiple corner dimensions exist, there will be a single straight line and multiple corner power and amplitude values, meaning the correspondence between laser power and swing amplitude at the corner is no longer as... Figure 6 As shown, the relationship between laser power and oscillation amplitude is not determined by the change in corner size, but by the variation in corner size.
[0058] Optionally, the straight section weld can be compatible with line segments of different lengths.
[0059] Step 1.5: Under the corner weld path, measure the corresponding fitted axial speed at different corners. Use the fitted axial speed measured at this corner as a reference, input and optimize the laser power and oscillation amplitude. In actual welding, use the optimized laser power and oscillation amplitude to weld, so that the line width and penetration depth of the corner weld are consistent with those of the straight weld.
[0060] Optionally, the corner weld can be in the form of rounded corners, obtuse corners, right angles or acute angles of different sizes.
[0061] During mass production, the motion axis encoder feeds back the fitted shaft speed of the corner weld to the control module in real time. After receiving the fitted shaft speed signal, the control module quickly changes the laser power and swing amplitude according to the adaptive curve function, ultimately achieving the effect that the width and penetration depth of the corner weld are consistent with those of the straight weld.
[0062] Furthermore, the motion trajectory is divided into multiple small line segments. The X and Y axis velocities detected by the encoder are vector-fitted using the Pythagorean theorem to obtain the fitted axis velocity for each small segment, thus obtaining the fitted axis velocity of the motion trajectory, which serves as the fitted axis velocity for the entire corner weld. Specifically, after moving from the straight section of the weld to the corner weld, a motion trajectory is formed. This trajectory is divided into small line segments and then fitted to obtain the fitted axis velocity for the entire corner weld.
[0063] Optionally, after forming the laser power-oscillation amplitude-fitted shaft speed curve, the method further includes: determining an initial fitted shaft speed; and, based on the laser power and oscillation amplitude corresponding to the initial fitted shaft speed, determining a correction coefficient for the laser power and oscillation amplitude of each fitted shaft speed relative to the laser power and oscillation amplitude of the initial fitted shaft speed. Using correction coefficients facilitates rapid adjustment of different laser powers and oscillation amplitudes during the welding process, which improves work efficiency compared to directly inputting specific laser power and oscillation amplitudes.
[0064] Taking the welding of straight welds and R2 chamfers as an example, as shown in Table 2 and... Figure 4 As shown in (a)-(d), Figure 4 (a) is an enlarged view of the weld effect on the straight section. Figure 4 (b) is an enlarged view of a cross-section of the weld seam on the straight section. Figure 4 (c) is a magnified view of the R2 chamfer weld effect. Figure 4 (d) is an enlarged cross-section of the R2 chamfer weld. As can be seen from the figure, the width and penetration depth of the straight weld and the R2 chamfer weld are very similar, which can be considered as achieving the effect of consistent width and penetration depth between the corner weld and the straight weld.
[0065] Table 2 Welding parameters for straight lines and corners
[0066] Weld type Weld width dimensions Slice Melting Depth Welding shaft speed Welding power Welding swing amplitude Straight weld 0.200mm 0.081mm 200mm / s 90.4W 0.181mm Corner (R2) weld 0.201mm 0.081mm 90mm / s 51.2W 0.114mm
[0067] Based on the same inventive concept as the aforementioned method, the present invention also provides a laser sealing welding system, comprising: a laser generating module for generating a laser beam; a laser optics module for transmitting, oscillating, focusing, and real-time imaging of the welding area of the laser beam; a motion module for driving a motion axis to perform precise and rapid welding according to a preset trajectory; and a control module for real-time control of laser output power, fitting speed control, and monitoring of the fitting axis speed of the motion module, determining the laser power of the laser generating module and the oscillation amplitude of the laser optics module based on the fitting axis speed, and controlling the welding head to perform high-speed welding according to the set welding trajectory and oscillation mode.
[0068] The laser generating module outputs a continuous laser beam in the 1060–1090 nm wavelength range. The laser's output power ranges from 0 to 500 W. The laser's transmission fiber core diameter is less than 25 μm, resulting in a high-quality output laser beam. 2 With a value less than 1.2, the laser beam is output after passing through the X and Y double-swing mirrors to perform welding, which increases the interaction time and width between the laser and the sample, effectively increases the weld fusion area, and improves the welding sealing effect.
[0069] The control module comprises a control board integrating laser control, oscillation control, and motion control interfaces. It includes motion axis fitting speed monitoring, laser power control, oscillation control, and motion control functions. Based on different weld geometry paths, the control module uses the fitting speed monitoring function to report different fitting speeds for different geometric paths. Then, through the laser control and oscillation control functions, it adapts different laser powers and oscillation amplitudes to the geometric paths under different fitting speeds, thereby ensuring consistent welding results for different geometric paths. The control module's transmission synchronization time is in the millisecond range, guaranteeing both welding accuracy and welding quality.
[0070] The motion module includes a linear module that directly converts electrical energy into linear motion mechanical energy. It can be two-dimensional or three-dimensional and has advantages such as high transmission stiffness, fast dynamic response, high motion resolution, and high positioning accuracy.
[0071] The laser optical template includes a transmission fiber, a fiber optic connector, a collimating lens, a 45° folding mirror, a CCD assembly, a scanning galvanometer, and an F-θ field lens. The laser beam generated by the laser is output to the collimating lens through the transmission fiber. The collimating lens and the transmission fiber are connected through the fiber optic connector, which is either a QBH or D80 connector. The collimating lens shapes the diverging laser beam into a parallel laser beam. After passing through the 45° folding mirror, the parallel laser beam enters the scanning galvanometer, which deflects the laser beam to the F-θ field lens. The F-θ field lens focuses the laser beam onto the surface of the workpiece for welding. The CCD assembly enables real-time monitoring of the welding process.
[0072] Furthermore, the focal length range of the collimating lens is 50–100 mm;
[0073] Furthermore, the focal length range of the F-θ field lens is 100–210 mm.
[0074] Furthermore, the scanning galvanometer enables high-speed, high-precision laser welding of small weld widths (<0.25mm) by setting an oscillation pattern, with an oscillation speed range of 1000–5000 mm / s.
[0075] The swing control function adapts different swing amplitudes to the geometric path under different fitted shaft speeds, and sends the adapted swing amplitude to the scanning galvanometer so that it swings according to the adapted swing amplitude.
[0076] As one implementation method, taking the welding of a 0.1mm thick electrode plate to another 0.1mm thick electrode plate as an example, the material is 316L stainless steel, the welding area is a rectangle of 400×150mm, and the welding is performed in two stages. The lower layer is required to have a penetration depth of 0.08±0.01mm, a weld width of less than 0.25mm, and good consistency in the overall weld surface, penetration depth, and back mark. The welding time should be less than 50 seconds per piece. A 1064nm fiber single-mode laser (M...) is used. 2 <1.1), the linear oscillation amplitude is 0.19mm, the oscillation speed is 3000mm / s, the axis movement speed is 200mm / s, the welding power is set to 100W, and the correction coefficients for the laser power and oscillation amplitude under different fitted axis speeds are input. Welding is performed according to the preset path. The welding effect is as follows: the lower layer penetration is 0.082mm, the weld width is 0.21mm, the welding efficiency is 40 seconds / piece, and the weld surface, penetration, and back mark are consistent, meeting the welding requirements.
[0077] Example 1 uses the welding of a 0.08mm thick electrode plate to another 0.08mm thick electrode plate as an example. The material is 316L stainless steel, and the welding area is a rectangle of 350×100mm. Welding is performed in two stages, requiring a penetration depth of 0.06±0.01mm for the lower layer, a weld width of less than 0.2mm, good consistency in overall weld surface, penetration depth, and back marks, and a welding time of less than 45 seconds per piece. A 1064nm fiber single-mode laser (M...) is used. 2 <1.1), the linear oscillation amplitude is 0.17mm, the oscillation speed is 2500mm / s, the axis movement speed is 210mm / s, the welding power is set to 90W, and the correction coefficients for the laser power and oscillation amplitude under different fitted axis speeds are input. Welding is performed according to the preset path. The welding effect is as follows: the lower layer penetration is 0.058mm, the weld width is 0.19mm, the welding efficiency is 37 seconds / piece, and the weld surface, penetration, and back mark are consistent, meeting the welding requirements.
[0078] Although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and alterations can be made to these embodiments without departing from the principles and spirit of the invention, the scope of which is defined by the appended claims and their equivalents.
Claims
1. A laser sealing welding method, characterized in that, Laser sealing welding of ultrathin metal bipolar plates, the method does not require running the welding procedure according to the welding pattern of idle run speed increase, reaching speed and turning on the light, welding completion and turning off the light and decelerating, including: Confirm the power output linearity and welding focus of the laser welding system; The fitted shaft speed is acquired in real time during the welding process; Based on the fitted axial speed, combined with the current weld path and the pre-constructed laser power-oscillation amplitude-fitted axial speed curve, the laser power and oscillation amplitude corresponding to the current fitted axial speed are determined. The pre-construction of the laser power-oscillation amplitude-fitted axial speed curve includes: under a straight weld path, measuring the laser power and oscillation amplitude corresponding to different fitted axial speeds for the same weld width and penetration depth, forming a laser power-oscillation amplitude-fitted axial speed curve; under a non-straight weld path, measuring the fitted axial speed corresponding to different non-straight welds, and based on the fitted axial speed combined with the laser power-oscillation amplitude-fitted axial speed curve, determining the laser power and oscillation amplitude corresponding to the current non-straight weld, satisfying the consistency requirements of welding width and depth for straight and non-straight welds. A laser beam is generated based on a determined laser power and transmitted to the welding head, which then performs motion welding according to a set welding trajectory, oscillation mode, and determined oscillation amplitude.
2. The laser sealing welding method according to claim 1, characterized in that, The straight welds include straight welds of different lengths; the non-straight welds include corner welds of different sizes.
3. The laser sealing welding method according to claim 1, characterized in that, After forming the laser power-oscillation amplitude-fitted axis speed curve, the method further includes: determining the initial fitted axis speed; and, based on the laser power and oscillation amplitude corresponding to the initial fitted axis speed, determining the correction coefficients of the laser power and oscillation amplitude of each fitted axis speed relative to the laser power and oscillation amplitude of the initial fitted axis speed.
4. The laser sealing welding method according to claim 1, characterized in that, The real-time acquisition of the fitted axis speed during the welding process also includes: dividing the motion trajectory into multiple small line segments, performing vector fitting on the two sets of monitored X-axis speed and Y-axis speed according to the Pythagorean theorem to obtain the fitted axis speed of each small segment, and obtaining the fitted axis speed of the motion trajectory based on the fitted axis speed of each small segment, which is used as the fitted axis speed of the current weld path.
5. The laser sealing welding method according to claim 1, characterized in that, The method also includes: enabling closed-loop communication between the laser, welding head, and motion axis via a circuit board.
6. A laser sealing welding system for implementing the laser sealing welding method according to any one of claims 1 to 5, characterized in that, This welding program eliminates the need for inefficient methods like idle acceleration, speed-up activation, welding completion shutdown, and deceleration. It includes: a laser generation module for generating a laser beam; a laser optics module for transmitting, oscillating, focusing, and real-time imaging of the welding area; a motion module for driving the motion axis to perform precise and rapid welding along a preset trajectory; and a control module for real-time control of laser output power, fitting speed control, and monitoring of the fitting axis speed of the motion module. Based on the fitting axis speed, it determines the laser power of the laser generation module and the oscillation amplitude of the laser optics module, and controls the welding head to perform high-speed welding according to the set welding trajectory and oscillation pattern.
7. The laser sealing welding system according to claim 6, characterized in that, The control module includes a laser control unit, a swing control unit, a motion control unit, and a fitted axis speed monitoring unit. The fitted axis speed monitoring unit monitors the fitted axis speed of the motion axis and sends the monitored fitted axis speed to the laser control unit and the swing control unit. The laser control unit determines the appropriate laser power based on the fitted axis speed and sends it to the laser generating module. The swing control unit determines the appropriate swing amplitude based on the fitted axis speed and sends it to the welding head. The motion control unit controls the welding head to perform high-speed welding according to the set welding trajectory and swing mode.
8. The laser sealing welding system according to claim 7, characterized in that, Both the laser control unit and the swing control unit store pre-constructed laser power-swing amplitude-fitted axis speed curves.
9. The laser sealing welding system according to claim 7, characterized in that, The fitted axis speed monitoring unit includes an X-axis encoder, a Y-axis encoder, and a fitter. The fitter is used to fit the X-axis and Y-axis motion speeds obtained by the X-axis encoder and the Y-axis encoder to obtain the fitted axis speed.
Citation Information
Patent Citations
Self-adaptive power control method for laser welding
CN114951990A
Laser welding control method, device and equipment and storage medium
CN116900489A