A localized surface plasmon high entropy alloy and its preparation method and application

By using the carbon thermal shock method to introduce metal elements with localized surface plasmon resonance properties into high-entropy alloys, the response strength and cost problems of existing electrocatalysts are solved, and efficient catalytic performance for alcohol oxidation and PET degradation is achieved.

CN118207590BActive Publication Date: 2024-10-22SUZHOU UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410616012.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-17
Publication Date
2024-10-22
Estimated Expiration
2044-05-17

AI Technical Summary

Technical Problem

Existing localized surface plasmon resonance (LSPR) effect electrocatalysts have problems such as weak surface plasmon response intensity, low energy utilization, limited basic activity, high cost and complicated preparation. It is necessary to develop new ones with An electrocatalyst with strong light responsiveness, high catalytic activity, low cost and simple preparation.

Method used

The carbon thermal shock method is used to introduce metal element components with significant localized surface plasmon resonance properties into high-entropy alloys, adjust the surface electronic structure properties of nanoparticles, and prepare materials with significant localized surface plasmon resonance properties. The specific steps include dropping the mixed precursor salt solution on the carbon paper, applying instantaneous voltage and current for high-temperature treatment, and determining the concentration of the precursor salt, heating time, heating temperature and other conditions.

Benefits of technology

Successfully designed and synthesized a localized surface plasmon high-entropy alloy nanoparticle catalyst with good catalytic performance and enhanced ability. It was used in alcohol oxidation and PET degradation, significantly improving catalytic activity and electrocatalytic performance, and reducing preparation costs. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118207590B_ABST
    Figure CN118207590B_ABST
Patent Text Reader

Abstract

The present invention belongs to the field of high entropy alloys, and specifically relates to a localized surface plasmon high entropy alloy and a preparation method and application thereof. In order to obtain a localized surface plasmon high entropy alloy in which each element is uniformly mixed, the present invention prepares a localized surface plasmon high entropy alloy by adding a metal element having a significant localized surface plasmon resonance property into a precursor solution and using a rapid high-temperature quenching method-carbon thermal shock method. First, a mixed metal salt alcohol solution is dripped onto the surface of carbon paper and dried at room temperature, and then an instantaneous voltage and current are applied to the carbon paper loaded with metal salts so that it can reach 1100°C within 0.5 s, and the required high entropy alloy is obtained by carbon thermal shock.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of high entropy alloys, and in particular relates to a localized surface plasmon high entropy alloy and a preparation method and application thereof. Background Art

[0002] Solar energy is the cleanest and cheapest energy on the earth's surface. Using solar energy to produce chemical fuels and to remediate the environment through solar energy-enhanced catalytic reactions have been considered to be important ways to solve the current global environmental and energy crisis. The localized surface plasmon resonance (LSPR) effect is a unique property of nanomaterials. It can effectively capture solar energy and drive chemical reactions. It plays an important role in catalytic reactions and is one of the most effective ways to achieve light-assisted electrocatalysis. However, the current electrocatalysts with LSPR effect have problems such as weak surface plasmon response intensity, low surface plasmon energy utilization, limited basic activity, high cost and complex preparation. They are still in the early stages of research and application and require more in-depth exploration and research. It is urgent to develop new localized surface plasmon electrocatalysts with strong light response, high surface plasmon capacity utilization, high catalytic activity, low cost and simple preparation method.

[0003] In recent years, high entropy alloys (HEAs) have attracted widespread attention due to their unique physical and chemical properties, and have been applied to different electrocatalytic fields such as ammonia oxidation, water decomposition, methanol oxidation, and CO2 reduction. Compared with traditional bimetallic and trimetallic alloys, the basic advantage of HEAs is that they contain multiple metals and have excellent physical, chemical, surface, and electromagnetic properties, including extraordinary catalytic activity and fairly good stability. In addition, the "cocktail" effect produced by the synergistic action of multiple elements can give high entropy alloys special physical and chemical properties, providing favorable conditions for high entropy alloys to have LSPR effects, and also providing new ideas for solving the problems faced by surface plasmon-based electrocatalysts. Therefore, it is of great significance to prepare high entropy alloys with LSPR properties.

[0004] Previously, multi-metallic nanoparticles were synthesized using traditional reduction methods. However, these synthesis methods often produce phase-separated heterostructures between immiscible elements, which greatly reduces the configurational entropy of mixing. The high-temperature carbon thermal shock (CTS) method is a general method for the controllable and efficient synthesis of high-entropy alloy nanoparticles with single-phase structure and uniform dispersion. In this method, metal precursors are first loaded on a carbon substrate, and then the temperature is instantaneously increased by passing an electric current through the sample for a short time to form nanoparticles. This method can easily mix multiple metals, providing exciting new possibilities for studying multi-element nanoparticles. Summary of the invention

[0005] Therefore, in response to the challenges currently faced by localized surface plasmon nanomaterials, the present invention proposes to introduce metal element components with significant localized surface plasmon resonance properties into high-entropy alloys through a carbon thermal shock method, and cleverly utilizes the special structure and properties of high-entropy alloys to regulate the surface electronic structure characteristics of nanoparticles, so that the high-entropy alloys exhibit obvious localized surface plasmon resonance characteristics.

[0006] In the present invention, the concentration of the precursor salt, the heating time and the heating temperature are explored respectively to determine the preparation conditions of the localized surface plasmon high entropy alloy prepared by the carbon thermal shock method. The influence of the proportion of each salt in the precursor solution on the proportion of each element in the high entropy alloy is analyzed. Then, the prepared high entropy alloy doped with metal elements having surface plasmon properties is spectrally characterized using ultraviolet-visible absorption spectroscopy to determine the optical properties of high entropy alloys with different components, element ratios and sizes. The development of the present invention provides a prerequisite for the widespread application of localized surface plasmon high entropy alloys in practice.

[0007] In order to solve the above-mentioned technical problems, this application provides the following technical solutions:

[0008] The present invention provides a method for preparing a localized surface plasmon high entropy alloy, comprising the following steps:

[0009] S11: adding a mixed precursor salt solution to the surface of the hydrophilic carbon paper treated with the precursor and then drying; the metal element in the mixed precursor salt solution is selected from one or more of gold, platinum, copper, cobalt, iron, palladium, nickel and iridium, and the solution is ethanol;

[0010] S12: Under a protective atmosphere, instantaneous voltage and current are applied to both ends of the hydrophilic carbon paper to which the mixed precursor salt solution is dropped in step S11, and heated to 1100-1700° C. in 0.5-1 s to obtain the localized surface plasmon high entropy alloy.

[0011] Preferably, in step S11, the drying method is air-drying at room temperature (25±5°C).

[0012] Preferably, the solute in the mixed precursor salt solution is selected from one or more of chloroauric acid, chloroplatinic acid, cupric chloride, cobalt chloride, ferrous chloride, palladium chloride, nickel chloride and chloroiridic acid.

[0013] Preferably, in the mixed precursor salt solution, the total concentration of the solute is in the range of 10-100 mM; and the concentration of each metal element in the solute is in the range of 2.5-20 mM.

[0014] Preferably, the metal element in the mixed precursor salt solution also includes ruthenium.

[0015] Preferably, in step S11, the precursor treatment method is oxygen plasma cleaning.

[0016] Preferably, the oxygen plasma cleaning has a power of 140-160 W and a time of 45-55 s.

[0017] Preferably, in step S12, under a protective atmosphere, the two ends of the hydrophilic carbon paper are respectively connected to copper tape, then fixed with silver paste, heated and fixed on a graphite electrode of a Joule heating device after the silver paste is solidified, and instantaneous voltage and current are applied to obtain the localized surface plasmon high entropy alloy; the temperature is monitored when the instantaneous voltage and current are applied.

[0018] Furthermore, the heating temperature is 55-65°C and the heating time is 3-5 h.

[0019] Furthermore, the protective atmosphere is a nitrogen atmosphere.

[0020] In order to obtain a localized surface plasmon high entropy alloy with uniformly mixed elements, the present invention prepares a localized surface plasmon high entropy alloy by adding a metal element with significant localized surface plasmon resonance properties into a precursor solution and using a rapid high-temperature quenching method - a carbon thermal shock method. The specific preparation process is as follows: Figure 1 First, a mixed metal salt alcohol solution is dripped onto the surface of carbon paper and dried at room temperature. Then, an instantaneous voltage and current are applied to the carbon paper loaded with metal salts, so that it can reach above 1100°C in a short time, and the required high entropy alloy is obtained by carbon thermal shock.

[0021] The present invention also provides a localized surface plasmon high entropy alloy prepared by the above preparation method.

[0022] Preferably, the localized surface plasmon high entropy alloy is selected from AuCuPtNiCo, AuCuPtNiFe, AuCuCoPtPd, AuCuNiIrCo, AuCuNiIrPt or AuCuPtCoFe.

[0023] The present invention also provides application of the localized surface plasmon high entropy alloy in electrocatalytic alcohol oxidation.

[0024] Preferably, the alcohol is methanol or ethanol.

[0025] The present invention also provides application of the localized surface plasmon high entropy alloy in electrocatalytic degradation of polyethylene terephthalate (PET).

[0026] The technical solution of the present invention has the following advantages over the prior art:

[0027] The present invention successfully designed and synthesized a high entropy alloy nanoparticle catalyst with localized surface plasmon properties on a carbon paper substrate, and applied it to the electrocatalytic alcohol oxidation reaction and electrocatalytic PET degradation, with very good catalytic performance and enhancement ability. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 Schematic diagram of the preparation process of high entropy alloy nanoparticles.

[0029] Figure 2 The SEM morphology and corresponding particle size distribution of high entropy alloys prepared with different precursor salt concentrations. From left to right, they are 2.5 mM / metal element, 5 mM / metal element, and 10 mM / metal element.

[0030] Figure 3 The SEM morphology and corresponding particle size distribution of high entropy alloys prepared at different heating times, from left to right, are 0.5 s, 0.8 s, and 1 s.

[0031] Figure 4 The SEM morphology and particle size distribution of high entropy alloys prepared at different heating temperatures. The SEM morphology from left to right is 1100 ℃, 1300 ℃, 1500 ℃ and 1700 ℃, and the particle size distribution from left to right is 1100 ℃, 1300 ℃ and 1500 ℃.

[0032] Figure 5 The SEM morphology of high entropy alloys with different element compositions are AuCuPtNiCo, AuCuPtNiFe, AuCuCoPtPd, AuCuNiIrCo, AuCuNiIrPt and AuCuPtCoFe.

[0033] Figure 6 HAADF images and STEM-EDX element maps of high entropy alloys with different element combinations, including AuCuNiIrCo, AuCuPtNiCo, AuCuPtNiFe and AuCuCoPtPd.

[0034] Figure 7 These are the SEM morphology images of high entropy alloys containing Ru elements, namely AuCuNiCoRu and AuCuCoRuIr.

[0035] Figure 8 The SEM morphology of AuCuPtPd with different element ratios are Au 17 Cu 22 Pt 27 Pd 34 ;Au 29 Cu26 Pt 25 Pd 20 .

[0036] Fig. 9 These are the SEM morphologies of alloys with different element combinations based on AuCu and PtCoFe, namely AuCu; AuCuPt; AuCuCo; AuCuFe; AuCuPtCo; AuCuCoFe; AuCuPtFe and PtCoFe.

[0037] Fig.10 HAADF images and EDX element maps of AuCu-based alloys with different element combinations are AuCu, AuCuCo, AuCuPt, and AuCuFe.

[0038] Fig.11 HAADF images and EDX elemental maps of AuCu-based alloys with different element combinations and PtCoFe, namely PtCofe, AuCuCoFe, AuCuPtCo, and AuCuPtFe.

[0039] Fig.12 The extinction spectra of AuCu and PtCoFe.

[0040] Fig.13 The extinction spectra of AuCuPtCoFe alloys with different AuCu-based element combinations are shown in Figure 1. They are AuCuPt; AuCuFe; AuCuCo; AuCuCoFe; AuCuPtFe; AuCuPtCo.

[0041] Fig.14 SEM images, particle size statistics and extinction spectra of AuCuPtCoFe at low and high magnification.

[0042] Fig.15 SEM images, particle size statistics and extinction spectra of AuCuPtPd at low and high magnifications.

[0043] Fig.16 SEM images, particle size statistics and extinction spectra of AuCuPtNi at low and high magnifications.

[0044] Fig.17 The basic catalytic performance of AuCuPtCoFe and commercial PtC for methanol and ethanol oxidation.

[0045] Fig.18 The catalytic performance of AuCuPtCoFe for photo-assisted electrocatalytic methanol and ethanol oxidation.

[0046] Fig.19Experimental and FDTD simulated extinction spectra for AuCuPtCoNi.

[0047] Fig. 20 LSV curves of AuCuPtCoNi in 1 M KOH with and without 1 M EG, scan rate 5 mV·s -1 .

[0048] Fig.21 The EGOR LSV curves of AuCuPtCoNi before and after light addition. From left to right, the current density is normalized to the geometric area and the unit mass of Pt.

[0049] Fig. 22 The electrolyte before and after electrolysis 1 H NMR spectra and the Faradaic efficiency and yield of glycolic acid produced at different voltages for 1 h were measured. DETAILED DESCRIPTION

[0050] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments so that those skilled in the art can better understand the present invention and implement it, but the embodiments are not intended to limit the present invention.

[0051] The main factors affecting the morphology and distribution of high entropy alloys are as follows: the concentration of the precursor salt, the heating time and the heating temperature, etc. In order to explore the influence of the precursor salt on the particle size and distribution of the nanoparticles, Examples 1 to 4 respectively change the concentration of the precursor salt, the heating rate and the heating temperature conditions on the basis of determining the four element components of AuCuPtPd, and characterize the prepared nanoparticles through SEM images and corresponding particle size distribution diagrams. Example 1

[0052] Cut a certain size of hydrophilic carbon paper (1.4×2 cm 2 ), use oxygen plasma cleaning to perform precursor treatment (150 W, 50 s) to make its surface extremely hydrophilic, providing favorable conditions for the uniform dispersion of the subsequent solution. Weigh 200 mg of chloroauric acid, 85.2 mg of copper chloride, 204.9 mg of chloroplatinic acid and 88.7 mg of palladium chloride powder, dissolve them in 10 mL of anhydrous ethanol respectively, and disperse them evenly by ultrasound. The concentration of the prepared precursor solution can be adjusted as needed, ranging from 50-200 mM. Here, a 50 mM precursor solution is prepared for use.

[0053] When preparing the sample, the separately prepared precursor solutions are mixed according to the same molar ratio of metal elements. The total concentration of the mixed precursor salt solution can also be adjusted as needed, ranging from 10-100 mM. Here, it is diluted to a mixed precursor salt solution with a total concentration of 20 mM.

[0054] Use a pipette to transfer 20 μL of the mixed precursor salt solution and drop it on the hydrophilic treated carbon paper surface and let it dry at room temperature.

[0055] The two ends of the carbon paper were connected to two copper tapes and fixed with silver paste. The silver paste was solidified by heating at 60 °C for 4 h. The frame was then placed on a graphite electrode in the vacuum chamber of a Joule heating device, and an instantaneous voltage and current were applied to it in a nitrogen atmosphere so that it could reach 1100 °C within 0.5 s, thereby obtaining a high entropy alloy AuCuPtPd. The corresponding temperature and heating rate were monitored by an infrared thermometer. Example 2

[0056] After determining the four elemental components of AuCuPtPd, we tried to change the concentration of the precursor salt. Figure 2 As shown, precursor salt solutions of chloroauric acid, cupric chloride, chloroplatinic acid and palladium chloride mixed in equal molar ratios of 2.5, 5 and 10 mM / metal element (the total concentration of the mixed precursor salt solution is 10 mM, 20 mM and 40 mM, respectively) are added dropwise to the treated carbon paper surface, and Joule heating treatment is performed by applying the same instantaneous voltage and current at the heating temperature (1100 ° C) and heating rate (0.5 s), and the remaining steps are the same as in Example 1.

[0057] It can be found that the metal salt has been completely decomposed and formed uniformly distributed nanoparticles on the carbon paper, and the particle size of the metal nanoparticles increases from 16 nm to 47 nm as the concentration of the precursor salt increases. This is mainly because as the salt content increases, more atoms tend to condense together during the heating process, thus making the particle size larger. Example 3

[0058] This example investigates the effect of the heating rate on the particle size distribution. The four element components of AuCuPtPd (i.e., chloroauric acid, cupric chloride, chloroplatinic acid, and palladium chloride mixed in equal molar ratios) are still selected. The precursor salt is determined to be 5 mM / metal element. Under the same conditions of applying instantaneous voltage and current and heating temperature of 1100°C, the heating rate is adjusted to reach the desired temperature in 0.5 s, 0.8 s, and 1 s, respectively. The remaining steps are the same as in Example 1.

[0059] The prepared samples were characterized by scanning electron microscopy (SEM) and the particle size statistics were performed, such as Figure 3As shown in the figure. As the heating rate decreases, the diameter of the nanoparticles increases first and then decreases. This is mainly because when the temperature rises, atoms or molecules have higher thermal energy and are therefore easier to diffuse in the solid material. If the heating rate is very fast, the atoms or molecules will not have enough time to diffuse to form a larger crystal structure. Therefore, a faster heating rate forms smaller grains. In addition, rapid heating may lead to high temperatures in local areas, which promotes the formation of crystal nuclei. When the temperature rises quickly, there are more opportunities for crystal nuclei to form, so more small grains will be formed instead of larger crystals. Example 4

[0060] This example explores the effect of different heating temperatures on the micromorphology and distribution state of high entropy alloys. Four elements of AuCuPtPd (i.e., chloroauric acid, cupric chloride, chloroplatinic acid, and palladium chloride mixed in equal molar ratios) were selected, and a 5 mM / metal element salt mixed solution was dripped onto carbon paper, and the heating time was set to 0.5 s when the same instantaneous voltage and current were applied, and the temperature was heated to 1100 ° C, 1300 ° C, 1500 ° C, and 1700 ° C, respectively. The rest of the method was the same as in Example 1.

[0061] It was characterized by scanning electron microscopy ( Figure 4 ), as the temperature increases, the diameter of the nanoparticles first decreases and then increases. However, when the temperature increases to 1500 °C, the surface of the nanoparticles is covered by a layer of film, and the higher the temperature, the more severe the coating, making it impossible for the nanoparticles to be exposed on the surface. Example 5

[0062] Through the exploration of the preparation conditions of high entropy alloys, and in order to meet the requirements of the LSPR effect on particle size, it was preliminarily determined that the total concentration of the precursor salt was 20 mM, the heating time when applying instantaneous voltage and current was 0.5 s, and the heating temperature was 1100°C as the optimal conditions for preparing localized surface plasmon high entropy alloys. Under this preparation condition, high entropy alloys of different element components of AuCuPtNiCo, AuCuPtNiFe, AuCuCoPtPd, AuCuNiIrCo, AuCuNiIrPt, and AuCuPtCoFe were prepared respectively (where each metal element was mixed in the mixed precursor solution in an equimolar ratio, with a total concentration of 20 mM), and the rest of the method was the same as in Example 1.

[0063] These elements have different atomic radii (1.24-1.44 Å), reduction potentials (-0.25-1.5 V vs. RHE), crystal structures, and melting temperatures, which would normally not favor the formation of solid solutions. Figure 5As shown in the figure, the high entropy alloys of various elements prepared by carbon thermal shock method can be evenly distributed on carbon paper, and the particle size distribution is relatively uniform. They were characterized by scanning transmission electron microscopy (STEM), high angle annular dark field (HAADF) and energy dispersive X-ray spectroscopy (EDS), as shown in the figure. Figure 6 As shown. The figure shows uniform atomic-scale mixing without obvious element segregation and phase separation. The size of the nanoparticles is also uniform regardless of the elemental composition. This is because the heating temperature far exceeds the thermal decomposition temperature of the metal precursor salt, so the salts are easily decomposed to form solid solution nanoparticles. This shows that this preparation method can be extended to more complex high-entropy alloy nanoparticles. Example 6

[0064] In the process of preparing different high entropy alloys, the incorporation of special elements will affect the particle size of nanoparticles, such as Figure 7 The same preparation conditions as in Example 1 were used, except that ruthenium element (Ru) was doped into the mixed salt solution, and a mixed precursor salt solution with a total concentration of 20 mM was prepared by mixing a ruthenium chloride solution with other metal element salt solutions in the element combination in an equimolar ratio, and then dripped onto the treated carbon paper surface, and AuCuNiCoRu and AuCuCoRuIr were prepared respectively by applying an instantaneous voltage, a current, a heating temperature of 1100 °C, and a heating time of 0.5 s.

[0065] Compared to when only one element is changed while the other four elements remain the same, the particle size of the nanoparticles is significantly reduced, shrinking to only 3-5 nm. This is due to the catalytically driven carbon metabolism reaction that occurs during the carbon thermal shock process. The carbon metabolism reaction involves C (fuel), O* (oxidant), and metal (catalyst), which relates the surface defect concentration of carbon paper and the catalytic activity of the metal to the final nanoparticle size and dispersibility. During high-temperature exposure, liquid metal droplets can move and split under the catalytic driving force. The use of larger O* concentrations and highly catalytically active metals can drive vigorous metabolic reactions, making the catalyst move and fission more frequent. Specifically, the higher the catalytic activity of the metal used, the smaller the size of the nanoparticles and the denser the distribution on the conductive substrate. Example 7

[0066] Under the same preparation conditions, by changing the ratio of each element in the precursor salt solution, the influence of the content of each element and the particle morphology in the prepared high entropy alloy was investigated.

[0067] In this example, a mixed precursor solution of chloroauric acid, chloroplatinic acid, cupric chloride and palladium chloride mixed in equal molar ratios and a mixed precursor solution of 6.5 mM chloroauric acid, 5 mM chloroplatinic acid, 5 mM cupric chloride and 3.5 mM palladium chloride dissolved in anhydrous ethanol were added respectively, and the remaining steps were the same as in Example 1 to prepare AuCuPtPd with different ratios.

[0068] Table 1 ICP-OES results of AuCuPtPd with different metal element ratios

[0069]

[0070] SEM morphology Figure 8 As shown, Table 1 is the proportion of each element under different proportions and the calculated mixed configuration entropy obtained by the inductively coupled plasma optical emission spectroscopy (ICP-OES) test. When the elements in the precursor solution are added in an equimolar ratio (Example 1), the element ratio of the prepared high entropy alloy is not completely equal, which is due to the different vapor pressures of the elements. After adjusting the proportion of the precursor salt (Example 7), its morphology and distribution did not change much, but the proportion of each element changed significantly. With the decrease of the Pd content in the precursor salt and the increase of the Au content, the proportion of Pd in ​​the prepared high entropy alloy was also reduced from 34% to 20%, the proportion of Au was increased from 17% to 29%, and the mixed configuration entropy was also increased from the original 1.35 R to 1.38 R. Therefore, changing the proportion of the precursor salt can achieve effective control of the component ratio. Example 8

[0071] The preparation method of localized surface plasmon high entropy alloys has been explored in the previous section, and their optical properties will be studied next. As we all know, gold and copper have obvious localized surface plasmon resonance effects, so this example will focus on the localized surface plasmon high entropy alloy prepared based on AuCu.

[0072] Taking the high entropy alloy AuCuPtCoFe of Example 5 as an example, its optical properties were explored, and the AuCu alloy and PtCoFe alloy were studied respectively.

[0073] By exploring the methods of preparing high entropy alloys, different AuCu-based alloys AuCuPt, AuCuCo, AuCuFe, AuCuPtCo, AuCuCoFe, AuCuPtFe and PtCoFe were prepared uniformly distributed on carbon paper. The metal elements were mixed in equal molar ratios, and the total concentration range was 10-100 mM. Here, the mixed precursor solution with a total concentration of 20 mM was taken as an example.

[0074] The preparation scheme is to prepare a mixed precursor solution of AuCuPt, AuCuCo, AuCuFe, AuCuPtCo, AuCuCoFe, AuCuPtFe and PtCoFe with a total concentration of 20 mM by mixing the prepared metal salt solutions in an equimolar ratio, and to pipette 20 μL of the mixture and drop it on the treated carbon paper surface, and to prepare the above alloy by applying instantaneous voltage and current, heating at 1100 °C, and heating time of 0.5 s. The remaining steps are the same as in Example 1. Its morphology distribution is as follows: Fig. 9 shown.

[0075] Fig.10 and Fig.11 High-angle annular dark field scanning transmission electron microscopy (HAADF-STEM) and energy dispersive X-ray spectroscopy (EDX) elemental analysis of individual nanoparticles of different alloys are shown. The elements in the figure are evenly distributed throughout the nanoparticles, without obvious element separation or segregation, which confirms that under this preparation condition, the carbon thermal shock method can prepare different alloys that are mixed evenly.

[0076] The UV-Vis extinction spectra of AuCu alloy and PtCoFe alloy are shown in Figure 2. Fig.12 As shown. Fig.12 It can be seen that the AuCu alloy nanoparticles have a strong UV-visible absorption peak centered at 590 nm, indicating that AuCu has good LSPR properties and photoresponse. However, the PtCoFe alloy has no absorption peak in the visible light wavelength range ( Fig.12 As shown in Figure 2, alloys composed of non-surface plasmon elements alone do not have LSPR properties.

[0077] Gold and copper were randomly combined with three elements, platinum, cobalt, and iron, and their extinction spectra were collected by UV-visible spectrophotometer, such as Fig.13 As shown. It can be observed that different element combinations based on AuCu have obvious extinction peaks in the range of 550-570 nm, which is mainly caused by the surface plasmon excitation of gold and copper, which also proves the feasibility of preparing high entropy alloys with surface plasmon properties. Compared with the single AuCu alloy, AuCuPt, AuCuFe, AuCuCo, AuCuCoFe, AuCuPtCo and AuCuPtFe alloys all show a certain blue shift, which is caused by the electronic interaction between gold and copper and other metal elements. Example 9

[0078] Chloroauric acid, chloroplatinic acid, cupric chloride and nickel chloride powders were weighed respectively and dissolved in anhydrous ethanol, and evenly dispersed by ultrasonication to prepare precursor solutions with a concentration of 50 mM for use.

[0079] When preparing the sample, the prepared precursor solution is mixed in equal proportions according to the molar amount of each metal element, and diluted to a mixed precursor salt solution with a total concentration range of 10-100 mM, and here it is diluted to a mixed precursor solution with a total concentration of 20 mM. The mixed precursor solution is dripped onto the surface of the pre-treated carbon paper and dried naturally. A carbon thermal shock is applied to it at a temperature of 1100 ° C for 0.5 s to prepare AuCuPtNi high entropy alloy. The remaining steps are the same as in Example 1, and the extinction spectrum is detected with the AuCuPtCoFe of Example 5 and the AuCuPtPd of Example 1, as shown in FIG. Figures 14 to 16 As shown. Characterization of different regions of the prepared high entropy alloy nanoparticles at low and high magnifications respectively shows that the nanoparticles synthesized by the carbon thermal shock method are evenly distributed on the carbon substrate and the particle morphology and size are uniform, with good consistency. Subsequently, the light response ability of the high entropy alloy was detected by UV-visible spectrophotometer, and it was found that AuCuPtCoFe nanoparticles had an obvious extinction peak at 557nm, AuCuPtPd had a strong light absorption peak at 600 nm, and AuCuPtNi had obvious light absorption ability at 564 nm. This shows that high entropy alloy nanoparticles doped with elements with significant localized surface plasmon properties have good LSPR properties, which will resonate with the frequency of the matching incident photons in the visible light range, resulting in coherent oscillations of electrons in energy and space, and generating a strong electric field around the metal surface, thereby promoting various electrocatalytic reactions.

[0080] Application Example 1 Application of Localized Surface Plasmon High Entropy Alloys in Electrocatalytic Alcohol Oxidation

[0081] Example 5: AuCuPtCoFe high entropy alloy with localized surface plasmon resonance effect was prepared on carbon paper by carbon thermal shock method and applied to alcohol oxidation. The performance of the prepared AuCuPtCoFe catalyst was compared with that of commercial PtC supported on carbon paper. Fig.17 The cyclic voltammetry (CV) curves in 1 M KOH+1 M CH3OH and 1 MKOH+1 M C2H5OH saturated with N2 are shown. In methanol oxidation (MOR), AuCuPtCoFe has excellent catalytic performance, and its mass activity can reach 7.06 A·mg -1 Pt , is a commercial PtC (0.854 A·mg -1 Pt ) by 8.3 times. At the same time, the catalyst also showed good catalytic ability in ethanol oxidation (EOR), with a mass-normalized current density of 11.8 A·mg -1Pt , is a commercial PtC (0.483 A·mg -1 Pt This is mainly due to the unique coordination environment and nanometer size that expose abundant active sites, giving full play to the cocktail effect of high entropy alloys.

[0082] On the premise that AuCuPtCoFe has good basic activity, the role of localized surface plasmon resonance effect in high entropy alloy electrocatalytic reaction is explored. Based on the spectral information of nanoparticles characterized above, xenon lamp light source is used uniformly to simulate sunlight.

[0083] Fig.18 The cyclic voltammograms of MOR and EOR of AuCuPtCoFe with and without light irradiation are plotted, respectively. The current density is normalized to the unit mass of Pt. Fig.18 The characteristic peaks of methanol oxidation can be identified in both the forward and backward scans. -2 Under the irradiation of xenon lamp light source, the peak current density in the forward scan increased from 7.06 A·mg in the dark to -1 Pt Increased to 11.9 A·mg under light irradiation -1 Pt , which increased by about 68%. In addition, the onset potential was significantly lower than that without light. The increased peak current density and reduced onset potential indicate that light can significantly improve the electrocatalytic activity of AuCuPtCoFe for MOR. Its application in EOR also shows obvious light enhancement effect. In addition, Fig.18 In the case of light illumination, the current density of AuCuPtCoFe increased from the initial 11.8 A·mg -1 Pt Increased to 14.7 A·mg -1 Pt , the performance was improved by 25%. This shows that AuCuPtCoFe catalysts have high catalytic activity in alcohol oxidation and can give full play to the role of LSPR in high entropy alloys, further improving the performance.

[0084] Table 2 compares the MOR performance of Pt-based catalysts in alkaline solutions published in recent years with the present invention. Without light, the electrocatalytic MOR activity of AuCuPtCoFe itself is at the mainstream level compared with the same type of catalysts; after light, under the action of LSPR effect, its current density is significantly improved by 68%, which is much better than the catalytic activity of other catalysts.

[0085] Table 2 Comparison of MOR performance of Pt-based catalysts in alkaline solution

[0086]

[0087] Comparing the literature on the EOR performance of Pt-based catalysts in alkaline solutions reported in recent years, the results are shown in Table 3. The mass activity of the AuCuPtCoFe catalyst is significantly higher than that of the same type of catalysts without light addition; the performance is further improved after light addition, achieving better catalytic activity.

[0088] Table 3 Comparison of EOR performance of Pt-based catalysts in alkaline solution

[0089]

[0090] Application Example 2 Application of localized surface plasmon high entropy alloy in electrocatalytic degradation of PET

[0091] In this application example, a high entropy alloy AuCuPtCoNi with localized surface plasmon resonance effect and good electrocatalytic degradation of PET was successfully selected and prepared. The specific preparation method is to weigh chloroauric acid, chloroplatinic acid, copper chloride, cobalt chloride and nickel chloride powders respectively, dissolve them in anhydrous ethanol, disperse them evenly by ultrasonication, and prepare precursor solutions with a concentration of 200 mM respectively for use.

[0092] When preparing the sample, the separately prepared precursor solutions are mixed in a molar ratio of 1:1:3:1:2 of metal elements Au:Cu:Pt:Co:Ni and diluted to a mixed precursor salt solution with a total concentration range of 10-100 mM. Here, a mixed precursor solution with a total concentration of 90 mM is taken as an example.

[0093] The mixed precursor solution was dripped onto the pre-treated carbon paper surface and dried naturally. Then, a carbon thermal shock was applied to the carbon paper, and the AuCuPtCoNi high entropy alloy was prepared by applying instantaneous voltage and current, heating temperature to 1100 °C, and heating time to 0.5 s.

[0094] The LSPR properties of AuCuPtCoNi were studied by combining experiments with calculations. First, the nanoparticles loaded on the quartz plate were tested by UV-visible spectrophotometer, such as Fig.19 As shown, it can be observed that the particle has an extinction peak at 534nm, indicating that AuCuPtCoNi can resonate with light in this band and excite more hot carriers, providing a certain theoretical basis for the improvement of catalytic activity. This result is consistent with the results of the finite difference time domain (FDTD) simulation calculation. It is worth noting that the extinction peak obtained in the experimental test is relatively wide, which is attributed to the fact that the size of the AuCuPtCoNi nanoparticles prepared on the quartz wafer is not completely consistent, but tends to be normally distributed.

[0095] In order to study the electrocatalytic oxidation activity of the prepared AuCuPtCoNi electrocatalyst for ethylene glycol (EG) in alkaline electrolyte, the linear sweep voltammetry curves (LSV curves) of the catalyst in 1 M KOH and 1 M KOH + 1 M EG solutions were tested, respectively. Fig. 20 The LSV curves of AuCuPtCoNi in 1 M KOH aqueous solution with or without 1 M EG are shown. In the absence of EG, an anodic potential of 1.73 V is required to achieve a peak voltage of 10 mA cm -2 After adding 1 M EG, the current density increased dramatically, and only 0.6 V was required to reach 10 mA cm -2 The current density is significantly lower than that of oxygen evolution reaction (OER) by 1.13 V, which means that ethylene glycol oxidation (EGOR) is more kinetically favorable than OER. Such a large potential difference can effectively reduce the competitive reaction of OER in the process of EG oxidation.

[0096] In order to give full play to the advantages of localized surface plasmon high entropy alloys, a light addition test was carried out. Fig.18 In the characterization scheme, the LSPR properties of nanoparticles have been characterized by extinction spectroscopy. In order to simulate the influence of sunlight, xenon lamps were used as the light source in this experiment. Fig.21 The LSV curves of AuCuPtCoNi EGOR under light and dark conditions are shown, and the current density is normalized to the geometric area and the unit mass of Pt, respectively. It can be seen from the figure that when the light power density is 500 mW·cm -2 When irradiated with a xenon light source, the current density increased significantly and the starting potential decreased significantly, requiring only 0.55 V to reach 10 mA·cm -2 The mass activity of AuCuPtCoNi is 7.0 A·mg in the dark. -1 Pt Significantly increased to 9.7 A·mg -1 Pt , the performance was improved by 38.6%, which is better than most catalysts reported so far (Table 4). This result shows that AuCuPtCoNi catalyst has great potential in PET plastic degradation and fully utilizes the advantages of LSPR effect in high entropy alloys to further improve its performance.

[0097] Table 4 Comparison of the mass activity of AuCuPtCoNi EGOR with currently reported catalysts

[0098]

[0099] The catalyst was tested in an H-type electrolyzer at a voltage range of 0.7-1.1 V with a time-current test at intervals of 0.1 V. 1 The electrolysis products were qualitatively and quantitatively evaluated by H NMR to determine the selectivity of EG for the products. Fig. 22 As shown in Figure 2, glycolic acid (GA ~ 3.7 ppm) is the main product of EGOR. Dark conditions refer to the test without light, and the light condition is 500mW·cm -2 Xenon lamp irradiation. Fig. 22 As shown in the figure, under dark conditions, in a wide potential window of 0.7-1.1 V, the Faradaic efficiency of GA decreases with increasing potential, but can reach more than 92%, and can reach nearly 100% at 0.8 V. The yield of GA reaches a maximum of 0.59 mmol cm at 1 V. -2 ·h -1 After adding light, as the potential increases, the more complete the oxidation of ethylene glycol, the lower the Faradaic efficiency of GA. However, in the entire potential test range, the Faradaic efficiency of GA still reaches more than 92%. Compared with the dark condition, the yield of GA after adding light is significantly improved at different potentials. The improvement effect is most significant at 0.9 V (71.9%), and the yield reaches the maximum value at 1 V, which is 0.81 mmol·cm -2 ·h -1 The introduction of light-assisted conditions significantly enhanced its electrocatalytic EGOR ability and improved the production efficiency of GA.

[0100] In summary, the present invention successfully designed and synthesized a high-entropy alloy nanoparticle catalyst with localized surface plasmon resonance properties on a carbon paper substrate, and applied it to the electrocatalytic alcohol oxidation reaction and electrocatalytic PET degradation, with very good catalytic performance and enhancement ability.

[0101] Obviously, the above embodiments are merely examples for clear explanation and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from these are still within the protection scope of the invention.

Claims

1. A method for preparing a localized surface plasmon high entropy alloy, characterized in that: The steps include: S11: adding a mixed precursor salt solution to the surface of the hydrophilic carbon paper treated with the precursor and then drying; the metal elements in the mixed precursor salt solution are selected from a plurality of gold, platinum, copper, cobalt, iron and nickel, the solution is ethanol, and the metal elements are mixed in an equal molar ratio; S12: Under a protective atmosphere, applying instantaneous voltage and current to both ends of the hydrophilic carbon paper to which the mixed precursor salt solution is added in step S11, and heating to 1100-1700° C. in 0.5-1 s to obtain the localized surface plasmon high entropy alloy; in the step S12, under a protective atmosphere, connecting both ends of the hydrophilic carbon paper to copper tapes, fixing the silver paste, heating and fixing the silver paste on the graphite electrode of the Joule heating device after solidification, applying instantaneous voltage and current to obtain the localized surface plasmon high entropy alloy; monitoring the temperature when applying the instantaneous voltage and current; The localized surface plasmon high entropy alloy is selected from AuCuPtCoNi or AuCuPtCoFe.

2. The preparation method according to claim 1, characterized in that In the step S11, the drying method is air-drying at room temperature.

3. The preparation method according to claim 1, characterized in that: In the mixed precursor salt solution, the total concentration of the solute is in the range of 10-100 mM; in the solute, the concentration of each metal element is in the range of 2.5-20 mM.

4. The preparation method according to claim 1, characterized in that: The metal elements in the mixed precursor salt solution also include ruthenium.

5. The preparation method according to claim 1, characterized in that: In the step S11, the precursor treatment method is oxygen plasma cleaning.

6. A localized surface plasmon high entropy alloy prepared by the preparation method according to any one of claims 1 to 5.

7. Use of the localized surface plasmon high entropy alloy described in claim 6 in electrocatalytic alcohol oxidation.

8. Use of the localized surface plasmon high entropy alloy according to claim 6 in electrocatalytic degradation of polyethylene terephthalate.