A modified hydrogel for achieving high solar water evaporation rates, its preparation method, and its applications.

By grafting charged nanoparticles onto the surface of a solar-powered water evaporation gel and treating it with a DC electric field, the limitations of evaporation rate and energy utilization efficiency in existing technologies have been solved, achieving a higher water evaporation rate and environmentally friendly modification effect.

CN118236928BActive Publication Date: 2026-11-10FUDAN UNIVERSITY
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410295442.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-15
Publication Date
2026-11-10
Estimated Expiration
2044-03-15

AI Technical Summary

Technical Problem

The evaporation rate and energy utilization efficiency of existing solar water evaporation gels are limited by environmental factors such as light intensity, temperature and humidity. Furthermore, existing modification methods suffer from problems such as local high-temperature aging, poor production repeatability, lengthy modification steps, and chemical reagent residues.

Method used

By grafting charged nanoparticles onto the surface of a solar water evaporation gel under the action of a DC electric field, including adding charged nanoparticles and salt solution to a two-electrode membrane electrolysis cell system, performing DC electric field grafting treatment, and optimizing the electric field strength and time, the interaction between nanoparticles and gel can be enhanced.

Benefits of technology

This method improves the water evaporation rate and light utilization, reduces the chemical potential of the gel surface, increases the evaporation area, weakens the hydrogen bond network, and achieves a higher water evaporation rate and energy utilization efficiency, while avoiding the complexity of chemical modification steps and chemical reagent residues.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118236928B_ABST
    Figure CN118236928B_ABST
Patent Text Reader

Abstract

This application discloses a modified hydrogel for achieving a high solar water evaporation rate, its preparation method, and its application, belonging to the field of solar water evaporation materials technology. The preparation method includes: preparing charged nanoparticles and grafting these charged nanoparticles onto the surface of a solar water evaporation gel under a DC electric field to obtain a modified hydrogel with a high solar water evaporation rate. This preparation method significantly reduces the chemical potential of the solar water evaporation gel surface, thereby significantly accelerating the transport and transfer of water from the interior of the gel to its surface, thus increasing the water evaporation rate. Furthermore, it reduces light reflection and effectively increases the evaporation area, significantly improving light utilization and further promoting the water evaporation rate. Thirdly, it effectively weakens the hydrogen bond network of the water layer on the surface of the solar water evaporation gel, promoting water evaporation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application belongs to the field of solar water evaporation materials technology, and particularly relates to a modified hydrogel for achieving high solar water evaporation rates, its preparation method and application. Background Technology

[0002] Solar-powered water evaporation purification boasts advantages such as low carbon footprint, environmental friendliness, and low cost, making it a research hotspot in the water purification field. However, limitations imposed by environmental factors such as light intensity, temperature, and humidity restrict the evaporation rate and efficiency of solar-powered water evaporation gels to meet practical production demands. Therefore, developing and preparing solar-powered water evaporation gels with high evaporation rates and high energy utilization efficiency is urgently needed.

[0003] Currently, solar water evaporation gels are mainly hydrogels, and the main methods to modify their evaporation rate and energy utilization efficiency are: (1) mixing photothermal particles into the solar water evaporation gel to enhance the photothermal conversion efficiency; (2) designing directional channels in the solar water evaporation gel to promote the directional transport of water molecules; (3) modifying the surface of the solar water evaporation gel to destroy the hydrogen bond network of water and achieve low-energy evaporation of water.

[0004] However, the above preparation method has the following drawbacks in practical applications: First, the mixing of photothermal particles in the solar water evaporation gel will generate local high temperatures during actual production, causing the solar water evaporation gel to age rapidly, and the water evaporation rate and purification degree to decrease rapidly; Second, designing directional channels in the solar water evaporation gel requires water to form columnar ice crystals rapidly with the assistance of liquid nitrogen. Since the conditions for ice crystal formation are very harsh and energy-intensive, the reproducibility of actual production is poor, making it difficult to scale up production; Third, the surface modification is mainly chemical etching modification, which has problems such as lengthy modification steps, complex post-processing, and low precision in modification space. At the same time, the chemical reagents used for modification may remain inside the solar water evaporation gel and volatilize during the water evaporation process, which does not meet the requirements of environmentally friendly production. Summary of the Invention

[0005] This application discloses a modified hydrogel for achieving a high solar water evaporation rate, its preparation method, and its application, effectively solving the aforementioned technical problems existing in current solar water evaporation gel preparation methods.

[0006] To achieve the above objectives, the first aspect of this application provides a method for preparing a modified hydrogel for achieving a high solar water evaporation rate. The preparation method of this application includes:

[0007] Preparation of charged nanoparticles;

[0008] By grafting the charged nanoparticles onto the surface of a solar water evaporation gel under the action of a DC electric field, a modified hydrogel with a high solar water evaporation rate is obtained.

[0009] In some embodiments, grafting the charged nanoparticles onto the surface of a solar-powered water evaporation gel under a direct current electric field includes:

[0010] In a two-electrode membrane electrolytic cell system, the solar water evaporation gel is used as a membrane, and charged nanoparticles and salt solution are added for DC electric field grafting treatment.

[0011] The electric field strength for the DC electric field grafting treatment is preferably 5 to 30 V / cm, and the time is preferably 0.5 to 2 hours.

[0012] The salt solution preferably includes a sodium salt solution or a potassium salt solution.

[0013] In some embodiments, the charged nanoparticles include one of the following: core-shell micelles with a polyelectrolyte shell, core-shell composite microgels with a polyelectrolyte shell, core-shell composite metal or inorganic nanoparticles with a polyelectrolyte shell.

[0014] In some embodiments, the polyelectrolyte comprises polyacrylic acid and fully quaternized poly(4-vinylpyridine).

[0015] In some embodiments, the core-shell micelles with a shell of polyelectrolyte include fully quaternized polystyrene-b-poly(4-vinylpyridine) core-shell micelles, fully quaternized polyhexafluorobutyl acrylate-b-poly(4-vinylpyridine) core-shell micelles, polystyrene-b-polyacrylate core-shell micelles, and polyhexafluorobutyl acrylate-b-polyacrylate core-shell micelles.

[0016] Preferably, the polystyrene block or the polyhexafluorobutyl acrylate block is also doped with photothermal particles.

[0017] In some embodiments, the method for preparing the fully quaternized polystyrene-b-poly(4-vinylpyridine) core-shell micelles includes:

[0018] Core-shell micelles of polystyrene-b-poly(4-vinylpyridine) block copolymers are provided;

[0019] The polystyrene-b-poly(4-vinylpyridine) block copolymer core-shell micelles were subjected to a complete quaternization reaction with a quaternizing agent in a co-solvent of N,N-dimethylformamide and methanol. The reaction product was then dialyzed in deionized water, and the dispersion of the fully quaternized polystyrene-b-poly(4-vinylpyridine) block copolymer core-shell micelles in water was collected.

[0020] The quaternizing agent preferably includes a haloaromatic hydrocarbon or a haloalkane with 1-5 carbon atoms;

[0021] When the polystyrene-b-poly(4-vinylpyridine) core-shell micelles undergo a complete quaternization reaction with the quaternizing agent, the molar ratio of the quaternizing agent to the pyridine groups in the polystyrene-b-poly(4-vinylpyridine) block copolymer is preferably greater than 10:1.

[0022] In some embodiments, the halogenated aromatic hydrocarbons include benzyl bromide and p-methylbenzyl bromide; the halogenated alkanes with 1-5 carbon atoms include iodomethane, iodoethane, 1-iodopropane, 1-iodobutane, 1-iodopentane, bromomethane, and bromoethane.

[0023] In some embodiments, the core-shell composite microgel with a polyelectrolyte shell includes fully quaternized poly(4-vinylpyridine)-b-poly(N-isopropylacrylamide) microgel and polyacrylic acid-b-poly(N-isopropylacrylamide) microgel.

[0024] In some embodiments, the shell is a core-shell composite metal or inorganic nanoparticle of polyelectrolyte, including gold nanoparticles with fully quaternized poly(4-vinylpyridine) or polyacrylic acid grafted on the surface, and titanium pentoxide nanoparticles.

[0025] In some embodiments, the solar water evaporation gel includes polymer hydrogels and supramolecular hydrogels;

[0026] The polymer hydrogel preferably includes polyvinyl alcohol hydrogel, polyacrylamide hydrogel, poly(2-hydroxyethyl methacrylate) hydrogel, polyacrylamide / agarose dual-network hydrogel, polyacrylamide / calcium alginate dual-network hydrogel, and polyethylene glycol hydrogel, and the hydrogel preferably also contains photothermal particles.

[0027] The supramolecular hydrogel preferably includes cyclodextrin hydrogel and poly(methacrylamide-co-methacrylic acid) hydrogel.

[0028] In some embodiments, the photothermal particles include titanium pentoxide nanoparticles, titanium dioxide nanoparticles, gold nanoparticles, graphene, and conductive carbon black.

[0029] The second aspect of this application provides a modified hydrogel with a high solar water evaporation rate, which is prepared by the preparation method described in the first aspect of this application.

[0030] A third aspect of this application provides a solar water evaporator, which includes a solar water evaporator body and a solar water evaporation component disposed at the outlet of the solar water evaporator body, wherein the solar water evaporation component is prepared by a modified hydrogel with a high solar water evaporation rate as described in this application.

[0031] Compared with the prior art, the advantages or beneficial effects of this application include at least the following:

[0032] The preparation method provided in this application grafts charged nanoparticles onto the surface of a solar water evaporation gel under a DC electric field. On the one hand, it can significantly reduce the chemical potential of the surface of the solar water evaporation gel without changing its network structure, thereby significantly accelerating the transport and transfer of water from the interior of the solar water evaporation gel to its surface and improving the water evaporation rate. On the other hand, the grafting of charged nanoparticles onto the surface of the solar water evaporation gel roughens its surface, thereby reducing light reflection and effectively increasing the evaporation area, thus improving the light utilization rate and improving the water evaporation rate. Thirdly, the electrostatic interaction between the charged nanoparticles can weaken the hydrogen bond network of the water layer on the surface of the solar water evaporation gel, which is beneficial to promoting water evaporation. Attached Figure Description

[0033] To more clearly illustrate the technical solutions of the embodiments of this application, the accompanying drawings used in the description of the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments recorded in this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0034] Figure 1 SEM image of the ST8-PVA hydrogel sample provided in the embodiments of this application;

[0035] Figure 2 PS provided for embodiments of this application 50000 -b-P4VP 13000 - Confocal microscopy image of a PVA hydrogel sample of Nile red core-shell micelles;

[0036] Figure 3 The ST1-PVA-Ti3O5, ST2-PVA-GO, ST4-PVA-Ti2O3, ST7-PHEMA, and ST provided in the embodiments of this application are for use in the present application. 18 -PVA-Ti2O3 and ST 19 - Evaporation rate data of PVA hydrogel samples (Data selection principles: 1- Reflects the highest achievable water evaporation rate; 2- Reflects the proportion of water evaporation rate improvement due to modification, 10-60%). Detailed Implementation

[0037] The technical solutions of the embodiments of this application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some, not all, of the embodiments of this application. All other embodiments obtained by those skilled in the art based on the embodiments of this application without creative effort are within the scope of protection of this application.

[0038] In the following description of this embodiment, the term "and / or" is used to describe the association relationship between related objects, indicating that three relationships can exist. For example, A and / or B can represent: A existing alone, B existing alone, and A and B existing simultaneously. A and B can be singular or plural. The character " / " generally indicates that the preceding and following related objects have an "or" relationship.

[0039] In the following description of this embodiment, the term "at least one" means one or more, and "more than one" means two or more. "At least one of the following" or similar expressions refer to any combination of these items, including any combination of single or multiple items. For example, "at least one of a, b, or c", or "at least one of a, b, and c", can both mean: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, and c can be single or multiple.

[0040] The terminology used in the embodiments of this application is for the purpose of describing particular embodiments only and is not intended to be limiting of this application. The singular forms "a" and "the" as used in the embodiments of this application and the appended claims are also intended to include the plural forms, unless the context clearly indicates otherwise.

[0041] Those skilled in the art should understand that, in the following description of the embodiments of this application, the sequence of numbers does not imply the order of execution. Some or all steps may be executed in parallel or sequentially. The execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of the embodiments of this application.

[0042] Those skilled in the art will understand that the numerical ranges in the embodiments of this application should be understood to specifically disclose each intermediate value between the upper and lower limits of the range. Each smaller range between any stated value or intermediate value within a stated range, and any other stated value or intermediate value within said range, is also included within the scope of this invention. The upper and lower limits of these smaller ranges may be independently included or excluded from the range.

[0043] Unless otherwise stated, the technical / scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this application pertains. While this application describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may be used in the implementation or testing of this application. All references to this specification are incorporated by way of citation to disclose and describe methods and / or materials associated with those references. In the event of any conflict with any incorporated reference, the content of this specification shall prevail.

[0044] In a first aspect, embodiments of this application provide a method for preparing a modified hydrogel for achieving a high solar water evaporation rate, the preparation method preferably comprising the following steps:

[0045] Preparation of charged nanoparticles;

[0046] By grafting the charged nanoparticles onto the surface of a solar water evaporation gel under the action of a DC electric field, a modified hydrogel with a high solar water evaporation rate is obtained.

[0047] In this embodiment, by grafting charged nanoparticles onto the surface of a solar water evaporation gel under a DC electric field, the chemical potential of the gel's surface can be significantly reduced without altering its network structure. This significantly accelerates the transport and transfer of water from the gel's interior to its surface, thereby increasing the water evaporation rate. Furthermore, the grafting of charged nanoparticles onto the surface of the gel roughens it, reducing light reflection and effectively increasing the evaporation area, thus improving light utilization and further enhancing the water evaporation rate. Finally, the electrostatic interactions between the charged nanoparticles weaken the hydrogen bond network of the water layer on the gel's surface, promoting water evaporation.

[0048] This application provides a method for grafting charged nanoparticles onto the surface of a solar-powered water evaporation gel under the action of a direct current electric field. The method preferably includes:

[0049] In a two-electrode membrane electrolytic cell system, the solar water evaporation gel to be modified is used as a membrane, and charged nanoparticles and salt solution are added for DC electric field grafting treatment.

[0050] It should be noted that the construction of a DC electric field grafting system by adding charged nanoparticles in this application specifically falls into two categories:

[0051] One method involves using the solar water evaporation gel to be modified as the membrane of the electrolytic cell, adding positively charged nanoparticles to the anode and deionized water to the cathode, and adding a small amount of salt solution to both electrodes.

[0052] Secondly, the solar water evaporation gel to be modified was used as the diaphragm of the electrolytic cell. Negatively charged nanoparticles were added to the cathode and deionized water was added to the anode, and a small amount of salt solution was added to both electrodes.

[0053] The salt solution includes sodium salt solution and potassium salt solution. For example, it can be sodium chloride, sodium nitrate, sodium acetate, sodium sulfate, potassium chloride, potassium nitrate, potassium acetate, potassium sulfate, etc. This application embodiment does not impose any special restrictions on this, as long as the performance requirements of inert electrolyte are met.

[0054] In this embodiment, the electric field strength for DC electric field grafting is preferably 5–30 V / cm, for example, it can be 5 V / cm, 10 V / cm, 15 V / cm, 20 V / cm, 25 V / cm, 30 V / cm, or any one within the range of the electric field strength; the time is preferably 0.5–2 h, for example, it can be 0.5 h, 1 h, 1.5 h, 2 h, or any one within the range of the time. In this embodiment, by using the above-mentioned electric field strength and grafting time, not only can the interaction between the shell polyelectrolyte and the three-dimensional network structure of the solar water evaporation gel be enhanced, improving grafting stability and thus obtaining a solar water evaporator that operates stably for a long time, but it can also provide sufficient time and space for the shell polyelectrolyte to adjust its conformation, allowing the polyelectrolyte to be uniformly distributed on the surface of the solar water evaporation gel, providing low chemical potentials, enhancing the driving force for water molecules to move from the solar water evaporation gel phase towards its surface, and thus significantly improving the water evaporation rate.

[0055] In this embodiment, the charged nanoparticles preferably include one of the following: core-shell micelles with a polyelectrolyte shell, core-shell composite microgels with a polyelectrolyte shell, core-shell composite metal or inorganic nanoparticles with a polyelectrolyte shell. The polyelectrolyte is preferably polyacrylic acid (PAA) and fully quaternized poly(4-vinylpyridine) (P4VP).

[0056] It should be noted that the core size of the core-shell (micelles, composite microgels, composite metals, or inorganic nanoparticles) with a polyelectrolyte shell needs to be larger than the mesh size of the solar water evaporation gel. This ensures that the modified part is confined to the surface of the solar water evaporation gel and does not affect the solar water evaporation gel itself. Furthermore, the polyelectrolyte in the shell can promote the uniform distribution of charged nanoparticles on the surface of the solar water evaporation gel through electrostatic interactions, resulting in good surface modification and significantly improving the water evaporation rate.

[0057] In the embodiments of this application, the core-shell micelles with a shell layer of polyelectrolyte include fully quaternized polystyrene-b-poly(4-vinylpyridine) core-shell micelles (PS-b-P4VP), fully quaternized polyhexafluorobutyl acrylate-b-poly(4-vinylpyridine) core-shell micelles (PHFBA-b-P4VP), polystyrene-b-polyacrylate core-shell micelles (PS-b-PAA), and polyhexafluorobutyl acrylate-b-polyacrylate core-shell micelles (PHFBA-b-PAA).

[0058] In this embodiment, the polystyrene block or the polyhexafluorobutyl acrylate block is preferably also doped with photothermal particles. These photothermal particles can be gold nanoparticles, titanium pentoxide nanoparticles, etc.

[0059] It should be noted that, in the embodiments of this application, photothermal conversion efficiency is improved by doping photothermal particles into polystyrene blocks or polyhexafluorobutyl acrylate blocks, thereby providing more energy for water evaporation and increasing the water evaporation rate.

[0060] This application provides a method for preparing fully quaternized polystyrene-b-poly(4-vinylpyridine) core-shell micelles, the method preferably comprising:

[0061] Core-shell micelles of polystyrene-b-poly(4-vinylpyridine) block copolymers are provided;

[0062] The polystyrene-b-poly(4-vinylpyridine) block copolymer core-shell micelles were subjected to a complete quaternization reaction with a quaternizing agent in a co-solvent of N,N-dimethylformamide and methanol. The reaction product was then dialyzed in deionized water, and the dispersion of the fully quaternized polystyrene-b-poly(4-vinylpyridine) block copolymer core-shell micelles in water was collected.

[0063] In this application, the preparation method of the core-shell micelles of polystyrene-b-poly(4-vinylpyridine) block copolymer is not limited. They can be prepared using methods known in the art, such as those described in this application, which include the following steps:

[0064] PS 50000 -b-P4VP 13000 (Subscripts indicate molecular weight) Dissolve in ultra-dry N,N-dimethylformamide (DMF), and add methanol dropwise to form a PS-b-P4VP micelle dispersion with a core-shell structure.

[0065] Of course, this application does not impose any particular limitations on the molecular weight, solvent, etc. of the copolymer used to prepare the core-shell micelle dispersion of PS-b-P4VP with a core-shell structure. Those skilled in the art can choose according to actual needs, for example, PS 50000 -b-P4VP 13000 You can use Photoshop 300000 -b-P4VP 175000 Alternatively, DMF can be replaced with other anhydrous good solvents for PS-b-P4VP, and methanol can be replaced with other solvents that can promote the formation of a shell structure in PS-b-P4VP micelles. In addition, when preparing PS-b-P4VP micelle dispersions with core-shell structures, photothermal particles such as gold and titanium pentoxide can be added simultaneously to prepare fully quaternized PS-b-P4VP micelle dispersions with core-shell structures and doped with photothermal particles in the core.

[0066] In the embodiments of this application, the quaternizing agent preferably includes a haloaromatic hydrocarbon or a haloalkane with 1-5 carbon atoms. The haloaromatic hydrocarbon can be benzyl bromide, p-methylbenzyl bromide; the haloalkane with 1-5 carbon atoms can be iodomethane, iodoethane, 1-iodopropane, 1-iodobutane, 1-iodopentane, bromomethane, bromoethane, etc.

[0067] It should be noted that water exists in three states within the solar-powered water evaporation gel: free water, intermediate water, and bound water. The proportion of intermediate water is a crucial factor affecting the water evaporation rate. These quaternizing agents, possessing a large number of alkyl groups, can effectively disrupt the hydrogen bond network formed by free water, converting it into intermediate water. This increases the proportion of intermediate water, lowers the enthalpy of vaporization, and promotes water evaporation. Specifically, when the quaternizing agent is iodomethane, the alkyl group's volume is already larger than the pore size of the hydrogen bond network, thus sufficiently disrupting it. Furthermore, iodomethane has the largest alkyl surface area, resulting in the highest efficiency in disrupting the hydrogen bond network and the greatest contribution to the water evaporation rate. Therefore, iodomethane is preferred as the quaternizing agent in this application.

[0068] In the embodiments of this application, when the polystyrene-b-poly(4-vinylpyridine) core-shell micelles undergo a complete quaternization reaction with the quaternizing agent, the molar ratio of the quaternizing agent to the pyridine groups in the polystyrene-poly(4-vinylpyridine) block copolymer is preferably greater than 10:1.

[0069] In this embodiment of the application, the core-shell composite microgel with a shell of polyelectrolytes includes fully quaternized poly(4-vinylpyridine)-b-poly(N-isopropylacrylamide) (P4VP-b-PNIPAM) microgel and polyacrylic acid-b-poly(N-isopropylacrylamide) (PAA-b-PNIPAM) microgel.

[0070] In the embodiments of this application, the core-shell composite metal or inorganic nanoparticles with a shell of polyelectrolyte preferably include gold nanoparticles (AuNPs) or titanium pentoxide nanoparticles (Ti3O5NPs) with fully quaternized poly(4-vinylpyridine) (P4VP) or polyacrylic acid (PAA) grafted on their surface.

[0071] In this embodiment, the solar water evaporation gel includes polymer hydrogels and supramolecular hydrogels. The polymer hydrogels include polyvinyl alcohol (PVA) hydrogels, polyacrylamide (PAAm) hydrogels, poly(2-hydroxyethyl methacrylate) (PHEMA) hydrogels, polyacrylamide-agarose double-network (PAAm-Agarose) hydrogels, polyacrylamide-calcium alginate double-network (PAAm-AlgCa) hydrogels, polyethylene glycol (PEG) hydrogels, etc.; the supramolecular hydrogels include cyclodextrin hydrogels, poly(methacrylamide-co-methacrylic acid) (P(MAAm-co-MAAc)) hydrogels, etc.

[0072] In this embodiment, the polymer hydrogel is further doped with photothermal particles. These photothermal particles can be titanium pentoxide nanoparticles (Ti3O5NPs), titanium trioxide nanoparticles (Ti2O3NPs), gold nanoparticles (AuNPs), graphene (GO), and conductive carbon black (CB).

[0073] Secondly, embodiments of this application provide modified hydrogels prepared by the method described in this application. The preparation method of this application reduces the chemical potential of the surface of the solar-evaporated water gel, effectively reduces light reflection, increases the evaporation area, and weakens the hydrogen bond network of the water layer. Therefore, the modified hydrogels prepared by this application possess higher water evaporation rates and energy utilization efficiency, while achieving low-energy water evaporation, making them suitable for commercial production applications.

[0074] Thirdly, this application provides a solar water evaporator, which includes a solar water evaporator body and a solar water evaporation component disposed at the outlet of the solar water evaporator body. The solar water evaporation component is prepared from the modified hydrogel prepared in this application. Since the modified hydrogel has a higher water evaporation rate and energy utilization efficiency and can achieve low-energy evaporation of water, the water evaporation rate of the solar water evaporator in this application is significantly improved, effectively reducing the impact of environmental factors.

[0075] The technical solution of this application will be further described below with reference to specific embodiments.

[0076] Example 1

[0077] This embodiment provides a method for preparing ST1-PVA-Ti3O5 hydrogel, including the following steps:

[0078] S1: Dissolve 1.8g PVA and 0.108g Ti3O5 in 10mL DMSO, pour into a glass mold and immerse in deionized water for 2 days, changing the water every 6 hours to obtain a PVA-Ti3O5 hydrogel matrix;

[0079] S2: Add 5mg PS 50000 -b-P4VP 13000 Dissolved in 5 mL DMF, and then 9 mL of methanol was added dropwise at a rate of 4.5 mL / h to obtain PS with a core-shell structure. 50000 -b-P4VP 13000 Micellar dispersion;

[0080] S3: In the PS with a core-shell structure 50000 -b-P4VP 13000 20 μL of iodomethane was added to the micelle dispersion, and the mixture was reacted overnight at 40 °C. The product was then dialyzed against deionized water for at least 2 h to obtain fully quaternized PS. 50000 -b-P4VP 13000 Micellar dispersion MS1;

[0081] S4: In a two-electrode diaphragm electrolytic cell, a PVA-Ti3O5 hydrogel matrix is ​​sandwiched in the middle of the cell as a diaphragm, and 5 mL of fully quaternized PS is added to the anode. 50000 -b-P4VP 13000 Micelle dispersion MS1 ​​was prepared by adding 5 mL of deionized water to the cathode and a small amount of sodium chloride to both electrodes. Then, electric field grafting was performed for 1 h under an electric field strength of 5 V / cm to obtain ST1-PVA-Ti3O5 hydrogel.

[0082] Example 2

[0083] This embodiment provides a method for preparing ST2-PVA-GO hydrogel, including the following steps:

[0084] S1: Dissolve 1.8g PVA and 0.18g GO in 10mL DMSO, pour into a glass mold and immerse in deionized water for 2 days, changing the water every 6 hours to obtain the PVA-GO hydrogel matrix;

[0085] S2: Preparation of fully quaternized PS 50000 -b-P4VP 13000 Micellar dispersion MS1 ​​(same as Example 1);

[0086] S3: In a two-electrode membrane electrolytic cell, a PVA-GO hydrogel matrix is ​​sandwiched in the middle of the cell as a membrane, and 5 mL of fully quaternized PS is added to the anode. 50000 -b-P4VP 13000 Micelle dispersion MS1 ​​was prepared by adding 5 mL of deionized water to the cathode and a small amount of potassium chloride to both electrodes. The mixture was then subjected to electric field grafting for 0.5 h at an electric field strength of 5 V / cm to obtain ST2-PVA-GO hydrogel.

[0087] Example 3

[0088] This embodiment provides a method for preparing ST3-PVA-CB hydrogel, including the following steps:

[0089] S1: Dissolve 1.8g PVA and 0.18g CB in 10mL DMSO, pour into a glass mold and soak in deionized water for 2 days, changing the water every 6 hours to obtain a PVA-CB hydrogel matrix;

[0090] S2: Preparation of fully quaternized PS 50000 -b-P4VP 13000 Micellar dispersion MS1 ​​(same as Example 1);

[0091] S3: In a two-electrode diaphragm electrolytic cell, a PVA-CB hydrogel matrix is ​​sandwiched in the middle of the cell as a diaphragm, and 5 mL of fully quaternized PS is added to the anode. 50000 -b-P4VP 13000 Micelle dispersion MS1 ​​was prepared by adding 5 mL of deionized water to the cathode and a small amount of sodium nitrate to both electrodes. The mixture was then subjected to electric field grafting for 1.5 h under an electric field strength of 10 V / cm to obtain ST3-PVA-CB hydrogel.

[0092] Example 4

[0093] This embodiment provides a method for preparing ST4-PVA-Ti2O3 hydrogel, including the following steps:

[0094] S1: Dissolve 1.8g PVA and 0.108g Ti2O3 in 10mL DMSO, pour into a glass mold and soak in deionized water for 2 days, changing the water every 6 hours to obtain a PVA-Ti2O3 hydrogel matrix;

[0095] S2: Preparation of fully quaternized PS 50000 -b-P4VP 13000 Micellar dispersion MS1 ​​(same as Example 1);

[0096] S3: In a two-electrode diaphragm electrolytic cell, a PVA-Ti2O3 hydrogel matrix is ​​sandwiched in the middle of the cell as a diaphragm, and 5 mL of fully quaternized PS is added to the anode. 50000 -b-P4VP 13000 Micelle dispersion MS1 ​​was prepared by adding 5 mL of deionized water to the cathode and a small amount of potassium nitrate solution to both electrodes. The mixture was then subjected to electric field grafting for 1 h under an electric field strength of 10 V / cm to obtain ST4-PVA-Ti2O3 hydrogel.

[0097] Example 5

[0098] This embodiment provides a method for preparing ST5-PAAm-Agarose dual-network hydrogel, including the following steps:

[0099] S1: Dissolve 1.24g AAM, 43.03g MBAA, 39.1mg photoinitiator 2959 and 0.15g agarose in deionized water and purge with argon gas for 10 min to remove oxygen. Inject into a glass mold, crosslink under ultraviolet light for 1 h and allow to fully swell in water to obtain PAAm-Agarose double network hydrogel matrix.

[0100] S2: Preparation of fully quaternized PS 50000 -b-P4VP 13000 Micellar dispersion MS1 ​​(same as Example 1);

[0101] S3: In a two-electrode diaphragm electrolytic cell, a PAAm-Agarose dual-network hydrogel matrix is ​​sandwiched in the middle of the cell as a diaphragm, and 5 mL of fully quaternized PS is added to the anode. 50000 -b-P4VP 13000 Micelle dispersion MS1 ​​was prepared by adding 5 mL of deionized water to the cathode and a small amount of sodium sulfate solution to both electrodes. The mixture was then subjected to electric field grafting for 1 h at an electric field strength of 15 V / cm to obtain ST5-PAAm-Agar dual-network hydrogel.

[0102] Example 6

[0103] This embodiment provides a method for preparing ST6-PAAm-AlgCa dual-network hydrogel, including the following steps:

[0104] S1: Dissolve 1.24g AAM, 43.03g MBAA, 39.1mg photoinitiator 2959 and 0.15g sodium alginate in deionized water, purge with argon gas to remove oxygen for 10min, inject into a glass mold, crosslink with ultraviolet light for 1h and immerse in saturated CaCl2 solution overnight, and fully swell in water to obtain PAAm-AlgCa double network hydrogel matrix;

[0105] S2: Preparation of fully quaternized PS50000 -b-P4VP 13000 Micellar dispersion MS1 ​​(same as Example 1);

[0106] S3: In a two-electrode membrane electrolytic cell, PAAm-Alginate-Ca 2+ A dual-network hydrogel matrix is ​​sandwiched in the middle of the electrolytic cell as a diaphragm, and 5 mL of fully quaternized PS is added at the anode. 50000 -b-P4VP 13000 Micelle dispersion MS1 ​​was prepared by adding 5 mL of deionized water to the cathode and a small amount of potassium sulfate solution to both electrodes. The mixture was then subjected to electric field grafting at an electric field strength of 15 V / cm for 1 h to obtain ST6-PAAm-Alginate-Ca. 2+ Dual-network hydrogel.

[0107] Example 7

[0108] This embodiment provides a method for preparing ST7-PHEMA hydrogel, including the following steps:

[0109] S1: Dissolve 6 mL of HEMA and 9.56 mg of benzoin dimethyl ether in 4 mL of deionized water, purge with argon gas to remove oxygen for 10 min, inject into a glass mold, crosslink under ultraviolet light for 10 min, and allow to fully swell in water to obtain the PHEMA hydrogel matrix;

[0110] S2: Preparation of fully quaternized PS 50000 -b-P4VP 13000 Micellar dispersion MS1 ​​(same as Example 1);

[0111] S3: In a two-electrode diaphragm electrolytic cell, a PHEMA hydrogel matrix is ​​sandwiched between the cells as a diaphragm, and 5 mL of fully quaternized PS is added to the anode. 50000 -b-P4VP 13000 MS1 micelle dispersion was prepared by adding 5 mL of deionized water to the cathode and a small amount of sodium acetate solution to both electrodes. The mixture was then subjected to electric field grafting for 1 h at an electric field strength of 20 V / cm to obtain ST7-PHEMA hydrogel.

[0112] Example 8

[0113] This embodiment provides a method for preparing ST8-PVA hydrogel, including the following steps:

[0114] S1: Dissolve 1.8g PVA in 10mL DMSO, pour into a glass mold and soak in deionized water for 2 days, changing the water every 6 hours to obtain the PVA hydrogel matrix;

[0115] S2: Preparation of fully quaternized PS 50000-b-P4VP 13000 Micellar dispersion (same as in Example 1);

[0116] S3: In a two-electrode diaphragm electrolytic cell, a PVA hydrogel matrix is ​​sandwiched between the cells as a diaphragm, and 5 mL of fully quaternized PS is added to the anode. 50000 -b-P4VP 13000 MS1 micelle dispersion was prepared by adding 5 mL of deionized water to the cathode and a small amount of potassium acetate solution to both electrodes. The mixture was then subjected to electric field grafting for 1 h at an electric field strength of 20 V / cm to obtain ST8-PVA hydrogel.

[0117] Example 9

[0118] This embodiment provides a method for preparing ST9-PVA-PEG dual-network hydrogel, including the following steps:

[0119] S101: Dissolve 1g PVA in 10mL of water, add 0.4g PEG and dissolve it completely, pour it into a glass mold, freeze it at -20℃ for 12h, and then thaw it at 30℃ for 1h to obtain a PVA-PEG dual-network hydrogel matrix.

[0120] S102: Preparation of fully quaternized PS 50000 -b-P4VP 13000 Micellar dispersion MS1 ​​(same as Example 1);

[0121] S103: In a two-electrode diaphragm electrolytic cell, a PVA-PEG dual-network hydrogel matrix is ​​sandwiched in the middle of the electrolytic cell as a diaphragm, and 5 mL of fully quaternized PS is added to the anode. 50000 -b-P4VP 13000 Micelle dispersion MS1 ​​was prepared by adding 5 mL of deionized water to the cathode and a small amount of potassium nitrate solution to both electrodes. The mixture was then subjected to electric field grafting for 1 h at an electric field strength of 25 V / cm to obtain ST9-PVA-PEG dual-network hydrogel.

[0122] Example 10

[0123] This embodiment provides ST 10 The preparation method of PVA hydrogel includes the following steps:

[0124] S1: Preparation of PVA hydrogel matrix (same as in Example 8);

[0125] S2: Preparation of PS with core-shell structure 50000 -b-P4VP 13000 Micellar dispersion (same as in Example 1);

[0126] S3: In the PS with a core-shell structure50000 -b-P4VP 13000 20 μL of 1-iodopropane was added to the micelle dispersion, and the reaction was carried out overnight at 40 °C. The reaction product was then dialyzed against deionized water for at least 2 h to obtain fully quaternized PS. 50000 -b-P4VP 13000 Micellar dispersion MS2;

[0127] S4: In a two-electrode diaphragm electrolytic cell, a PVA hydrogel matrix is ​​sandwiched between the cells as a diaphragm, and 5 mL of fully quaternized PS is added to the anode. 50000 -b-P4VP 13000 Micelle dispersion MS2 was subjected to electric field grafting for 0.5 h under an electric field strength of 25 V / cm, with 5 mL of deionized water added to the cathode and a small amount of sodium nitrate solution added to both electrodes. ST was obtained. 10 -PVA hydrogel.

[0128] Example 11

[0129] This embodiment provides ST 11 The preparation method of PVA hydrogel includes the following steps:

[0130] S1: Preparation of PVA hydrogel (same as in Example 1);

[0131] S2: Preparation of PS with core-shell structure 50000 -b-P4VP 13000 Micellar dispersion (same as in Example 1);

[0132] S3: In the PS with a core-shell structure 50000 -b-P4VP 13000 20 μL of neopentyl iodine was added to the micelle dispersion, and the reaction was carried out overnight at 40 °C. The reaction product was then dialyzed against deionized water for at least 2 h to obtain fully quaternized PS. 50000 -b-P4VP 13000 Micellar dispersion MS3;

[0133] S4: In a two-electrode diaphragm electrolytic cell, a PVA hydrogel matrix is ​​sandwiched between the cells as a diaphragm, and 5 mL of fully quaternized PS is added to the anode. 50000 -b-P4VP 13000 Micelle dispersion MS3 was subjected to electric field grafting for 1 hour under the condition of 30 V / cm, with 5 mL of deionized water added to the cathode and a small amount of potassium nitrate solution added to both electrodes. ST was obtained. 11 -PVA hydrogel.

[0134] Example 12

[0135] This embodiment provides ST 12 The preparation method of PAAm hydrogel includes the following steps:

[0136] S1: Dissolve 1.24g AAM, 43.03g MBAA and 39.1mg photoinitiator 2959 in deionized water, purge with argon gas to remove oxygen for 10min, inject into a glass mold, crosslink with ultraviolet light for 1h, and fully swell in water to obtain PAAm hydrogel matrix;

[0137] S2: Preparation of fully quaternized PS 300000 -b-P4VP 175000 Micellar dispersion MS4 (same as Example 1);

[0138] S3: In a two-electrode diaphragm electrolytic cell, a PAAm hydrogel matrix is ​​sandwiched between the cells as a diaphragm, and 5 mL of fully quaternized PS is added to the anode. 300000 -b-P4VP 175000 Micelle dispersion MS4 was prepared by adding 5 mL of deionized water to the cathode and a small amount of sodium sulfate solution to both electrodes. The mixture was then subjected to electric field grafting at an electric field strength of 30 V / cm for 1 hour to obtain ST. 12 -PAAm hydrogel.

[0139] Example 13

[0140] This embodiment provides ST 13 The preparation method of PVA hydrogel includes the following steps:

[0141] S1: Preparation of PVA hydrogel matrix (same as in Example 8);

[0142] S2: Preparation of fully quaternized PS 12000 -b-P4VP 9500 Micellar dispersion MS5 (same as Example 1);

[0143] S3: In a two-electrode diaphragm electrolytic cell, a PVA hydrogel matrix is ​​sandwiched between the cells as a diaphragm, and 5 mL of fully quaternized PS is added to the anode. 12000 -b-P4VP 9500 Micelle dispersion MS5 was prepared by adding 5 mL of deionized water to the cathode and a small amount of potassium nitrate solution to both electrodes. The mixture was then subjected to electric field grafting at an electric field strength of 30 V / cm for 1 hour to obtain ST. 13 -PVA hydrogel.

[0144] Example 14

[0145] This embodiment provides ST 14 The preparation method of PVA hydrogel includes the following steps:

[0146] S1: Preparation of PVA hydrogel matrix (same as in Example 8);

[0147] S2: Preparation of fully quaternized PS 350000 -b-P4VP 450000 Micellar dispersion MS6 (same as Example 1);

[0148] S3: In a two-electrode diaphragm electrolytic cell, a PVA hydrogel matrix is ​​sandwiched between the cells as a diaphragm, and 5 mL of fully quaternized PS is added to the anode. 350000 -b-P4VP 450000 Micelle dispersion MS6 was prepared by adding 5 mL of deionized water to the cathode and a small amount of potassium nitrate solution to both electrodes. The mixture was then subjected to electric field grafting at an electric field strength of 15 V / cm for 1 hour to obtain ST. 14 -PVA hydrogel.

[0149] Example 15

[0150] This embodiment provides ST 15 The preparation method of PVA hydrogel includes the following steps:

[0151] S1: Preparation of PVA hydrogel matrix (same as in Example 8);

[0152] S2: Take 20 mL of 0.01% chloroauric acid solution, heat to boiling, add 2 mL of 1% sodium citrate solution under high-speed stirring, reflux for 10 min, remove the heat source and continue stirring for 15 min, cool to room temperature, and obtain gold nanoparticles (AuNPs) with a diameter of about 40 nm; take 15 mL of AuNPs solution, purge with argon gas to remove oxygen for 15 min, add 278 mg of fully quaternized 4-vinylpyridine and 5.8 mg of vinylacetic acid, stir for 15 min, add 100 μL of 0.1 M azobisisobutyramidine hydrochloride and react for 10 min, stop argon gas, react at 70 °C for 4 h, and dilute the reaction product to 60 mL, centrifuge at 4500 rpm for 30 min, disperse in 10 mL of water, repeat 5 times to obtain a core-shell structured gold nanoparticle (Au@P4VPNPs) solution with fully quaternized P4VP grafted on the surface.

[0153] S3: In a two-electrode diaphragm electrolytic cell, a PVA hydrogel matrix is ​​sandwiched between the cells as a diaphragm. 5 mL of deionized water and a small amount of potassium sulfate solution are added to the anode, and 5 mL of Alu@P4VPNPs solution (MS7) is added to the cathode. Electric field grafting is performed for 1 hour at an electric field strength of 15 V / cm to obtain ST. 15 -PVA hydrogel.

[0154] Example 16

[0155] This embodiment provides ST 16 The preparation method of PVA hydrogel includes the following steps:

[0156] S1: Preparation of PVA hydrogel matrix (same as in Example 8);

[0157] S2: 9.6 mg Ti3O5 was dispersed in 15 mL of deionized water, 278 mg of fully quaternized 4-vinylpyridine and 5.8 mg of vinylacetic acid were added, and the mixture was stirred for 15 min. 100 μL of 0.1 M azobisisobutyramidine hydrochloride was added and the reaction was carried out for 10 min. Argon gas was stopped and the reaction was carried out at 70 °C for 4 h. The reaction product was diluted to 60 mL, centrifuged at 4500 rpm for 30 min, and dispersed in 10 mL of water. The reaction was repeated 5 times to obtain a solution MS8 of core-shell structured Ti3O5 nanoparticles (Ti3O5@P4VPNPs) with fully quaternized P4VP grafted on the surface.

[0158] S3: In a two-electrode diaphragm electrolytic cell, a PVA hydrogel matrix is ​​sandwiched between the cells as a diaphragm. 5 mL of Ti3O5@P4VPNPs solution (MS8) is added to the anode, and 5 mL of deionized water is added to the cathode. Small amounts of potassium nitrate solution are added to both electrodes. Electric field grafting is performed for 1 hour at an electric field strength of 15 V / cm to obtain ST. 16 -PVA hydrogel.

[0159] Example 17

[0160] This embodiment provides ST 17 The preparation method of PVA-PEG dual-network hydrogel includes the following steps:

[0161] S1: Preparation of PVA-PEG dual-network hydrogel matrix (same as Example 9);

[0162] S2: In a two-electrode diaphragm electrolytic cell, a PVA-PEG dual-network hydrogel matrix is ​​sandwiched in the middle of the cell as a diaphragm. 5 mL of deionized water is added to the anode, and 5 mL of Ti3O5@P4VP NPs solution MS9 is added to the cathode. A small amount of sodium nitrate solution is added to both electrodes. Electric field grafting is performed for 1 hour under an electric field strength of 20 V / cm to obtain ST. 17 -PVA-PEG dual-network hydrogel.

[0163] Example 18

[0164] This embodiment provides ST 18 The preparation method of PVA-Ti2O3 hydrogel includes the following steps:

[0165] S1: Preparation of PVA-Ti2O3 hydrogel matrix (same as Example 4);

[0166] S2: Mix 0.3 mg Ti3O5 with 5 mg PS 50000 -b-P4VP 13000 Dissolved in 5 mL DMF, and 9 mL of methanol was added dropwise at a rate of 4.5 mL / h to obtain PS doped Ti3O5NPs with a core-shell structure. 50000 -b-P4VP 13000 Micellar dispersion;

[0167] S3: PS of doped Ti3O5 NPs with core-shell structure 50000 -b-P4VP 13000 20 μL of methyl bromide was added to the micelle dispersion, and the reaction was carried out overnight at 45 °C. The reaction product was then dialyzed in deionized water for at least 2 h to obtain PS of fully quaternized doped Ti3O5 NPs. 50000 -b-P4VP 1300 Micellar dispersion MS 10 ;

[0168] S4: In a two-electrode membrane electrolytic cell, a PVA-Ti2O3 hydrogel matrix is ​​sandwiched in the middle of the cell as a membrane. 5 mL of fully quaternized doped Ti3O5 NPs in PS is added to the anode. 50000 -b-P4VP 1300 Micellar dispersion MS 10 Add 5 mL of deionized water to the cathode and a small amount of potassium chloride solution to each electrode. Perform electric field grafting for 1 hour under an electric field strength of 25 V / cm to obtain ST. 18 -PVA-Ti2O3 hydrogel.

[0169] Example 19

[0170] This embodiment provides ST 19 The preparation method of PVA hydrogel includes the following steps:

[0171] S1: Preparation of PVA hydrogel matrix (same as in Example 8);

[0172] S2: Mix 0.3 mg Ti2O3 with 5 mg PS 50000 -b-P4VP 13000 Dissolved in 5 mL DMF, and 9 mL of methanol was added dropwise at a rate of 4.5 mL / h to obtain PS doped Ti₂O₃NPs with a core-shell structure. 50000 -b-P4VP 13000 Micellar dispersion;

[0173] S3: PS of doped Ti2O3NPs with a core-shell structure50000 -b-P4VP 13000 20 μL of iodoethane was added to the micelle dispersion, and the reaction was carried out overnight at 45 °C. The reaction product was then dialyzed in deionized water for at least 2 h to obtain PS of fully quaternized doped Ti₂O₃NPs. 50000 -b-P4VP 13000 Micellar dispersion MS 11 ;

[0174] S4: In a two-electrode diaphragm electrolytic cell, a PVA hydrogel matrix is ​​sandwiched between the cells as a diaphragm. 5 mL of fully quaternized doped Ti3O5NPs PS is added to the anode. 50000 -b-P4VP 13000 Micellar dispersion MS 11 Add 5 mL of deionized water to the cathode and a small amount of sodium chloride solution to each electrode. Perform electric field grafting for 1 hour under an electric field strength of 30 V / cm to obtain ST. 19 -PVA-Ti2O3 hydrogel.

[0175] Example 20

[0176] This embodiment provides ST 20 The preparation method of -P(MAAm-co-MAAc) supramolecular hydrogel includes the following steps:

[0177] S1: Dissolve 3.064g MAAm, 7.231g MAAc and 0.162g potassium persulfate in 20mL of deionized water, purge with argon gas to remove oxygen for 10min, add 20μL of tetramethylethylenediamine (TEMDA), inject into a glass mold, and polymerize at room temperature for 24h to obtain P(MAAm-co-MAAc) supramolecular hydrogel matrix;

[0178] S2: Preparation of fully quaternized PS 50000 -b-P4VP 13000 Micellar dispersion MS1 ​​(same as Example 1);

[0179] S3: In a two-electrode membrane electrolytic cell, a P(MAAm-co-MAAc) supramolecular hydrogel matrix is ​​sandwiched in the middle of the electrolytic cell as a membrane, and 5 mL of fully quaternized PS is added to the anode. 50000 -b-P4VP 13000 Micelle dispersion MS1 ​​was prepared by adding 5 mL of deionized water to the cathode and a small amount of potassium sulfate solution to both electrodes. The mixture was then subjected to electric field grafting at an electric field strength of 15 V / cm for 1 hour to obtain ST. 20 -P(MAAm-co-MAAc) supramolecular hydrogel.

[0180] Example 21

[0181] This embodiment provides ST 21 The preparation method of (β-cyclodextrin / adamantane) supramolecular hydrogel includes the following steps:

[0182] S1: 0.2 g of methacrylamide-β-cyclodextrin (βCDAAmMe) and 33 mg of acrylamide-adamantane (AdAAm) were dissolved in 8 mL of water and stirred at 80 °C for 3 h to form a host-guest structure; 1.11 g of acrylamide was added at 25 °C, followed by 43 mg of potassium persulfate and 18.6 mg of tetramethylethylenediamine, and the reaction was carried out for 20 min to form a host-guest gel; the host-guest hydrogel was soaked in dimethyl sulfoxide for 72 h, and then soaked in water for 72 h to obtain the β-CD / Ad (β-cyclodextrin / adamantane) supramolecular hydrogel matrix;

[0183] S2: Preparation of fully quaternized PS 50000 -b-P4VP 13000 Micellar dispersion MS1 ​​(same as Example 1);

[0184] S3: In a two-electrode diaphragm electrolytic cell, a (β-cyclodextrin / adamantane) supramolecular hydrogel matrix is ​​sandwiched in the middle of the electrolytic cell as a diaphragm, and 5 mL of fully quaternized PS is added to the anode. 50000 -b-P4VP 13000 Micelle dispersion MS1 ​​was prepared by adding 5 mL of deionized water to the cathode and a small amount of potassium sulfate solution to both electrodes. The mixture was then subjected to electric field grafting at an electric field strength of 10 V / cm for 2 hours to obtain ST. 21 -(β-cyclodextrin / adamantane) supramolecular hydrogel.

[0185] Example 22

[0186] This embodiment provides ST 22 The preparation method of PVA hydrogel includes the following steps:

[0187] S1: Preparation of PVA hydrogel matrix (same as in Example 8);

[0188] S2: Add 5mg PS 30000 -b-PAA 8000 Dissolved in 5 mL of methanol, and then 9 mL of pure water was added dropwise at a rate of 4.5 mL / h to obtain a PS-b-PAA micelle dispersion MS with a core-shell structure. 12 The product was dialyzed in deionized water for at least 2 hours.

[0189] S3: In a two-electrode diaphragm electrolytic cell, a PVA hydrogel matrix is ​​sandwiched in the middle of the cell as a diaphragm. 5 mL of deionized water is added to the anode, and 5 mL of PS-b-PAA micelle dispersion with a core-shell structure is added to the cathode. 12A small amount of sodium sulfate solution was added to each electrode, and electric field grafting was performed for 2 hours under an electric field strength of 5 V / cm to obtain ST. 22 -PVA hydrogel.

[0190] Example 23

[0191] This embodiment provides ST 23 The preparation method of PVA hydrogel includes the following steps:

[0192] S1: Preparation of PVA hydrogel matrix (same as in Example 8);

[0193] S2: Add 5mg PAA 11000 -b-PHFBA 72000 Dissolved in 5 mL of methanol, and then 9 mL of pure water was added dropwise at a rate of 4.5 mL / h to obtain a PAA-b-PHFBA micelle dispersion with a core-shell structure (MS). 13 The product was dialyzed in deionized water for at least 2 hours.

[0194] S3: In a two-electrode diaphragm electrolytic cell, a PVA hydrogel matrix is ​​sandwiched in the middle of the cell as a diaphragm. 5 mL of deionized water is added to the anode, and 5 mL of PAA-b-PHFBA micelle dispersion with a core-shell structure is added to the cathode. 13 A small amount of potassium sulfate solution was added to both electrodes, and electric field grafting was performed for 1.5 hours under an electric field strength of 20 V / cm to obtain ST. 23 -PVA hydrogel.

[0195] Example 24

[0196] This embodiment provides ST 24 The preparation method of PVA hydrogel includes the following steps:

[0197] S1: Preparation of PVA hydrogel matrix (same as in Example 8);

[0198] S2: Add 5mg P4VP 18000 -b-PHFBA 50000 Dissolve in 5 mL of methanol and add 9 mL of pure water dropwise at a rate of 4.5 mL / h to obtain a P4VP-b-PHFBA micelle dispersion with a core-shell structure. Dialyze in deionized water for at least 2 h for later use.

[0199] S3: In the standby P4VP with a core-shell structure 18000 -b-PHFBA 50000 20 μL of 1-iodopropane was added to the micelle dispersion, and the reaction was carried out overnight at 45 °C. The reaction product was then dialyzed against deionized water for at least 2 h to obtain fully quaternized P4VP.18000 -b-PHFBA 50000 Micellar dispersion MS 14 ;

[0200] S4: In a two-electrode diaphragm electrolytic cell, a PVA hydrogel matrix is ​​sandwiched in the middle of the cell as a diaphragm. 5 mL of deionized water is added to the anode, and 5 mL of fully quaternized P4VP is added to the cathode. 18000 -b-PHFBA 50000 Micellar dispersion MS 14 A small amount of potassium chloride solution was added to each electrode, and electric field grafting was performed for 0.5 h under an electric field strength of 10 V / cm to obtain ST. 24 -PVA hydrogel.

[0201] Example 25

[0202] This embodiment provides ST 25 The preparation method of PVA hydrogel includes the following steps:

[0203] S1: Preparation of PVA-GO hydrogel matrix (same as in Example 2);

[0204] S2: Add 10g of acrylic acid, 3.64g of 2-[dodecylthio(thiocarbonyl)thio]-2-methylpropionic acid, 16.4mg of azobisisobutyronitrile and 20mL of 1,4-dioxane to a 50mL sealing tube. After three cycles of freezing-vacuuming-melting, seal the tube and react at 80℃ for 6 hours. Immerse the sealing tube in liquid nitrogen to terminate the reaction. Dilute with tetrahydrofuran, then precipitate in excess diethyl ether, filter, and vacuum dry to obtain polyacrylic acid chain transfer agent.

[0205] S3: Dissolve 1.0 g N-isopropylacrylamide, 20 mg N,N'-methylenebisacrylamide, 50 mg potassium persulfate, 80 mg polyacrylic acid chain transfer agent and 80 mg potassium carbonate in 50 mL of water, purge with argon gas to remove oxygen for 30 min, and react at 70 °C for 24 h to obtain negatively charged PAA-b-PNIPAM microgel with a polyelectrolyte shell, and dilute to 0.1 mg / mL for later use;

[0206] S4: In a two-electrode diaphragm electrolytic cell, a PVA-GO hydrogel matrix is ​​sandwiched in the middle of the cell as a diaphragm. 5 mL of deionized water is added to the anode, and 5 mL of negatively charged PAA-b-PNIPAM microgel with a polyelectrolyte shell is added to the cathode. A small amount of sodium chloride solution is added to both electrodes. Electric field grafting is performed for 0.5 h under an electric field strength of 10 V / cm to obtain ST. 25 -PVA-GO hydrogel.

[0207] Example 26

[0208] This embodiment provides ST 26 The preparation method of PVA-CB hydrogel includes the following steps:

[0209] S1: Preparation of PVA-CB hydrogel matrix (same as in Example 3);

[0210] S2: Add 10g N-isopropylacrylamide, 0.18g 2-[dodecylthio(thiocarbonyl)thio]-2-methylpropionic acid, 30.7mg azobisisobutyronitrile, 0.2g N,N'-methylenebisacrylamide and 20mL 1,4-dioxane to a 50mL sealing tube. After three cycles of freezing-vacuuming-melting, seal the tube and react at 70℃ for 24h. Immerse the sealing tube in liquid nitrogen to terminate the reaction. Dilute with tetrahydrofuran, then precipitate in excess diethyl ether. Filter and vacuum dry to obtain poly(N-isopropylacrylamide) chain transfer agent.

[0211] S3: Dissolve 3.0g of poly(N-isopropylacrylamide) chain transfer agent, 1.0g of 4-vinylpyridine and 10mg of azobisisobutyronitrile in 50mL of N,N-dimethylformamide, purge with argon gas for 30min, and react at 70℃ for 24h to obtain P4VP-b-PNIPAM microgel.

[0212] S4: Add 6 mL of bromoethane to P4VP-b-PNIPAM organic microgel and react overnight at 45°C to obtain fully quaternized P4VP-b-PNIPAM microgel. Dialyze in deionized water for 2 days, changing the water every 6 hours during the process, and then dilute to 0.1 mg / mL for later use.

[0213] S5: In a two-electrode diaphragm electrolytic cell, a PVA-CB hydrogel matrix is ​​sandwiched between the cells as a diaphragm. 5 mL of a fully quaternized P4VP-b-PNIPAM microgel solution is added to the anode, and 5 mL of deionized water is added to the cathode. A small amount of potassium chloride solution is added to both electrodes. Electric field grafting is performed for 1.5 h at an electric field strength of 10 V / cm to obtain ST. 26 -PVA-CB hydrogel.

[0214] To illustrate the practical effect of the preparation method of this application, comparative examples 1-4 will be designed using ST8-PVA hydrogel as the experimental sample, and tests will be conducted using the ST8-PVA hydrogel sample and the products prepared in comparative examples 1-4 as examples. The specific preparation methods for comparative examples 1-4 are as follows:

[0215] Comparative Example 1

[0216] The difference between it and Comparative Example 8 is that the modification operation of fully quaternizing PS-b-P4VP micelles with shell structure is omitted, and the remaining steps and treatments are the same as in Example 8.

[0217] The product is designated as ST. 8a -PVA hydrogel.

[0218] Comparative Example 2

[0219] The difference between it and Comparative Example 8 is that the quaternizing agent for the complete quaternization of PS-b-P4VP micelles with shell structure is 1-iodobutane, and the remaining steps and treatments are the same as in Example 8.

[0220] The product is designated as ST. 8b -PVA hydrogel.

[0221] Comparative Example 3

[0222] The difference between it and Comparative Example 8 is that the quaternizing agent for the complete quaternization of PS-b-P4VP micelles with shell structure is 1-bromopentane, and the remaining steps and treatments are the same as in Example 8.

[0223] The product is designated as ST. 8c -PVA hydrogel.

[0224] Comparative Example 4

[0225] The difference between it and Comparative Example 8 is that the quaternizing agent for the complete quaternization of PS-b-P4VP micelles with shell structure is benzyl bromide, and the remaining steps and treatments are the same as in Example 8.

[0226] The product is designated as ST. 8d -PVA hydrogel.

[0227] The ST8-PVA hydrogel sample was characterized by SEM, and the results were as follows: Figure 1 As shown. Among them, Figure 1 This is a SEM image of the ST8-PVA hydrogel sample.

[0228] according to Figure 1 It can be seen that after the PVA hydrogel matrix is ​​modified by electric field grafting, PS is uniformly distributed on the surface of the PVA hydrogel matrix. 50000 -b-P4VP 13000 Micelles demonstrate that electric field grafting can achieve precise and stable surface modification of PVA hydrogel matrices.

[0229] Figure 2 For PS 50000 -b-P4VP 13000 - Confocal microscopy image of a PVA hydrogel with Nile red core-shell micelles. Among them, PS 50000-b-P4VP 13000 - Methods for preparing Nile red core-shell micelles include:

[0230] In the preparation of PS with core-shell structure 50000 -b-P4VP 13000 When dispersing in micelles, add PS to the solution. 50000 -b-P4VP 13000 Nile red fluorescent dye was added to DMF to obtain PS with a core-shell structure. 50000 -b-P4VP 13000 -Nile red core shell micelles.

[0231] according to Figure 2 It can be seen that after electric field grafting, PS with a core-shell structure 50000 -b-P4VP 13000 - Nile red core-shell micelles are concentrated on the surface of the PVA hydrogel matrix and will not affect the PVA hydrogel matrix.

[0232] The coverage of micelles on the hydrogel surface was calculated based on XPS (X-ray photoelectron spectroscopy).

[0233] XPS tests were performed on the surface portion of the PVA hydrogel after surface modification by grafting with an electric field of 10V / cm. The measured data are shown in Table 1 below.

[0234] Table 1 - Micellar Coverage at Different Grafting Times

[0235]

[0236] Table 1 shows that nitrogen is present on the surface of the PVA hydrogel matrix, which originates from fully quaternized PS. 50000 -b-P4VP 13000 The pyridine groups in the micelles demonstrate the presence of fully quaternized PS on the surface of the PVA hydrogel matrix. 50000 -b-P4VP 13000 Micelles. When the electric field strength is fixed at 10V / cm, the nitrogen-carbon ratio and the coverage of micelles on the hydrogel surface continuously increase, and basically reach saturation after 1.5h.

[0237] Evaporation rate test

[0238] The hydrogels prepared in Examples 1-26 and Comparative Examples 1-4 were cut to suitable sizes, fixed onto containers filled with artificial seawater, and connected with cotton thread to obtain a solar water evaporator. The resulting solar evaporator was placed under a solar lamp, and the mass change over 1 hour was measured. The evaporation rate of the solar water evaporator was calculated, and the results are shown in Table 2. Figure 3 The above. Among them, Figure 3ST1-PVA-Ti3O5 hydrogel, ST2-PVA-GO hydrogel, ST4-PVA-Ti2O3 hydrogel, ST7-PHEMA hydrogel, ST 18 -PVA-Ti2O3 hydrogel and ST 19 - Evaporation rate data of PVA hydrogel.

[0239] Table 2 - Evaporation rates of solar water evaporators based on hydrogels of Examples 1-26 and Comparative Examples 1-4

[0240]

[0241]

[0242] From the table above and Figure 3 It can be seen that surface modification with charged nanoparticles grafted onto the hydrogel using an electric field increases the evaporation rate by 15% to 64%, with the highest evaporation rate reaching 6.92 kg / m³. 2 / h, demonstrating that surface modification using the electric field grafting charged nanoparticle physical method significantly improves the evaporation rate of solar hydrogel evaporators.

[0243] The various embodiments in this specification are described in a progressive manner. The same or similar parts between the various embodiments can be referred to each other. Each embodiment focuses on describing the differences from other embodiments.

[0244] The above embodiments are only used to illustrate the technical solutions of this application, and are not intended to limit this application. Although this application has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features therein. Such modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of this application.

Claims

1. A method for preparing a modified hydrogel for achieving a high solar water evaporation rate, characterized in that, Includes the following steps: Preparation of charged nanoparticles; The charged nanoparticles are grafted onto the surface of a solar water evaporation gel under the action of a DC electric field to obtain a modified hydrogel with a high solar water evaporation rate. The charged nanoparticles include one of the following: core-shell micelles with a polyelectrolyte shell, core-shell composite microgels with a polyelectrolyte shell, and core-shell composite metal inorganic nanoparticles with a polyelectrolyte shell. The shell layer is a core-shell micelle of a polyelectrolyte, including polystyrene. b -Polyacrylate core-shell micelles, polyhexamethylene acrylate- b -Polyacrylic acid core-shell micelles, fully quaternized polystyrene- b -Poly(4-vinylpyridine) core-shell micelles, fully quaternized polyhexafluorobutyl acrylate- b - Poly(4-vinylpyridine) core-shell micelles; The shell layer is a core-shell composite microgel of polyelectrolytes, including polyacrylic acid- b -gathering( N -Isopropylacrylamide) microgel, fully quaternized poly(4-vinylpyridine)- b -gathering( N -Isopropylacrylamide) microgel; The core-shell composite metal inorganic nanoparticles with a polyelectrolyte shell include gold nanoparticles with polyacrylic acid or fully quaternized poly(4-vinylpyridine) grafted onto their surface, and titanium pentoxide nanoparticles with polyacrylic acid or fully quaternized poly(4-vinylpyridine) grafted onto their surface.

2. The preparation method according to claim 1, characterized in that, The process of grafting the charged nanoparticles onto the surface of a solar-powered water evaporation gel under the influence of a direct current electric field includes: In a two-electrode membrane electrolytic cell system, the solar water evaporation gel is used as a membrane, and charged nanoparticles and salt solution are added for DC electric field grafting treatment. The salt solution includes sodium salt solution and potassium salt solution.

3. The preparation method according to claim 2, characterized in that, The electric field strength of the DC electric field grafting treatment is 5~30V / cm, and the time is 0.5~2h.

4. The preparation method according to claim 1, characterized in that, The polystyrene block or the polyhexafluorobutyl acrylate block is also doped with photothermal particles.

5. The preparation method according to claim 1, characterized in that, The fully quaternized polystyrene- b Methods for preparing poly(4-vinylpyridine) core-shell micelles include: Provide polystyrene - b Core-shell micelles of poly(4-vinylpyridine) block copolymers; Make the polystyrene- b - Poly(4-vinylpyridine) block copolymer core-shell micelles with quaternizing agents in N,N The complete quaternization reaction occurs in a co-solvent of dimethylformamide and methanol. The reaction product is then dialyzed against deionized water, and the fully quaternized polystyrene is collected. b A dispersion of poly(4-vinylpyridine) block copolymer core-shell micelles in water.

6. The preparation method according to claim 5, characterized in that, The quaternizing agent includes halogenated aromatic hydrocarbons or halogenated alkanes with 1-5 carbon atoms; The haloaromatic hydrocarbons include benzyl bromide and p-methylbenzyl bromide; The haloalkanes with 1-5 carbon atoms include iodomethane, iodoethane, 1-iodopropane, 1-iodobutane, 1-iodopentane, bromomethane, and bromoethane.

7. The preparation method according to claim 5, characterized in that, The polystyrene- b When poly(4-vinylpyridine) core-shell micelles undergo complete quaternization with the quaternizing agent, the molar ratio of the quaternizing agent to the pyridine groups in the polystyrene-poly(4-vinylpyridine) block copolymer is greater than 10:

1.

8. The preparation method according to any one of claims 1 to 7, characterized in that, The solar-powered water evaporation gel includes polymer hydrogels and supramolecular hydrogels; The polymer hydrogels include polyvinyl alcohol hydrogel, polyacrylamide hydrogel, poly(2-hydroxyethyl methacrylate) hydrogel, polyacrylamide / agarose dual-network hydrogel, polyacrylamide / calcium alginate dual-network hydrogel, and polyethylene glycol hydrogel. The supramolecular hydrogels include cyclodextrin hydrogels and poly(methacrylamide-) co 2-Methacrylic acid) hydrogel.

9. The preparation method according to claim 8, characterized in that, The polymer hydrogel is also doped with photothermal particles; The photothermal particles include titanium pentoxide nanoparticles, titanium trioxide nanoparticles, gold nanoparticles, graphene, and conductive carbon black.

10. A modified hydrogel with a high solar water evaporation rate, characterized in that, Prepared according to any one of claims 1 to 9.

11. A solar water evaporator, comprising a solar water evaporator body and a solar water evaporation component disposed at the outlet of the solar water evaporator body, characterized in that, The solar water evaporation module is prepared using the modified hydrogel with a high solar water evaporation rate as described in claim 10.

Citation Information

Patent Citations

  • Method and device for preparing hydrogel-based composite material under driving of electric field

    CN111841468A

  • Integrated multifunctional solar evaporator and preparation method thereof

    CN117209000A