A method for preparing low-temperature metal ion-doped silver-zinc oxide electrical contact material

By doping low electronegativity metal ions into the silver-zinc oxide electrical contact material and combining it with a high-speed pulverization process, the problems of easy agglomeration and poor dispersibility of ZnO in the Ag matrix are solved, achieving the effects of low temperature rise and low contact resistance, which is suitable for high-current charging in the new energy field.

CN118241067BActive Publication Date: 2026-11-17HARBIN INST OF TECH +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410334826.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-22
Publication Date
2026-11-17
Estimated Expiration
2044-03-22

AI Technical Summary

Technical Problem

Existing silver-zinc oxide electrical contact materials experience temperature rise and unstable contact resistance during service. This is mainly due to the tendency of ZnO to agglomerate and its poor dispersion in the Ag matrix, resulting in high resistivity, which cannot meet the high-current charging requirements of the new energy field.

Method used

A composite process combining solid-state sintering and high-speed pulverization was employed to improve the conductivity and dispersibility of ZnO by doping with low electronegativity metal ions (such as potassium oxide, copper oxide, and aluminum oxide), and to enhance interfacial bonding by combining high-speed pulverization, thus preparing a low-temperature-rise silver-zinc oxide electrical contact material.

Benefits of technology

It significantly reduces the temperature rise and contact resistance of silver-zinc oxide electrical contact materials, improves the conductivity and stability of the materials, and meets the requirements of high-current charging in the new energy field.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118241067B_ABST
    Figure CN118241067B_ABST
Patent Text Reader

Abstract

A method for preparing a low-temperature-rise metal ion-doped silver-zinc oxide electrical contact material is disclosed, relating to a method for preparing electrical contact materials. This invention aims to solve the technical problem of temperature rise during service of existing silver oxide electrical contact materials. This invention employs a high-temperature solid-state method to prepare metal ion-doped zinc oxide powder. The zinc oxide powder doped with metal ions is mixed with silver powder at high speed to obtain a mixed powder; the mixed powder is initially pressed to obtain a billet; the billet is hot-extruded to obtain a sheet; rolling annealing; and stamping blanking to obtain the contact point. In this invention, metal ion doping can reduce the resistivity of zinc oxide powder, and combined with high-speed stirring of the mixed powder, it ensures efficient densification of the material, improves the dispersibility of zinc oxide powder in the silver matrix, reduces the resistivity of the zinc oxide electrical contact material, and thus reduces the temperature rise and contact resistance during service. This invention is applicable to the preparation of silver-zinc oxide electrical contact materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a method for preparing an electrical contact material. Background Technology

[0002] In recent years, the new energy sector has developed rapidly. Taking new energy vehicles as an example, to meet the requirements of short charging times and long battery lifespans for a large number of vehicles, high-current charging has become an industry development goal. However, high-current charging increases the temperature rise of supporting electrical appliances, shortens their lifespan, and can even cause safety issues such as fires. As an indispensable part of low-voltage electrical appliances, electrical contact materials are mainly responsible for switching circuits, and their performance directly affects the reliability and lifespan of electrical appliances. Temperature rise is directly related to contact resistance. Therefore, developing new contact materials for low-voltage contactors with low temperature rise and stable contact resistance is an urgent need for the continued development of the power electrical appliance industry.

[0003] Silver-based electrical contact materials are most widely used in low-voltage electrical appliances. Among silver-based electrical contact materials, Ag / CdO has excellent overall performance and low cost, making it the most widely used in low-voltage electrical appliances. It has excellent electrical and thermal conductivity, low and stable contact resistance, and low temperature rise. However, because cadmium oxide decomposes to produce toxic cadmium vapor, which is harmful to the environment and human health, Western countries have explicitly banned the use of Cd in electronic and electrical equipment. Ag / SnO2In2O3 contact materials are widely used due to their significant resistance to arc erosion and low material transfer characteristics, but their high cost and limited supply restrict their development in the field of low temperature rise. Ag / ZnO is a typical Ag / MeO contact material. ZnO has a high melting point and is more stable at high arc temperatures, thus it is widely used in various levels of circuit breaking applications. At the same time, Ag / ZnO electrical contact materials also have a series of advantages such as low cost and non-toxicity. Therefore, Ag / ZnO, as an environmentally friendly electrical contact material, is expected to replace Ag / CdO electrical contact materials in the new energy industry and be widely used in low-voltage electrical appliances. However, due to the poor conductivity of zinc oxide and its tendency to agglomerate and accumulate in the Ag matrix, it can lead to problems such as high temperature rise and short electrical life during service.

[0004] Currently, the main methods for preparing zinc oxide silver are traditional powder metallurgy, internal oxidation, and high-energy ball milling. Due to the tendency of zinc oxide to agglomerate, the second phase of the prepared zinc oxide silver electrical contact material has poor dispersion, which seriously restricts the electrical contact performance of the composite material. The main reasons are as follows: (1) For powder metallurgy, when the wettability between the two phases is poor, the second phase of the material and the matrix have poor interfacial bonding, which makes it difficult to densify the material. Excessive porosity will hinder the transfer of free electrons, resulting in high resistivity of the material itself. (2) Due to the poor conductivity of ZnO, which is 8 orders of magnitude different from that of Ag matrix, coarse oxide particles will directly lead to unstable contact resistance. (3) Due to the tendency of ZnO to agglomerate on the surface of Ag matrix, the probability of coarse oxide particles coming into contact during service increases, which will directly lead to excessively high contact resistance, resulting in excessive temperature rise.

[0005] Wettability is essentially the strength of the bonding between two phase interfaces. If the wettability is poor, defects such as pores will remain after sintering due to the poor bonding between heterogeneous phase interfaces, reducing the density. However, metal ion doping enhances the semiconductor properties of ZnO:M, thereby increasing the charge transfer at the Ag-ZnO:M interface. Ag-O or Ag-M bonds are easily formed at the interface, resulting in stronger interfacial bonding ability and exhibiting superior wettability, which in turn increases the density. The connection between particles becomes tighter, thereby reducing the resistance to electron transport. A continuous silver network is formed inside the material, which ensures the smooth migration of electrons and gives the material good electrical conductivity. Because ZnO has intrinsic donor defects, it exhibits weak n-type conductivity and generally has a high resistivity. However, metal doping can change the carrier type and concentration of ZnO:M, thereby forming an n-type or p-type semiconductor and improving its conductivity. Low electronegativity metal ion doping can enhance the p-type semiconductor characteristics of ZnO:M, reduce the adsorption capacity of ZnO powder for atmospheric hydroxyl groups, reduce its agglomeration size and intensity, and inhibit the agglomeration behavior of ZnO. This results in uniform dispersion of ZnO in the silver matrix, reducing the probability of oxide particle contact during service, thereby reducing contact resistance and temperature rise during service and improving the electrical contact life of silver-zinc oxide composite materials. Summary of the Invention

[0006] The present invention aims to solve the technical problem of temperature rise in existing silver oxide electrical contact materials during service, and proposes a method for preparing low-temperature-rise metal ion-doped silver oxide zinc electrical contact materials.

[0007] The method for preparing the low-temperature rise metal ion-doped silver-zinc oxide electrical contact material of the present invention is carried out according to the following steps:

[0008] I. Preparation of metal ion-doped zinc oxide powder by solid-state sintering: Water, zinc oxide powder and oxide powder are placed together in a ball mill jar for high-energy ball milling and mixing. The ball milling speed is 200 rpm to 550 rpm and the ball milling time is 2 h to 10 h. After ball milling, the mixed powder is placed in a muffle furnace and heat-treated at 800℃ to 1500℃ for 4 h to obtain doped oxide powder.

[0009] The oxide powder is potassium oxide powder, copper oxide powder, or aluminum oxide powder;

[0010] The doping ratio of potassium, copper, or aluminum in the doped oxide powder is 0.5 wt% to 10 wt%.

[0011] II. The doped oxide powder prepared in step one and elemental silver powder are mixed using a tissue homogenizer, wherein the mass percentage of the doped oxide powder prepared in step one is 12%~20%. The specific mixing process is as follows:

[0012] ① The rotation speed is 15000r / min~20000r / min, the medium is deionized water or anhydrous ethanol, mix for 1min~1.5min, and then let stand for 2min~3min;

[0013] ② Repeat the process described in ① 2 to 5 times, and then use a water bath to dry and evaporate the liquid;

[0014] Third, the mixed powder dried in step two is subjected to initial pressing to obtain a blank; the initial pressing process is as follows: the mixed powder is pressed into a blank by a cold isostatic press at a pressure of 150MPa~350MPa, and the holding time is 60s~70s.

[0015] 4. The billet prepared in step 3 is hot-extruded to obtain a sheet with a thickness of 2mm~3mm; the hot extrusion process is as follows: the extrusion cylinder and the die are heated to 300℃~600℃, the billet is preheated to 750℃~950℃, and placed in the die, with an extrusion ratio of 20~30.

[0016] 5. Roll the sheet material from step 4 using a rolling mill, with a reduction of 0.2mm~0.5mm per pass, to produce a sheet material with a thickness of 0.5~1.5mm; then anneal it at 600℃~800℃ for 0.5h~2h.

[0017] 6. Use a blanking press to blank the sheet metal obtained in step 5 to obtain the contact points.

[0018] The principle and beneficial effects of this invention are as follows:

[0019] This invention employs a composite process combining solid-state sintering and high-speed pulverization to achieve uniform dispersion of metal ion-doped modified zinc oxide phase in a silver matrix and to regulate the microstructure and properties of the composite material. Specifically, solid-state sintering enables the synthesis of metal ion-doped zinc oxide powder. The doping of metal ions improves the conductivity of the zinc oxide powder, and the low electronegativity of the metal ions inhibits the agglomeration of the zinc oxide powder in the silver matrix, improving the dispersion of the second phase and enhancing the interfacial bonding between the second phase and the matrix.

[0020] The mechanism by which the above-mentioned beneficial effects are formed is as follows:

[0021] 1. Because ZnO has intrinsic donor defects, it exhibits weak n-type conductivity and generally has high resistivity. However, metal doping can change the carrier type of ZnO:M, forming an n-type or p-type semiconductor, thereby increasing its conductivity by increasing the carrier concentration.

[0022] 2. Doping with low electronegativity elements can enhance the p-type semiconductor properties of ZnO:M, reduce the adsorption capacity of ZnO powder for atmospheric hydroxyl groups, reduce its agglomeration size and agglomeration intensity, and inhibit the agglomeration behavior of ZnO.

[0023] 3. Metal ion doping enhances the semiconductor properties of ZnO:M, thereby increasing the charge transfer at the Ag-ZnO:M interface. This facilitates the formation of Ag-O or Ag-M bonds at the interface, resulting in stronger interfacial bonding and superior wettability. Combined with high-speed pulverization, this ensures efficient material densification, resulting in tighter particle connections and smooth electron migration. It also reduces the resistivity of zinc oxide powder, improving second-phase dispersion and thus lowering the temperature rise of the contact material during low-voltage electrical appliance operation. This breaks through the electrical contact performance barriers of silver-zinc oxide materials, meeting the requirements of low-voltage, high-current electrical appliances for low temperature rise and low, stable contact resistance. Attached Figure Description

[0024] Figure 1 The XRD pattern is obtained from a fast scan.

[0025] Figure 2 The XRD pattern is obtained from a slow scan.

[0026] Figure 3 SEM images of the materials at the four contact points. Detailed Implementation

[0027] Specific Implementation Method 1: This implementation method is a method for preparing a low-temperature-rise metal ion-doped silver-zinc oxide electrical contact material, specifically carried out according to the following steps:

[0028] I. Preparation of metal ion-doped zinc oxide powder by solid-state sintering: Water, zinc oxide powder and oxide powder are placed together in a ball mill jar for high-energy ball milling and mixing. The ball milling speed is 200 rpm to 550 rpm and the ball milling time is 2 h to 10 h. After ball milling, the mixed powder is placed in a muffle furnace and heat-treated at 800℃ to 1500℃ for 4 h to obtain doped oxide powder.

[0029] The oxide powder is potassium oxide powder, copper oxide powder, or aluminum oxide powder;

[0030] The doping ratio of potassium, copper, or aluminum in the doped oxide powder is 0.5 wt% to 10 wt%.

[0031] II. The doped oxide powder prepared in step one and elemental silver powder are mixed using a tissue homogenizer, wherein the mass percentage of the doped oxide powder prepared in step one is 12%~20%. The specific mixing process is as follows:

[0032] ① The rotation speed is 15000r / min~20000r / min, the medium is deionized water or anhydrous ethanol, mix for 1min~1.5min, and then let stand for 2min~3min;

[0033] ② Repeat the process described in ① 2 to 5 times, and then use a water bath to dry and evaporate the liquid;

[0034] Third, the mixed powder dried in step two is subjected to initial pressing to obtain a blank; the initial pressing process is as follows: the mixed powder is pressed into a blank by a cold isostatic press at a pressure of 150MPa~350MPa, and the holding time is 60s~70s.

[0035] 4. The billet prepared in step 3 is hot-extruded to obtain a sheet with a thickness of 2mm~3mm; the hot extrusion process is as follows: the extrusion cylinder and the die are heated to 300℃~600℃, the billet is preheated to 750℃~950℃, and placed in the die, with an extrusion ratio of 20~30.

[0036] 5. Roll the sheet material from step 4 using a rolling mill, with a reduction of 0.2mm~0.5mm per pass, to produce a sheet material with a thickness of 0.5~1.5mm; then anneal it at 600℃~800℃ for 0.5h~2h.

[0037] 6. Use a blanking press to blank the sheet metal obtained in step 5 to obtain the contact points.

[0038] Specific Implementation Method Two: This implementation method differs from Specific Implementation Method One in that the mass ratio of balls to material during ball milling in step one is (1~10):1, and the balls are zirconia balls. Everything else is the same as in Specific Implementation Method One.

[0039] Specific Implementation Method 3: This implementation method differs from Specific Implementation Method 2 in that the zirconia spheres mentioned in step one are divided into large spheres, medium spheres, and small spheres according to their size, and the mass ratio of the three is 1:2:2; the diameters of the large, medium, and small spheres are 10mm, 5mm, and 2mm, respectively. Everything else is the same as in Specific Implementation Method 2.

[0040] Specific Implementation Method Four: This implementation method differs from one of Specific Implementation Methods One to Three in that the rotational speed in step two① is 18000 r / min. Everything else is the same as in one of Specific Implementation Methods One to Three.

[0041] Specific Implementation Method Five: This implementation method differs from Specific Implementation Method Four in that: in step two, a tissue pulverizer is used to mix the doped oxide powder prepared in step one with elemental silver powder, wherein the mass percentage of the doped oxide powder prepared in step one is 15%. Everything else is the same as in Specific Implementation Method Four.

[0042] Specific Implementation Method Six: This implementation method differs from Specific Implementation Method Five in that: in step three, the mixed powder is pressed into a blank at a pressure of 150 MPa, and the holding time is 60 seconds. Everything else is the same as in Specific Implementation Method Five.

[0043] Specific Implementation Method Seven: This implementation method differs from Specific Implementation Method Six in that the extrusion ratio in step four is 25. Everything else is the same as in Specific Implementation Method Six.

[0044] Specific Implementation Method Eight: This implementation method differs from Specific Implementation Method Seven in that the billet is preheated to 850°C in step four. Everything else is the same as in Specific Implementation Method Seven.

[0045] Specific Implementation Method Nine: This implementation method differs from Specific Implementation Method Eight in that both the extrusion cylinder and the mold are heated to 500°C in step four. Everything else is the same as in Specific Implementation Method Eight.

[0046] Specific Implementation Method Ten: This implementation method differs from Specific Implementation Method Nine in that annealing is performed at 800℃ for 2 hours in step five. Everything else is the same as in Specific Implementation Method Nine.

[0047] The invention was verified using the following experiments:

[0048] Experiment 1: This experiment demonstrates a method for preparing a low-temperature-rise metal ion-doped silver-zinc oxide electrical contact material, specifically carried out according to the following steps:

[0049] I. Preparation of metal ion-doped zinc oxide powder by solid-state sintering: Water, zinc oxide powder and potassium oxide powder were placed together in a ball mill jar and mixed by high-energy ball milling at a speed of 500 rpm for 4 hours. After ball milling, the mixed powder was placed in a muffle furnace and heat-treated at 1200℃ for 4 hours to obtain ZnO:K powder.

[0050] The potassium content in the ZnO:K powder is 1.5 wt%.

[0051] During ball milling, the mass ratio of balls to material is (1~10):1. The balls are zirconia balls, which are divided into large balls, medium balls and small balls according to their size, and the mass ratio of the three is 1:2:2. The diameters of the large balls, medium balls and small balls are 10mm, 5mm and 2mm respectively.

[0052] II. The ZnO:K powder prepared in step one and elemental silver powder are mixed using a tissue homogenizer. The ZnO:K powder accounts for 15% of the total mass. The specific mixing process is as follows:

[0053] ① The rotation speed is 18000 r / min, the medium is deionized water. Since a lot of heat will be generated during the high-speed mixing process, mix for 1 minute each time, and then let it stand for 2 minutes.

[0054] ② Repeat the process described in ① five times, and then use a water bath to dry and evaporate the liquid;

[0055] Third, the mixed powder dried in step two is subjected to initial pressing to obtain a blank; the initial pressing process is as follows: the mixed powder is pressed into a blank by a cold isostatic press at a pressure of 150MPa and the holding time is 60s.

[0056] 4. The billet prepared in step 3 is hot-extruded to obtain a sheet with a thickness of 2.5 mm. The hot extrusion process is as follows: the extrusion cylinder and the die are heated to 500°C, the billet is preheated to 850°C, and placed in the die. The extrusion ratio is 25.

[0057] 5. Roll the sheet material from step 4 using a rolling mill, with a reduction of 0.3 mm per pass, to produce a sheet material with a thickness of 1.5 mm; then anneal it at 800℃ for 2 hours.

[0058] 6. The sheet material obtained in step 5 is stamped and blanked using a stamping blanking machine to obtain contact material Ag / ZnO:K. The contact material is circular with a diameter of 10mm.

[0059] Comparative Example 1:

[0060] 1. Mixing zinc oxide powder and silver powder using a tissue crusher

[0061] Zinc oxide powder and elemental silver powder were mixed using a tissue homogenizer, with the zinc oxide powder content being 12 wt.%. The rotation speed was set to 18000 r / min, and each mixing cycle lasted 1 min, followed by a 2-min rest period before mixing continued, for a total of 5 mixing cycles. The mixing machine was manually turned several times during the mixing process to promote uniform mixing.

[0062] II. Obtaining a blank from the initial pressing and mixing of powders

[0063] The billet was obtained by pressing with a cold isostatic press. The initial pressing was carried out at a pressure of 150 MPa to press the above mixed powder into a billet, and the holding time was 60 s.

[0064] III. Hot extrusion of billets to obtain sheet metal

[0065] Hot extrusion is used to extrude the billet into a sheet with an extrusion ratio of 25. The billet is preheated to 750°C, and the extrusion cylinder and die are heated to 500°C to obtain a sheet with a thickness of 2.5 mm.

[0066] IV. Rolling Annealing

[0067] The sheet metal was rolled into a 1.5mm thick sheet using a rolling mill, with a reduction of 0.3mm per pass; then annealed at 800℃ for 2 hours.

[0068] V. Stamping and blanking

[0069] A stamping blanking machine is used to cut the sheet metal into contact material Ag / ZnO, and the contact is circular with a diameter of 10mm.

[0070] Comparative Example 2:

[0071] 1. A crusher is used to mix tin dioxide powder, indium oxide powder, and elemental silver powder.

[0072] According to the current formula for AgSnO2(10)In2O3(5) used in low-temperature rise AC contactors, tin dioxide powder, indium oxide powder and elemental silver powder were mixed using a tissue crusher. The content of tin dioxide powder was 10 wt.% and the content of indium oxide was 5 wt.%. The rotation speed was set to 18000 r / min. Each mixing session lasted 1 min, followed by a 2-min rest period before mixing was repeated 5 times. The powder mixer was manually turned over several times during mixing to promote uniform mixing.

[0073] II. Obtaining a blank from the initial pressing and mixing of powders

[0074] The billet was obtained by pressing with a cold isostatic press. The initial pressing was carried out at a pressure of 150 MPa to press the above mixed powder into a billet, and the holding time was 60 s.

[0075] III. Hot extrusion of billets to obtain sheet metal

[0076] Hot extrusion is used to extrude the billet into a sheet with an extrusion ratio of 25. The billet is preheated to 750°C, and the extrusion cylinder and die are heated to 500°C to obtain a sheet with a thickness of 2.5 mm.

[0077] IV. Rolling Annealing

[0078] The sheet metal was rolled into a 1.5mm thick sheet using a rolling mill, with a reduction of 0.3mm per pass; then annealed at 800℃ for 2 hours.

[0079] V. Stamping and blanking

[0080] A stamping blanking machine is used to cut the sheet into contact material Ag / SnO2In2O3, and the contact is circular with a diameter of 10mm.

[0081] Comparative Example 3:

[0082] 1. Mixing cadmium oxide powder and silver powder using a tissue crusher

[0083] According to the current formula of AgCdO (15) for low-temperature rise AC contactors, cadmium oxide powder and elemental silver powder are mixed using a tissue crusher. The content of cadmium oxide powder is 15wt.%, the speed is set to 18000r / min, each mixing is 1min, and after standing for 2min, the mixing is continued. The mixing is repeated 5 times in total. The powder mixer is manually turned over many times during the mixing process to promote uniform mixing.

[0084] II. Obtaining a blank from the initial pressing and mixing of powders

[0085] The billet was obtained by pressing with a cold isostatic press. The initial pressing was carried out at a pressure of 150 MPa to press the above mixed powder into a billet, and the holding time was 60 s.

[0086] III. Hot extrusion of billets to obtain sheet metal

[0087] Hot extrusion is used to extrude the billet into a sheet with an extrusion ratio of 25. The billet is preheated to 750°C, and the extrusion cylinder and die are heated to 500°C to obtain a sheet with a thickness of 2.5 mm.

[0088] IV. Rolling Annealing

[0089] The sheet metal was rolled into a 1.5mm thick sheet using a rolling mill, with a reduction of 0.3mm per pass; then annealed at 800℃ for 2 hours.

[0090] V. Stamping and blanking

[0091] A stamping blanking machine is used to cut the sheet into contact material Ag / CdO, and the contact is circular with a diameter of 10mm.

[0092] The following comparative experiments were conducted on the contact elements prepared by Experiment 1 (Ag / ZnO:K) and the three comparative examples (Ag / ZnO, Ag / SnO2In2O3, and Ag / CdO), respectively:

[0093] The four contact materials prepared above were subjected to metallographic and polishing treatments, and then characterized by SEM. The results are as follows. Figure 3 As shown, comparing the SEM results of Ag / ZnO:K and Ag / ZnO reveals that: K + Doping significantly alleviates the agglomeration characteristics of ZnO, thereby improving the dispersion of the second phase in the Ag matrix. The dispersion of oxides in AgSnO2In2O3 and AgCdO is relatively good.

[0094] The application specifications of contact materials are closely related to the structure of electrical appliances. Therefore, type testing after installation in the electrical appliance is a key method for evaluating the quality of contact materials. According to GB / T10963.1-2020 requirements for the temperature rise performance of circuit breakers, the temperature rise of the terminals connected to external conductors should not exceed 60K to ensure the normal operation of the circuit breaker is not damaged. The four prepared φ10mm contacts were welded onto the contact base and measured using an NXC-100 AC contactor type tester (380V-100A-3h). Each test was conducted for 3 hours. After temperature rise and contact resistance tests, the contact resistance R and temperature rise ΔT of different materials were compared. The data listed in Table 1 are the average values ​​of 5 to 10 measurements.

[0095] Table 1

[0096]

[0097] Table 1 shows the results of temperature rise type tests using an NXC-100 AC contactor, indicating that potassium ion doping effectively reduces the contact resistance and temperature rise of the electrical contact material. The Ag / ZnO electrical contact material, by doping with low electronegativity metal ions, improves the conductivity of ZnO, enhances the dispersion of ZnO in the Ag matrix, reduces the probability of oxide phase contact during the temperature rise test, and increases density, thereby reducing the temperature rise and contact resistance of the Ag / ZnO electrical contact material. Therefore, compared with existing methods, the method of this invention can effectively reduce the contact resistance and temperature rise of electrical contact materials, improving the reliability and durability of electrical switch contacts in the new energy field.

[0098] Figure 1 The XRD patterns are obtained by fast scanning, corresponding to Experiment 1 and Comparative Example 1, respectively. It can be seen that the diffraction peaks of the powders prepared in the two experiments are the same as the standard diffraction peaks of ZnO, indicating that the two products have high purity and are free of impurities.

[0099] Figure 2The XRD patterns are slow scans, corresponding to Experiment 1 and Comparative Example 1, respectively, indicating that Experiment 1 successfully prepared high-purity potassium ion-doped ZnO powder.

Claims

1. A method for preparing a low-temperature-rise metal ion-doped silver-zinc oxide electrical contact material, characterized in that... The preparation method of low-temperature rise metal ion-doped silver-zinc oxide electrical contact material is carried out according to the following steps: I. Preparation of metal ion-doped zinc oxide powder by solid-state sintering: Water, zinc oxide powder and oxide powder are placed together in a ball mill jar for high-energy ball milling and mixing. The ball milling speed is 200 rpm to 550 rpm and the ball milling time is 2 h to 10 h. After ball milling, the mixed powder is placed in a muffle furnace and heat-treated at 800℃ to 1500℃ for 4 h to obtain doped oxide powder. The oxide powder is potassium oxide powder, copper oxide powder, or aluminum oxide powder; The doping ratio of potassium, copper, or aluminum in the doped oxide powder is 0.5 wt% to 10 wt%. II. The doped oxide powder prepared in step one and elemental silver powder are mixed using a tissue homogenizer, wherein the mass percentage of the doped oxide powder prepared in step one is 12%~20%. The specific mixing process is as follows: ① The rotation speed is 15000r / min~20000r / min, the medium is deionized water or anhydrous ethanol, mix for 1min~1.5min, and then let stand for 2min~3min; ② Repeat the process described in ① 2 to 5 times, and then use a water bath to dry and evaporate the liquid; Third, the mixed powder dried in step two is subjected to initial pressing to obtain a blank; the initial pressing process is as follows: the mixed powder is pressed into a blank by a cold isostatic press at a pressure of 150MPa~350MPa, and the holding time is 60s~70s.

4. The billet prepared in step 3 is hot-extruded to obtain a sheet with a thickness of 2mm~3mm; the hot extrusion process is as follows: the extrusion cylinder and the die are heated to 300℃~600℃, the billet is preheated to 750℃~950℃, and placed in the die, with an extrusion ratio of 20~30.

5. Roll the sheet material from step 4 using a rolling mill, with a reduction of 0.2mm~0.5mm per pass, to produce a sheet material with a thickness of 0.5~1.5mm; then anneal it at 600℃~800℃ for 0.5h~2h.

6. Use a blanking press to blank the sheet metal obtained in step 5 to obtain the contact points.

2. The method for preparing a low-temperature-rise metal ion-doped silver-zinc oxide electrical contact material according to claim 1, characterized in that... In step one, during ball milling, the mass ratio of balls to material is (1~10):1, and the balls are zirconia balls.

3. The method for preparing a low-temperature-rise metal ion-doped silver-zinc oxide electrical contact material according to claim 2, characterized in that... The zirconia spheres mentioned in step one are divided into large spheres, medium spheres and small spheres according to their size, and the mass ratio of the three is 1:2:2; the diameters of the large spheres, medium spheres and small spheres are 10mm, 5mm and 2mm respectively.

4. The method for preparing a low-temperature-rise metal ion-doped silver-zinc oxide electrical contact material according to claim 1, characterized in that... The rotational speed in step 2① is 18000 r / min.

5. The method for preparing a low-temperature-rise metal ion-doped silver-zinc oxide electrical contact material according to claim 1, characterized in that... In step two, a tissue pulverizer is used to mix the doped oxide powder prepared in step one with elemental silver powder, wherein the mass percentage of the doped oxide powder prepared in step one is 15%.

6. The method for preparing a low-temperature-rise metal ion-doped silver-zinc oxide electrical contact material according to claim 1, characterized in that... In step three, the mixed powder is pressed into a blank at a pressure of 150 MPa, and the holding time is 60 s.

7. The method for preparing a low-temperature-rise metal ion-doped silver-zinc oxide electrical contact material according to claim 1, characterized in that... The extrusion ratio in step four is 25.

8. The method for preparing a low-temperature-rise metal ion-doped silver-zinc oxide electrical contact material according to claim 1, characterized in that... In step four, the billet is preheated to 850°C.

9. The method for preparing a low-temperature-rise metal ion-doped silver-zinc oxide electrical contact material according to claim 1, characterized in that... In step four, both the extrusion cylinder and the mold are heated to 500°C.

10. The method for preparing a low-temperature-rise metal ion-doped silver-zinc oxide electrical contact material according to claim 1, characterized in that... In step five, annealing is carried out at 800℃ for 2 hours.

Citation Information

Patent Citations

  • Silver zinc oxide electric contact material and preparation method thereof

    CN101944441A

  • Preparation method of silver metal oxide electrical contact material

    CN115710653A