A long-life, easily activated, high-capacity vanadium-based composite hydrogen storage material and its preparation method

By introducing AB3 superlattice alloy as an additive into vanadium-based alloys, the problems of high activation temperature and high cost of vanadium-based hydrogen storage alloys are solved, achieving rapid activation at room temperature and high hydrogen storage capacity, which is suitable for large-scale applications.

CN118256787BActive Publication Date: 2026-11-10SHANGHAI UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410532379.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-30
Publication Date
2026-11-10
Estimated Expiration
2044-04-30

AI Technical Summary

Technical Problem

Existing vanadium-based hydrogen storage alloys suffer from problems such as high activation temperature, high cost, and loss of hydrogen storage capacity, which limit their large-scale application.

Method used

A high-vanadium alloy V75TixCr(25-x) was used as the matrix, and AB3 superlattice alloy La0.88-yY0.1Ca0.7+yMg1.32Ni9 was used as the additive. The composite material was formed by high-energy ball milling process, resulting in an easily activated and high-capacity vanadium-based composite hydrogen storage material.

Benefits of technology

Rapid activation at room temperature was achieved, reducing alloy costs while maintaining high hydrogen storage capacity, making it suitable for large-scale applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118256787B_ABST
    Figure CN118256787B_ABST
Patent Text Reader

Abstract

This invention discloses a long-life, easily activated, high-capacity vanadium-based composite hydrogen storage material and its preparation method. The composite hydrogen storage material comprises a vanadium-based alloy V... 75 Ti x Cr (25‑x) and AB3 superlattice alloy La 0.88‑y Y 0.1 Ca 0.7+y Mg 1.32 The vanadium-based composite hydrogen storage material is prepared by high-energy ball milling of Ni9, wherein 6≤x≤10, 0≤y≤0.4, and AB3 superlattice alloy content is 5-10 wt.%. The advantages of the vanadium-based composite hydrogen storage material prepared by this invention are that the selected AB3 alloy itself has high hydrogen absorption and desorption capacity, is easily activated at room temperature, and has a hydrogen desorption plateau pressure similar to that of high-vanadium alloys, thus giving the vanadium-based composite hydrogen storage material long lifespan, easy activation, and high capacity. This invention uses a mechanical ball milling process to prepare the composite hydrogen storage material. This method is simple, and the composite material reduces the overall vanadium content, lowering the alloy cost and facilitating large-scale preparation and application.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a long-life, easily activated, high-capacity vanadium-based composite hydrogen storage material and its preparation method, belonging to the field of solid-state hydrogen storage materials. Background Technology

[0002] Currently, the global non-renewable energy crisis is becoming increasingly severe, prompting researchers to intensify their research and development of new clean energy sources. Among the many energy sources under development, hydrogen energy, due to its significant characteristics, has become one of the most important renewable clean energy sources. Hydrogen is the lightest element in the periodic table, and its density is extremely low, making safe, economical, and efficient hydrogen storage a very challenging problem. There are three main methods for hydrogen storage: high-pressure gaseous hydrogen storage, cryogenic liquid hydrogen storage, and solid-state hydrogen storage. Among these, solid-state hydrogen storage alloys have become one of the most promising hydrogen storage technologies due to their advantages such as high safety, mild operating conditions, low energy consumption, and high volumetric hydrogen storage density.

[0003] Among solid-state hydrogen storage alloys, vanadium-based solid solution alloys are a promising hydrogen storage material, with a theoretical maximum hydrogen storage capacity of 3.8 wt.%, far exceeding other traditional hydrogen storage alloys, such as the AB5 alloy with a hydrogen absorption capacity of 1.4 wt.% and the AB alloy with 1.86 wt.%. Furthermore, vanadium-based solid solution alloys can absorb and release hydrogen at room temperature, making them one of the most promising high-capacity hydrogen storage materials. However, vanadium-based hydrogen storage alloys generally suffer from high activation temperatures and high costs, limiting their large-scale application. Current research mostly employs doping with rare earth elements to improve their activation performance, such as using Ce doping to improve the activation properties of high-vanadium alloys. 80 Ti5Cr 15 While the activation performance of vanadium-based hydrogen storage alloys is good (Journal of Alloys and Compounds, 2023, 934: 167947), doping elements usually cause a loss of hydrogen storage capacity in the alloy. Meanwhile, for vanadium-based hydrogen storage alloys, when the V content in the alloy is high, the cycle performance is improved (International Journal of Hydrogen Energy, 2010, 35(17): 9082-9087), but this also increases the alloy cost, which is not conducive to practical applications. Therefore, developing vanadium-based hydrogen storage materials that have good cycle performance, are easy to activate, and have high capacity while reducing the cost of hydrogen storage alloys is a key technology for their large-scale application and has become an urgent technical problem to be solved. Summary of the Invention

[0004] To address the aforementioned technical problems, this invention provides a long-life, easily activated, and high-capacity vanadium-based composite hydrogen storage material and its preparation method. The developed vanadium-based composite material possesses easy activation, high capacity, and long lifespan, while also reducing alloy costs and simplifying the preparation process, which is beneficial for large-scale preparation and application.

[0005] To achieve the above-mentioned objectives, the present invention adopts the following technical solution:

[0006] A long-life, easily activated, high-capacity vanadium-based composite hydrogen storage material, using high-vanadium alloy V 75 Ti x Cr (25-x) As the matrix for composite hydrogen storage materials, AB3 superlattice alloy La 0.88-y Y 0.1 Ca 0.7+y Mg 1.32 Ni9 is used as an additive, wherein the mass percentage content of AB3 superlattice alloy is 5-10 wt.%; the alloy chemical formula meets the conditions: 6≤x≤10, 0≤y≤0.4; the high vanadium alloy and AB3 superlattice alloy are compounded by a mixed ball milling process, so that the AB3 superlattice alloy powder particles are in full contact with the surface of the high vanadium alloy powder particles, and the AB3 superlattice alloy powder particles are loaded on the surface of the high vanadium alloy powder particles to form a high vanadium alloy activated composite catalyst, thereby obtaining the long-life, easily activated, high-capacity vanadium-based composite hydrogen storage material.

[0007] Preferably, the structure of the long-life, easily activated, and high-capacity vanadium-based composite hydrogen storage material of the present invention is mainly a body-centered cubic (BCC) phase.

[0008] Preferably, the alloy chemical formula satisfies the following conditions: 8≤x≤10, 0.33≤y≤0.4.

[0009] Preferably, after 1000 cycles of hydrogen absorption and desorption, the vanadium-based composite hydrogen storage material of the present invention has an effective hydrogen release capacity of not less than 1.95 wt% and an effective capacity retention rate of not less than 83.0%.

[0010] Preferably, the vanadium-based composite hydrogen storage material of the present invention can be fully activated after being evacuated at 353K for 30 minutes and then subjected to hydrogen absorption and desorption no more than 3 times at 298K.

[0011] Preferably, the effective hydrogen release capacity of the vanadium-based composite hydrogen storage material of the present invention is not less than 2.20 wt.%.

[0012] A method for preparing a long-life, easily activated, and high-capacity vanadium-based composite hydrogen storage material according to the present invention includes the following steps:

[0013] (1) Preparation of high-vanadium alloys:

[0014] High-vanadium alloy V was prepared by vacuum arc melting.75 Ti x Cr (25-x) As a base material, where 6≤x≤10, the purity of the raw materials used to prepare the high vanadium alloy is ≥99.9%;

[0015] (2) Preparation of AB3 superlattice alloy:

[0016] AB3 superlattice alloy La was prepared by vacuum induction melting. 0.88-y Y 0.1 Ca 0.7+y Mg 1.32 Ni9 is used as an additive material, where 0≤y≤0.4, and the purity of the raw materials used to prepare AB3 superlattice alloy is ≥99.9%;

[0017] (3) Preparation of vanadium-based composite hydrogen storage materials:

[0018] The high-vanadium alloy prepared in step (1) and the AB3 superlattice alloy prepared in step (2) were used as raw materials and ball-milled in a high-purity Ar atmosphere according to the raw material ratio. The raw material ratio was 5-10 wt.% of the AB3 superlattice alloy. The ball mill speed was controlled at 250-400 rpm / min, the ball-to-material ratio was (30-50):1, and the ball milling time was 1-5 h.

[0019] Preferably, in step (3), the ball mill runs for 15 minutes and then rests for 15 minutes.

[0020] Preferably, in step (1), a cast vanadium-based alloy is prepared by a vacuum non-consumable arc furnace melting method using inert argon as a protective gas. The cast vanadium-based alloy is then mechanically crushed to a size of 3-5 mm and used as a matrix material in the composite material.

[0021] Preferably, in step (2), an induction melting furnace with inert argon as the protective gas is used to obtain the as-cast AB3 alloy, which is then vacuum annealed at no higher than 1173K for no more than 20 hours; the AB3 alloy obtained after annealing is then mechanically crushed and ground to a size of 0.5-1mm and used as an additive material in the composite material.

[0022] Compared with existing technologies, the present invention has the following advantages:

[0023] 1. This invention uses AB3 superlattice alloy as an additive to achieve both catalytic and hydrogen absorption / desorption functions:

[0024] Firstly, AB3 alloy itself can absorb and release hydrogen at room temperature and is easily activated at room temperature. By ball milling and compounding it onto the surface of vanadium-based alloy, it can play a catalytic role, enabling the vanadium-based alloy to be activated at room temperature.

[0025] Secondly, the selected AB3 superlattice alloy has similar thermodynamic properties to the high vanadium alloy and has a similar hydrogen desorption plateau pressure, which can absorb and release hydrogen under the same conditions, so that the vanadium-based alloy can maintain its capacity without significant reduction while improving its activation performance.

[0026] 2. This invention prepares composite hydrogen storage materials through a mechanical ball milling process. This method is simple and can be widely used. In addition, the composite material reduces the overall vanadium content and alloy cost, which is beneficial for large-scale application. Attached Figure Description

[0027] Figure 1 The vanadium-based composite material (V) in Example 1 75 Ti8Cr 17 +10% La 0.55 Y 0.1 Ca 1.03 Mg 1.32 XRD pattern of Ni9.

[0028] Figure 2 The vanadium-based composite material (V) in Example 1 75 Ti8Cr 17 +10% La 0.55 Y 0.1 Ca 1.03 Mg 1.32 The activation performance curve of Ni9 at 298K and the comparison of alloy V in the V-type alloy 75 Ti8Cr 17 Activation performance curve at 298K.

[0029] Figure 3 The vanadium-based composite material (V) in Example 1 75 Ti8Cr 17 +10% La 0.55 Y 0.1 Ca 1.03 Mg 1.32 The PCT curves of Ni9 before and after 1000 cycles at 298K and the V curve in the comparative example. 75 Ti8Cr 17 PCT curve of the alloy at 298K. Detailed Implementation

[0030] To facilitate understanding of the present invention, specific embodiments are described below. However, these embodiments are merely illustrative and explanatory and do not constitute a limitation thereof. Preferred embodiments of the present invention are detailed below:

[0031] Example 1:

[0032] This embodiment provides a long-life, easily activated, high-capacity vanadium-based composite hydrogen storage material and its preparation method. The vanadium-based composite hydrogen storage material has a composition of V... 75 Ti8Cr 17 +10% La 0.55 Y 0.1 Ca 1.03 Mg 1.32 Ni9.

[0033] V prepared according to the target 75 Ti8Cr 17 The elemental composition of the alloy was determined, raw materials were weighed, and a cast vanadium-based alloy was prepared by melting in a vacuum non-consumable arc furnace using argon as the protective gas. The cast vanadium-based alloy was then mechanically crushed to a size of 3-5 mm and used as the matrix material in the composite material. La was prepared according to the target... 0.55 Y 0.1 Ca 1.03 Mg 1.32 The elemental composition of Ni9 alloy was determined, raw materials were weighed, and as-cast AB3 alloy was obtained using an induction melting furnace with inert argon as the protective gas. This as-cast alloy was then vacuum annealed at 1173K for 20 hours. The annealed AB3 alloy was mechanically crushed and ground to a size of 0.5-1mm to be used as an additive in the composite material. The two materials were mixed at a mass ratio of 90:10 and placed in a stainless steel ball mill jar. The composite material was obtained by ball milling under high-purity argon gas at a speed of 400 rpm / min, a ball-to-material ratio of 50:1, and a milling time of 5 hours. The ball mill operated for 15 minutes followed by a 15-minute pause.

[0034] The vanadium-based composite hydrogen storage material V prepared in Example 1 75 Ti8Cr 17 +10% La 0.55 Y 0.1 Ca 1.03 Mg 1.32 Ni9, whose structure is mainly body-centered cubic (BCC), such as Figure 1 As shown. This composite hydrogen storage material, after being vacuumed at 353K for 30 minutes, can rapidly absorb and desorb hydrogen at 298K without requiring high-temperature activation, such as... Figure 2 As shown. The hydrogen desorption plateau of this composite material at 298 K is 0.3 MPa, and the effective hydrogen desorption capacity is 2.36 wt.%, which is higher than that of pure V. 75 Ti8Cr17 The alloy exhibits high capacity. After 1000 cycles of hydrogen adsorption and desorption, its effective hydrogen release is 1.97 wt%, and its effective capacity retention rate is 83.5%. Figure 3 As shown in the figure. These results indicate that the composite material possesses properties such as long lifespan, easy activation, and high capacity, making it suitable for large-scale applications.

[0035] Example 2

[0036] This embodiment provides a long-life, easily activated, high-capacity vanadium-based composite hydrogen storage material and its preparation method. The vanadium-based composite hydrogen storage material has a composition of V... 75 Ti6Cr 19 +5% La 0.88 Y 0.1 Ca 0.7 Mg 1.32 Ni9.

[0037] V prepared according to the target 75 Ti6Cr 19 The elemental composition of the alloy was determined, raw materials were weighed, and a cast vanadium-based alloy was prepared by melting in a vacuum non-consumable arc furnace using argon as the protective gas. The cast vanadium-based alloy was then mechanically crushed to a size of 3-5 mm and used as the matrix material in the composite material. La was prepared according to the target... 0.88 Y 0.1 Ca 0.7 Mg 1.32 The elemental composition of Ni9 alloy was determined. Raw materials were weighed, and a cast AB3 alloy was prepared using an induction melting furnace with inert argon as the protective gas. This alloy was then vacuum annealed at 1173 K for 20 hours. The annealed AB3 alloy was mechanically crushed and ground to a size of 0.5-1 mm to be used as an additive in the composite material. The two materials were mixed at a mass ratio of 95:5 and placed in a stainless steel ball mill jar. The composite material was obtained by ball milling under high-purity argon at a speed of 350 rpm / min, a ball-to-material ratio of 40:1, and a milling time of 1 hour. The ball mill operated for 15 minutes followed by a 15-minute pause.

[0038] The vanadium-based composite hydrogen storage material V prepared in Example 2 75 Ti6Cr 19 +5% La 0.88 Y 0.1 Ca 0.7 Mg 1.32Ni9, with a predominantly body-centered cubic structure, was used in this composite hydrogen storage material. After being vacuumed at 353 K for 30 minutes, it was fully activated by three hydrogen adsorption / desorption cycles at 298 K, without requiring high-temperature activation. The hydrogen desorption plateau at 298 K was 0.9 MPa, with an effective hydrogen desorption capacity of 2.4 wt.%. After 1000 cycles of hydrogen adsorption / desorption, the effective hydrogen desorption capacity remained at 1.99 wt%, and the effective capacity retention was 83.0%. These results indicate that the composite material possesses long lifespan, easy activation, and high capacity, making it suitable for large-scale applications.

[0039] Example 3:

[0040] This embodiment provides a long-life, easily activated, high-capacity vanadium-based composite hydrogen storage material and its preparation method. The vanadium-based composite hydrogen storage material has a composition of V... 75 Ti 10 Cr 15 +8% La 0.48 Y 0.1 Ca 1.1 Mg 1.32 Ni9.

[0041] V prepared according to the target 75 Ti 10 Cr 15 The elemental composition of the alloy was determined, raw materials were weighed, and a cast vanadium-based alloy was prepared by melting in a vacuum non-consumable arc furnace using argon as the protective gas. The cast vanadium-based alloy was then mechanically crushed to a size of 3-5 mm and used as the matrix material in the composite material. La was prepared according to the target... 0.48 Y 0.1 Ca 1.1 Mg 1.32 The elemental composition of Ni9 alloy was determined. Raw materials were weighed, and a cast AB3 alloy was obtained using an induction melting furnace with inert argon as the protective gas. This alloy was then vacuum annealed at 1173K for 20 hours. The annealed AB3 alloy was mechanically crushed and ground to a size of 0.5-1mm to be used as an additive in the composite material. The two materials were mixed at a mass ratio of 92:8 and placed in a stainless steel ball mill jar. The composite material was obtained by ball milling under high-purity argon at a speed of 250 rpm / min, a ball-to-material ratio of 30:1, and a milling time of 2 hours. The ball mill operated for 15 minutes followed by a 15-minute pause.

[0042] The vanadium-based composite hydrogen storage material V prepared in Example 3 75 Ti 10 Cr 15 +8% La 0.48 Y 0.1 Ca 1.1 Mg 1.32Ni9, with a predominantly body-centered cubic structure, was used in this composite hydrogen storage material. After being vacuumed at 353 K for 30 minutes, it was fully activated by three hydrogen adsorption / desorption cycles at 298 K, without requiring high-temperature activation. The composite material exhibited a hydrogen desorption plateau of 0.3 MPa at 318 K, with an effective hydrogen desorption capacity of 2.32 wt.%. After 1000 cycles of hydrogen adsorption / desorption, the effective hydrogen desorption capacity remained at 1.95 wt%, with an effective capacity retention of 84.0%. These results demonstrate that the composite material possesses long lifespan, easy activation, and high capacity, making it suitable for large-scale applications.

[0043] Comparative example:

[0044] A high vanadium alloy V 75 Ti8Cr 17 and its preparation method, V prepared according to the target 75 Ti8Cr 17 The elemental ratio of the alloy was determined, raw materials were weighed, and a cast vanadium-based alloy was obtained by melting in a vacuum non-consumable arc furnace with inert argon as the protective gas. The cast vanadium-based alloy was mechanically crushed to a size of 3-5 mm and then placed in a stainless steel ball mill jar for ball milling under high-purity argon. The ball milling process parameters were the same as those in Example 1, namely, a ball milling speed of 400 rpm / min, a ball-to-material ratio of 50:1, a ball milling time of 5 h, and a 15-minute pause after every 15 minutes of ball milling.

[0045] V prepared in comparison 75 Ti8Cr 17 The alloy has a body-centered cubic (BCC) phase structure. V 75 Ti8Cr 17 When the alloy was ball-milled without the addition of AB3 alloy, the number of activation cycles increased significantly, and activation was not completed until the fourth hydrogen absorption cycle. Figure 2 As shown. V 75 Ti8Cr 17 The hydrogen desorption plateau pressure of the alloy is approximately 0.3 MPa, such as Figure 3 As shown, the plateau pressure of the composite material prepared in Example 1 is similar, but its maximum hydrogen absorption and effective hydrogen release are lower than those of the composite material prepared in Example 1. The comparison demonstrates that by combining with AB3 alloy, the activation performance and hydrogen storage capacity of the vanadium-based composite material are effectively improved, while the alloy cost is reduced to some extent.

[0046] In summary, the above embodiments provide a long-life, easily activated, high-capacity vanadium-based composite hydrogen storage material and its preparation method, which utilizes high-vanadium alloy V 75 Ti x Cr (25-x) As a matrix for composite hydrogen storage materials, AB3 superlattice alloy La 0.88-y Y0.1 Ca 0.7+ y Mg 1.32 Using Ni9 as an additive, the two are combined through a high-energy ball milling process to obtain a long-life, easily activated, and high-capacity hydrogen storage composite material, wherein 6≤x≤10, 0≤y≤0.4, and the AB3 content is 5-10 wt.%. The advantages of the above embodiments of the present invention are that the use of AB3 superlattice alloy as an additive plays a dual role in catalysis and hydrogen absorption / desorption, thereby improving the activation performance and hydrogen storage capacity of the vanadium-based alloy while reducing its alloy cost; moreover, the composite material preparation process is simple and suitable for large-scale preparation and application.

[0047] The embodiments of the present invention have been described above in conjunction with the accompanying drawings. However, the present invention is not limited to the above embodiments. Various changes can be made according to the purpose of the invention. Any changes, modifications, substitutions, combinations or simplifications made based on the spirit and principle of the technical solution of the present invention shall be equivalent substitutions. As long as they meet the purpose of the invention and do not deviate from the technical principle and inventive concept of the present invention, they shall fall within the protection scope of the present invention.

Claims

1. A long-life, easily activated, high-capacity vanadium-based composite hydrogen storage material, characterized in that: High vanadium alloy V 75 Ti x Cr (25-x) As the matrix for composite hydrogen storage materials, AB3 superlattice alloy La 0.88-y Y 0.1 Ca 0.7+y Mg 1.32 Ni9 is used as an additive, wherein the mass percentage content of AB3 superlattice alloy is 5-10 wt.%; the alloy chemical formula meets the conditions: 6≤x≤10, 0≤y≤0.4; the high vanadium alloy and AB3 superlattice alloy are compounded by a mixed ball milling process, so that the AB3 superlattice alloy powder particles are in full contact with the surface of the high vanadium alloy powder particles, and the AB3 superlattice alloy powder particles are loaded on the surface of the high vanadium alloy powder particles to form a high vanadium alloy activated composite catalyst, thereby obtaining the long-life, easily activated, high-capacity vanadium-based composite hydrogen storage material.

2. The long-life, easily activated, high-capacity vanadium-based composite hydrogen storage material according to claim 1, characterized in that: Its structure is mainly body-centered cubic (BCC).

3. The long-life, easily activated, high-capacity vanadium-based composite hydrogen storage material according to claim 1, characterized in that: The chemical formula of the alloy satisfies the following conditions: 8≤x≤10, 0.33≤y≤0.

4.

4. The long-life, easily activated, high-capacity vanadium-based composite hydrogen storage material according to claim 1, characterized in that: After 1000 cycles of hydrogen absorption and desorption, the vanadium-based composite hydrogen storage material has an effective hydrogen release capacity of not less than 1.95 wt% and an effective capacity retention rate of not less than 83.0%.

5. The long-life, easily activated, high-capacity vanadium-based composite hydrogen storage material according to claim 1, characterized in that: It can be fully activated by vacuuming at 353K for 30 minutes and then performing hydrogen adsorption / desorption no more than 3 times at 298K.

6. The long-life, easily activated, high-capacity vanadium-based composite hydrogen storage material according to claim 1, characterized in that: Its effective hydrogen release is not less than 2.20 wt.%.

7. A method for preparing the long-life, easily activated, high-capacity vanadium-based composite hydrogen storage material according to claim 1, characterized in that, Includes the following steps: (1) Preparation of high-vanadium alloys: High-vanadium alloy V was prepared by vacuum arc melting. 75 Ti x Cr (25-x) As a base material, where 6≤x≤10, the purity of the raw materials used to prepare the high vanadium alloy is ≥99.9%; (2) Preparation of AB3 superlattice alloy: AB3 superlattice alloy La was prepared by vacuum induction melting. 0.88-y Y 0.1 Ca 0.7+y Mg 1.32 Ni9 is used as an additive material, where 0≤y≤0.4, and the purity of the raw materials used to prepare AB3 superlattice alloy is ≥99.9%; (3) Preparation of vanadium-based composite hydrogen storage materials: The high-vanadium alloy prepared in step (1) and the AB3 superlattice alloy prepared in step (2) were used as raw materials and ball-milled in a high-purity Ar atmosphere according to the raw material ratio. The raw material ratio was 5-10 wt.% of the AB3 superlattice alloy. The ball mill speed was controlled at 250-400 rpm / min, the ball-to-material ratio was (30-50):1, and the ball milling time was 1-5 h.

8. The preparation method of the long-life, easily activated, high-capacity vanadium-based composite hydrogen storage material according to claim 7, characterized in that: In step (3), the ball mill runs for 15 minutes and then stops for 15 minutes.

9. The preparation method of the long-life, easily activated, high-capacity vanadium-based composite hydrogen storage material according to claim 7, characterized in that: In step (1), a cast vanadium-based alloy is prepared by a vacuum non-consumable arc furnace melting method using inert argon as a protective gas. The cast vanadium-based alloy is mechanically crushed to a size of 3-5 mm and then used as a matrix material in the composite material.

10. The method for preparing the long-life, easily activated, high-capacity vanadium-based composite hydrogen storage material according to claim 7, characterized in that: In step (2), an induction melting furnace with inert argon as the protective gas is used to obtain a cast AB3 alloy, which is then vacuum annealed at a temperature not higher than 1173K for no more than 20 hours. The AB3 alloy obtained after annealing is then mechanically crushed and ground to a size of 0.5-1mm and used as an additive material in the composite material.

Citation Information

Patent Citations

  • Method for preparing superlattice hydrogen storing alloy

    CN104294087A

  • Low-temperature activated vanadium-based hydrogen storage alloy, and preparation method and application thereof

    CN113502424A