A bainitic non-quenched and tempered steel and its preparation method
By controlling the content of elements such as C, Si, Mn, Mo, Cr, and V, and the processes of electric arc furnace steelmaking, refining, degassing, die casting or continuous casting, heating and rolling, and tempering, high-strength and high-toughness bainitic non-quenched and tempered steel is prepared, solving the problems of increased energy consumption and environmental pollution caused by traditional quenching and tempering processes, and achieving efficient and low-cost production.
Patent Information
- Application Number
- CN202410388722.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-01
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2044-04-01
AI Technical Summary
Existing technologies make it difficult to produce high-strength, high-toughness, and low-cost bainitic non-quenched and tempered steel without adding expensive alloying elements, and traditional quenching and tempering processes increase energy consumption and environmental pollution.
By controlling the content of elements such as C, Si, Mn, Mo, Cr, and V, and combining electric arc furnace steelmaking, refining, degassing, die casting or continuous casting, heating and rolling, and tempering processes, non-quenched and tempered steel with a stable bainitic matrix can be prepared, eliminating the need for the quenching and tempering process and allowing for direct cutting and use.
It has enabled the preparation of high-strength, high-toughness bainitic non-quenched and tempered steel, meeting the strength and toughness requirements of parts, improving production efficiency, reducing energy consumption, reducing environmental pollution, and controlling costs.
Smart Images

Figure CN118256825B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of non-quenched and tempered steel technology, specifically a bainitic non-quenched and tempered steel and its preparation method. Background Technology
[0002] Non-quenched and tempered steel, with its unique "green manufacturing" qualities and characteristics, has gradually gained market recognition and acceptance, bringing outstanding results to its users. It has been integrated into the automotive, construction machinery, and equipment manufacturing industries, fully leveraging its superior characteristics such as high quality, low cost, short manufacturing cycle, and high component precision. Market demand and development are increasingly reliant on it. With the development trends of downstream markets in the automotive, construction machinery, and equipment manufacturing industries, a lightweight, higher-strength, higher-quality, lower-cost, and more competitive non-quenched and tempered steel material—bainitic non-quenched and tempered steel—has emerged to meet market demand.
[0003] In studying the relationship between the cooling rate and mechanical properties of steel, it was found that low-alloy steel, after undergoing austenitization treatment and being held at a certain temperature for a period of time, can obtain acicular ferrite and a eutectoid structure of carbides precipitated at certain interfaces, thus giving the steel excellent comprehensive properties. This structure is called bainite, and a patent has been registered for the bainitic structure of steel and the isothermal quenching heat treatment process. The bainitic transformation occurs when the steel is supercooled to the intermediate temperature region after austenitization treatment, hence it is also called the intermediate temperature transformation. Because bainite, especially lower bainite, has excellent comprehensive mechanical properties, in production, steel is often austenitized and then supercooled to the intermediate temperature transformation region and held isothermally to obtain the bainitic structure. This heat treatment is called bainitic isothermal quenching.
[0004] Researchers have conducted extensive studies on bainitic steel, obtaining "cast bainitic steel" or "air-cooled bainitic steel after rolling" by adjusting chemical composition and modification processes, replacing the traditional isothermal quenching process and rapidly expanding its application range. Because the air-cooled bainitic steel process is simple, in addition to achieving excellent comprehensive mechanical properties, it also significantly reduces the deformation and cracking tendency that occurs with conventional quenching (which yields martensitic structure).
[0005] Bainitic steel, as one of the new steel grades of the 21st century, is classified into high-carbon bainitic steel, medium-carbon bainitic steel, and low-carbon bainitic steel based on its carbon content. Medium and high-carbon bainitic steels are used in power plants, mines, and aerospace due to their advantages of high hardness, simple alloy composition, and low cost. Low-carbon bainitic steel is widely used in construction, bridges, vehicles, aircraft components, and shafts. Bainitic steel achieves high strength and high toughness while also possessing good weldability, making it one of the most promising steel grades. Therefore, bainitic steel represents an important direction for the development of ultra-high-strength steel. Research on bainitic transformation and its preparation technology has significant theoretical and engineering application value for improving the strength, toughness, and overall performance of steel. Summary of the Invention
[0006] The present invention aims to provide a high-strength and high-toughness bainitic non-quenched and tempered steel and its preparation method. The steel obtains high strength and high toughness under air cooling and tempering conditions, and the matrix is a stable bainitic structure, which is suitable for producing parts with high strength and toughness.
[0007] To achieve the above objectives, the present invention adopts the following technical solution:
[0008] In a first aspect, a bainitic non-quenched and tempered steel comprises, by mass percentage, 0.12-0.20% C, 0.20-1.00% Si, 2.00-2.70% Mn, 0.05-0.25% Mo, 0.20-0.80% Cr, and 0.05-0.15% V, with the remainder being Fe and non-removable impurities, said non-removable impurities including: P ≤ 0.015%, S ≤ 0.015%, Cu < 0.05%, and Ni ≤ 0.20%.
[0009] Furthermore, 2.6% < Si + Mn < 3.2%.
[0010] Furthermore, the bainitic non-quenched and tempered steel is mainly composed of granular bainite and lath bainite; according to GB / T231.1, the hardness reaches 270-350 HBW; according to GB / T 228.1, the yield strength is ≥700MPa, the tensile strength is ≥900MPa, the elongation is ≥12%, and the reduction of area is ≥30%; according to GB / T 229, the impact energy is ≥30J.
[0011] Secondly, a method for preparing the bainitic non-quenched and tempered steel includes the following steps: electric furnace or converter steelmaking, refining, degassing, die casting or continuous casting, heating and rolling, air cooling and tempering; wherein the tempering temperature is 350-550℃ and the holding time is 8-12h.
[0012] Furthermore, in the electric furnace or converter steelmaking process, the proportion of liquid pig iron in the raw materials is 80-82 wt%, with the remainder being scrap steel and / or ferroalloys.
[0013] Furthermore, in the electric furnace or converter steelmaking process, the slag-forming agent used includes lime and dolomite, whose main chemical components are CaO+SiO+MgO.
[0014] Furthermore, in the electric furnace or converter steelmaking process, the steel is tapped after the C content in the molten steel is 0.05-0.10 wt% and the P content is ≤0.015 wt%. The tapping temperature of the molten steel is 1600-1700℃. During the tapping process, refining slag and lime are added to form slag, and Al ingots are added for precipitation deoxidation and some Si, Mn, and Cr alloys are added.
[0015] Furthermore, the refining process includes, but is not limited to, LF furnace refining;
[0016] And / or, in the refining process, Al particles are used for diffusion deoxidation, and the composition of the molten steel is adjusted to the range of alloy element content required for the bainitic non-quenched and tempered steel;
[0017] And / or, in the refining process, the refining temperature is 1600–1650°C.
[0018] Furthermore, the degassing is RH vacuum degassing, preferably carried out under a vacuum of less than 67 Pa, and the degassing time is preferably at least 15 minutes.
[0019] Furthermore, the casting temperature of the continuous casting is 1515–1535°C; and / or, the pre-rolling heating keeps the billet temperature above 1200°C, preferably 1200–1250°C.
[0020] Compared with the prior art, the present invention has the following beneficial effects:
[0021] 1. This invention relates to a bainitic non-quenched and tempered steel with a stable bainitic matrix, which meets the requirements for high-strength and high-toughness steel and is suitable for producing parts with high strength and toughness. Compared with traditional quenched and tempered steel, it eliminates the quenching and tempering process, allowing for direct cutting and use, improving production efficiency, reducing energy consumption, and minimizing environmental pollution. Compared with bainitic non-quenched and tempered steel containing more expensive alloying elements (such as Mo, Ni, and V), it offers superior cost control.
[0022] 2. The preparation method of this invention involves cutting multiple Φ25mm steel bar samples from rolled, air-cooled, and tempered steel. Testing revealed that the microstructure consisted of bainite (mainly granular and lath bainite) plus a small amount of ferrite. According to GB / T 231.1, the hardness reached 270-350 HBW. According to GB / T 228.1, the steel's yield strength was ≥700MPa, tensile strength ≥900MPa, elongation ≥12%, and reduction of area ≥30%. According to GB / T 229, the steel's impact energy was ≥30J, all meeting the design requirements. Attached Figure Description
[0023] Figure 1 This is a SEM image of the bainitic non-quenched and tempered steel obtained in Example 1 of the present invention. Detailed Implementation
[0024] To make the objectives, technical solutions, and advantages of this invention clearer, the technical solutions of this invention will be clearly and completely described below in conjunction with the embodiments of this invention. The embodiments of this invention are implemented based on the technical solutions of this invention, and detailed implementation methods and processes are given. However, the scope of protection of this invention is not limited to the following embodiments. Those skilled in the art should understand that the embodiments are merely helpful in understanding this invention and should not be considered as specific limitations on this invention. All other embodiments obtained by those skilled in the art based on the embodiments of this invention without creative effort are within the scope of protection of this invention.
[0025] The endpoints and any values of the ranges disclosed in this invention are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of the various ranges, the endpoint values of the various ranges and individual point values, and individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this invention.
[0026] In this invention, unless otherwise specified and / or stated, all numerical values relating to component amounts are "by weight or weight percentage" throughout. Process parameters in the following examples, unless otherwise specified, are generally performed under conventional conditions. The raw materials described in the following examples are all available from publicly available commercial sources.
[0027] According to a first aspect of the present invention, a bainitic non-quenched and tempered steel comprises, by mass percentage, 0.12-0.20% C, 0.20-1.00% Si, 2.00-2.70% Mn, 0.05-0.25% Mo, 0.20-0.80% Cr, and 0.05-0.15% V, with the remainder being Fe and non-removable impurities, said non-removable impurities including: P ≤ 0.015%, S ≤ 0.015%, Cu < 0.05%, and Ni ≤ 0.20%.
[0028] The composition design scheme of this invention is based on the following:
[0029] 1. In order to obtain a bainitic structure with sufficiently high hardenability during continuous cooling, alloying elements such as B, Si, Mn, Cr, Mo, and V are usually added to bainitic steel.
[0030] 1.1 The carbon content in bainite should not be too high. Exceeding 0.3% easily leads to the precipitation of excessive carbides, increasing the steel's strength but decreasing its toughness. Empirically, carbon content exceeding 0.2% narrows the tempering process window; the designed carbon content is 0.12-0.20%. As an optional embodiment of the bainitic non-quenched and tempered steel of this invention, the carbon content is typically, but not limited to, 0.13%, 0.14%, 0.15%, 0.16%, 0.17%, 0.18%, and 0.19%.
[0031] 1.2 Si element inhibits cementite precipitation, stabilizes retained austenite, and promotes the formation of carbide-free bainite. With increasing Si content, the phase transformation structure gradually refines, granular bainite decreases, and carbide-free bainite increases, thereby refining the bainite laths. Si plays a role in solid solution strengthening and lowering the bainite initiation temperature in bainitic steel. The designed Si content is controlled at 0.20-1.00%. As an optional embodiment of the non-quenched and tempered bainitic steel of this invention, the Si content is typically, but not limited to, 0.21%, 0.25%, 0.3%, 0.35%, 0.4%, 0.45%, 0.5%, 0.55%, 0.6%, 0.65%, 0.7%, 0.75%, 0.8%, 0.85%, 0.9%, 0.95%, and 0.99%.
[0032] Mn expands the austenite phase region, lowers the phase transformation temperature, and has a strong solid solution strengthening effect, significantly improving the hardenability and hardness of low-carbon bainitic steel and delaying the deformation-strengthening phase transformation process. During smelting, Mn combines with oxygen and sulfur in the molten steel and floats to the slag for removal, making it an economical and practical deoxidizer and desulfurizer. However, excessively high Mn content will reduce the plasticity of the steel; therefore, the Mn content is designed to be controlled between 2.00% and 2.70%. As an optional embodiment of the bainitic non-quenched and tempered steel of this invention, the Mn content can typically, but not exclusively, be selected as 2.05%, 2.1%, 2.15%, 2.2%, 2.25%, 2.3%, 2.35%, 2.4%, 2.45%, 2.5%, 2.55%, 2.6%, or 2.65%.
[0033] During the research process of this invention, it was specifically discovered that a proper balance of silicon and manganese can improve the strength and toughness of steel, which is beneficial for obtaining air-cooled bainite. Therefore, the design yielded 2.6% < Si + Mn < 3.2%. As an optional embodiment of the bainitic non-quenched and tempered steel of this invention, the Si + Mn content can typically, but not exclusively, be selected as 2.65%, 2.7%, 2.75%, 2.8%, 2.85%, 2.9%, 2.95%, 3%, 3.05%, or 3.15%.
[0034] 1.4 Typically, boron (B) is added to bainitic steel. B significantly shifts the ferrite transformation curve to the right, facilitating the formation of full bainite through air cooling. For example, in heavy-duty truck steering knuckle steel, which requires hot forging, adding B to the composition ensures the tensile and yield strength of the forged steering knuckle. However, this invention is for direct-cutting non-quenched steel, which must meet certain performance requirements after rolling. Therefore, this invention does not add B, because adding B would require increasing the Ti content, which would introduce TiN inclusions, affecting the fatigue life of the parts. Even if B and Ti are introduced into other raw materials in this invention, their content is very low: B < 0.0005% and Ti < 0.0025%, which are negligible impurities.
[0035] The addition of 1.5% Mo effectively delays the high-temperature ferrite phase transformation, lowers the Ms temperature, and strongly promotes bainite transformation, expanding the bainite transformation zone and enabling the formation of bainitic microstructures over a wide range of cooling rates. Mo significantly improves the strength and hardenability of steel, refines the austenite microstructure, inhibits crack initiation and propagation, and improves fatigue performance. Considering cost, the design controls Mo content to be 0.05-0.25%. As an optional embodiment of the bainitic non-quenched and tempered steel of this invention, the Mo content is typically, but not limited to, 0.06%, 0.08%, 0.1%, 0.12%, 0.14%, 0.16%, 0.18%, 0.2%, 0.22%, and 0.24%.
[0036] 1.6Cr is one of the most commonly used main alloying elements in the Mn-based air-cooled bainitic steel alloy system, and it can effectively control the microstructure and mechanical properties of bainitic steel. Adding Cr to steel allows for the formation of bainite at lower cooling rates, and significantly reduces the bainite transformation temperature range. Cr has a significant impact on the morphology and distribution of bainite. When Cr is 0.2%, the bainite morphology is mainly granular and lath bainite. When Cr is increased to 0.5%, a "willow leaf" shaped lower bainite structure is observed. Cr can significantly improve the hardness of bainitic steel. The design Cr content is 0.20-0.80%. As an optional embodiment of the bainitic non-quenched and tempered steel of the present invention, the Cr content is typically, but not limited to, 0.21%, 0.25%, 0.3%, 0.35%, 0.4%, 0.45%, 0.5%, 0.55%, 0.6%, 0.65%, 0.7%, 0.75%, and 0.79%.
[0037] 1.7 A small amount of V is added to the steel. V has a strong secondary hardening effect on steel. V can refine the grains, resulting in a fine-grained structure both on the surface and inside the steel, thus increasing the toughness of the steel. Considering cost, the V content is designed to be 0.05-0.15%. As an optional embodiment of the bainitic non-quenched and tempered steel of this invention, the V content can typically, but not exclusively, be selected as 0.06%, 0.07%, 0.08%, 0.09%, 0.1%, 0.11%, 0.12%, 0.13%, or 0.14%.
[0038] This invention relates to a non-quenched and tempered bainitic steel with a microstructure of granular bainite and lath bainite. According to GB / T 231.1, its hardness reaches 270-350 HBW; according to GB / T 228.1, its yield strength is ≥700 MPa, tensile strength is ≥900 MPa, elongation is ≥12%, and reduction of area is ≥30%; according to GB / T 229, its impact energy is ≥30 J, meeting the requirements for high-strength and high-toughness steel. Compared with traditional quenched and tempered steel, the quenching and tempering process can be eliminated, allowing for direct cutting and use, improving production efficiency, reducing energy consumption, and minimizing environmental pollution. Compared with non-quenched and tempered bainitic steel containing more expensive alloying elements (such as Mo, Ni, and V), it offers superior cost control. Quenched and tempered steel refers to steel that has been quenched (heated to above its critical temperature and rapidly cooled in a quenching medium to obtain martensite) followed by high-temperature tempering (transforming the martensite), resulting in a microstructure of tempered sorbite.
[0039] This invention relates to bainitic steel. During the steelmaking process, scrap steel and / or ferroalloys and / or liquid pig iron are typically used as raw materials. Residues from the scrap steel and molten iron introduce Ni impurities, typically not exceeding 0.2%. Furthermore, unavoidable Cu residues during steelmaking are <0.05%, a low content that avoids the copper embrittlement that can easily occur with high Cu content, leading to cracking during steel rolling. Al, as a deoxidizer, typically leaves 0.010-0.040% residue after deoxidation, ensuring a low oxygen level in the steel. To guarantee inclusion levels and internal quality, the oxygen content of the steel is ≤20ppm (e.g., 20ppm, 18ppm, 16ppm, 14ppm, 12ppm, 10ppm), and the hydrogen content is ≤2.0ppm (e.g., 2.0ppm, 1.8ppm, 1.6ppm, 1.4ppm, 1.2ppm, 1.0ppm). In addition, the present invention has a lower sulfur content, S≤0.015, which avoids the formation of sulfides by S that would affect the fatigue life of steel.
[0040] According to a second aspect of the present invention, a method for preparing the bainitic non-quenched and tempered steel includes the following steps: electric furnace or converter steelmaking, refining, degassing, die casting or continuous casting, heating and rolling, air cooling and tempering; wherein the tempering temperature is 350-550°C and the holding time is 8-12 hours.
[0041] The preparation method of this invention involves tempering the rolled and air-cooled steel to eliminate stress and promote the dissolution of bainitic carbides and retained austenite. This gives the bainitic non-quenched and tempered steel profiles of this invention excellent properties, especially suitable toughness. Preferably, the furnace is used at 350-550℃ (e.g., 360℃, 380℃, 400℃, 420℃, 440℃, 460℃, 480℃, 500℃, 520℃, 540℃) for 8-12 hours (e.g., 8.5 hours, 9 hours, 9.5 hours, 10 hours, 10.5 hours, 11 hours, 11.5 hours) to avoid incomplete stress release, which could lead to deformation during product use. It also prevents incomplete transformation of retained austenite and insufficient dissolution of carbides, which could result in poor toughness. The rolling process of this invention can be carried out using rolling mill rolls. The shape of the profile obtained after rolling is not particularly limited and can be determined according to the shape of the final product. For example, it can be in the form of sheet, block, wire, or bar. In the case of this invention, the shape of the profile is particularly preferably a bar. It is preferred that the profile be air-cooled to below 300°C after rolling before collection.
[0042] As an optional embodiment of the preparation method of the present invention, the typical production process of steel is as follows: converter → LF → RH → continuous casting → rolling → air cooling → tempering.
[0043] As an optional embodiment of the preparation method of the present invention, the process of electric furnace steelmaking or converter steelmaking is carried out using raw materials such as liquid pig iron, scrap steel, ferroalloys and slagging agents. The proportion of liquid pig iron in the raw materials is preferably about 80-82 wt% (e.g., 80.2 wt%, 80.5 wt%, 80.7 wt%, 81 wt%, 81.3 wt%, 81.5 wt%, 81.7 wt%, 81.9 wt%), and the remainder is mainly scrap steel and / or ferroalloys.
[0044] As an optional embodiment of the preparation method of the present invention, the slag-forming agent contains lime and dolomite, and its main chemical components are CaO+SiO+MgO.
[0045] As an optional embodiment of the preparation method of the present invention, in the electric furnace or converter steelmaking process, the steelmaking process is controlled so that the C content in the obtained molten steel is about 0.05-0.10 wt% (e.g., 0.06 wt%, 0.07 wt%, 0.08 wt%, 0.09 wt%), and the P content is about ≤0.015 wt% (e.g., 0.015 wt%, 0.013 wt%, 0.011 wt%, 0.009 wt%, 0.007 wt%, 0.005 wt%). After meeting the requirements, the steel is tapped into a prepared ladle. The temperature of the molten steel leaving the smelting furnace is about 1600-1700℃ (e.g., 1610℃, 1630℃, 1650℃, 1670℃, 1690℃). During the tapping process, refining slag, lime, etc. are added to form slag, and Al ingots are added for precipitation deoxidation and some Si, Mn, and Cr alloys. The tapping temperature is controlled at approximately 1600–1700℃. This avoids excessively high temperatures that could corrode the refractory material, affecting equipment lifespan and causing unnecessary waste. It also prevents corroded refractory material from entering the steel, affecting the steel's purity. Conversely, excessively low temperatures would require the LF furnace to increase the time spent on power supply and temperature raising, impacting production efficiency and increasing energy waste.
[0046] As an optional embodiment of the preparation method of the present invention, the molten steel obtained through the steelmaking process is refined, including but not limited to LF furnace refining.
[0047] As an optional embodiment of the preparation method of the present invention, in the refining process, Al particles are used for diffusion deoxidation, and the composition of the molten steel is adjusted to basically meet the alloy element content requirements of the bainitic non-quenched and tempered steel of the first aspect of the present invention.
[0048] As an optional embodiment of the preparation method of the present invention, the refining temperature can be, for example, approximately 1600–1650°C (e.g., 1605°C, 1610°C, 1615°C, 1620°C, 1625°C, 1630°C, 1635°C, 1640°C, 1645°C). Argon gas stirring is preferably used to homogenize the composition and temperature of the molten steel, while simultaneously causing inclusions in the molten steel to collide, grow, and float to the slag. The alloy element composition of the molten steel obtained after refining essentially meets the composition requirements of the bainitic non-quenched and tempered steel of the first aspect of the present invention.
[0049] As an optional embodiment of the preparation method of the present invention, the refined molten steel is further subjected to degassing treatment, preferably RH vacuum degassing. The degassing treatment is preferably carried out under a vacuum of about 67 Pa or less, and the degassing time is preferably at least about 15 minutes to ensure that the hydrogen content of the steel is ≤2.0 ppm; through the combined effect of vacuum degassing and refining deoxidation, the oxygen content of the steel is ensured to be ≤20 ppm.
[0050] As an optional embodiment of the preparation method of the present invention, after degassing, it can be carried out by die casting or continuous casting, preferably by continuous casting.
[0051] As an optional embodiment of the preparation method of the present invention, the casting temperature during the continuous casting process can be approximately 1515–1535℃ (e.g., 1516℃, 1518℃, 1520℃, 1522℃, 1524℃, 1526℃, 1528℃) to avoid excessively high temperatures affecting the uniformity of the steel cross-section and low magnification quality.
[0052] There are no particular restrictions on the shape of the resulting billet, which can be determined according to the shape of the final product. For example, depending on the specifications of the final part to be formed, it is preferred that the continuous casting billet has a cross-section of about 410×530mm or about 300×400mm.
[0053] Preheating is performed before rolling to ensure that the temperature of the cast billet is preferably maintained above approximately 1200°C, more preferably approximately 1200–1250°C (e.g., 1205°C, 1210°C, 1215°C, 1220°C, 1225°C, 1230°C, 1235°C, 1240°C, 1245°C). Such temperatures ensure that the subsequent rolling process can proceed smoothly and that the final profile has ideal properties.
[0054] The present invention will now be described in further detail with reference to specific embodiments.
[0055] Example 1
[0056] Bainitic non-quenched and tempered steel, production process: converter → LF → RH → continuous casting → heating and rolling → air cooling → tempering.
[0057] The process involves electric arc furnace steelmaking or converter steelmaking using raw materials such as molten pig iron, scrap steel, ferroalloys, and slagging agents. The proportion of molten pig iron in the raw materials is approximately 80-82 wt%, with the remainder primarily consisting of scrap steel and / or ferroalloys. The slagging agent comprises lime and dolomite, with its main chemical composition being CaO + SiO + MgO. The steelmaking process is controlled to ensure that the carbon content in the obtained molten steel is approximately 0.07 wt% and the phosphorus content is approximately 0.01 wt%. After meeting the requirements, the steel is tapped into a prepared ladle. The temperature of the molten steel leaving the furnace is approximately 1650°C. During tapping, refining slag, lime, and other slagging agents are added, along with Al ingots for precipitation and deoxidation, and some Si, Mn, and Cr alloys are added.
[0058] The molten steel obtained through the above steelmaking process is refined in an LF furnace. Al particles are used for diffusion deoxidation, and the steel composition is adjusted to basically meet the alloy element content requirements of the bainitic non-quenched and tempered steel of this invention. The refining temperature is approximately 1630℃. Argon gas is used for stirring to homogenize the steel composition and temperature, while simultaneously causing inclusions in the molten steel to collide, grow, and float to the slag. The alloy element composition of the steel obtained after refining basically meets the composition requirements of the bainitic non-quenched and tempered steel of this invention.
[0059] The refined molten steel is then further degassed under RH vacuum. Specifically, the vacuum level is below approximately 67 Pa, and the degassed time is 15 minutes. The hydrogen content of the steel is ≤2.0 ppm, and the oxygen content is ≤20 ppm.
[0060] Then, continuous casting is performed at a temperature of approximately 1525℃. The resulting billet has a cross-sectional shape of approximately 410×530mm. The billet temperature is maintained at approximately 1220℃ before rolling. This is done using a rolling mill with rolls. The rolled product is a bar. After rolling, the bar is air-cooled to below 300℃ and then collected for tempering. It is then held in a furnace at 380℃ for 10 hours.
[0061] The composition of the bainitic non-quenched and tempered steel obtained in this embodiment is shown in Table 1:
[0062] Table 1 Chemical composition (mass fraction) of bainitic non-quenched and tempered steel in Example 1 / %
[0063] C Si Mn P S Cr Ni Mo Cu V Fe 0.13 0.74 2.36 0.013 0.003 0.78 0.04 0.06 0.03 0.06 margin
[0064] For rolled, air-cooled, and tempered steel, multiple Φ25mm steel bar samples were cut. The microstructure was analyzed to be bainite (mainly granular bainite and lath bainite) + a small amount of ferrite (e.g. Figure 1 As shown, the hardness, tested according to GB / T231.1, is 298-301 HBW, which meets the design requirements of 270-320 HBW for bainitic steel; the yield strength, tested according to GB / T228.1, is 801-802 MPa, the tensile strength is 948-950 MPa, the elongation is 15-15.5%, and the reduction of area is 44-48%; the impact energy, tested according to GB / T229, is 45-50 J, all of which meet the design requirements.
[0065] Example 2
[0066] Bainitic non-quenched and tempered steel, the composition content is shown in Table 2:
[0067] Table 2 Chemical composition (mass fraction) of bainitic non-quenched and tempered steel in Example 2 / %
[0068] C Si Mn P S Cr Ni Mo Cu V Fe 0.16 0.32 2.05 0.015 0.003 0.52 0.02 0.06 0.04 0.06 margin
[0069] The production process is exactly the same as in Example 1.
[0070] For rolled, air-cooled, and tempered steel, multiple Φ25mm steel bar samples were cut. The microstructure was found to be bainite (mainly granular and lath bainite) with a small amount of ferrite. According to GB / T 228.1, the yield strength was 701–703 MPa, the tensile strength was 910–915 MPa, the elongation was 13–13.5%, and the reduction of area was 35–30%. According to GB / T 229, the impact energy was 31–35 J. According to GB / T 231.1, the hardness of the steel was 285–289 HBW.
[0071] Comparative Example 1
[0072] The only difference from Example 1 is that the tempering process involves holding the material at a temperature of 6 hours.
[0073] For the rolled, air-cooled and tempered steel, multiple Φ25mm steel bar samples were cut and tested according to GB / T 228.1. The yield strength was 643-645MPa, the tensile strength was 987-993MPa, the elongation was 12-13%, and the reduction of area was 28-30%. According to GB / T 229, the impact energy was 9-18J. According to GB / T 231.1, the hardness of the steel was 303HBW.
[0074] Comparative Example 2
[0075] Bainitic non-quenched and tempered steel, the composition content is shown in Table 3:
[0076] Table 3 Chemical composition (mass fraction) of bainitic non-quenched and tempered steel in Comparative Example 2 / %
[0077] C Si Mn P S Cr Ni Mo Cu V Fe 0.23 0.61 1.84 0.010 0.003 0.18 0.02 0.07 0.04 0.09 margin
[0078] The production process is exactly the same as in Example 1.
[0079] For the rolled, air-cooled and tempered steel, multiple Φ25mm steel bar samples were cut and tested according to GB / T 228.1. The yield strength was 615~627MPa, the tensile strength was 901~913MPa, the elongation was 16~18%, and the reduction of area was 36~39%. According to GB / T 229, the impact energy was 10~20J. According to GB / T 231.1, the hardness of the steel was 287~290HBW.
[0080] A comparison with comparative examples reveals that the bainitic non-quenched and tempered steels obtained in Examples 1 and 2 of this invention can meet the requirements for high-strength and high-toughness steels. Compared with traditional quenched and tempered steels, the quenching and tempering process can be eliminated, allowing for direct cutting and use, thus improving production efficiency, reducing energy consumption, and minimizing environmental pollution. Compared with bainitic non-quenched and tempered steels containing more expensive alloying elements, cost control is superior.
[0081] The above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention shall be within the scope of protection of the pending claims of the present invention.
Claims
1. A method of producing a bainitic non-quenched and tempered steel, characterized in that, The process includes the following steps: electric furnace or converter steelmaking, refining, degassing, ingot casting or continuous casting, heating and rolling, air cooling and tempering; wherein, the temperature of the billet before rolling is maintained at 1200~1250℃, and after rolling, it is air cooled to below 300℃ and then tempered, the tempering temperature is 350-380℃, and the holding time is 8-12h; The bainitic non-quenched and tempered steel, by mass percentage, comprises 0.13% C, 0.74% Si, 2.36% Mn, 0.06% Mo, 0.78% Cr, and 0.06% V, with the remainder being Fe and non-removable impurities, including: 0.013% P, 0.003% S, 0.03% Cu, and 0.04% Ni. The bainitic non-quenched and tempered steel is mainly composed of granular bainite and lath bainite; according to GB / T 231.1, the hardness reaches 298~301HBW; according to GB / T 228.1, the yield strength is 801~802MPa, the tensile strength is 948~950MPa, the elongation is 15~15.5%, and the reduction of area is 44~48%; according to GB / T 229, the impact energy is 45~50J.
2. The preparation method according to claim 1, characterized in that, In the electric furnace or converter steelmaking process, the proportion of liquid pig iron in the raw materials is 80-82 wt%, and the remainder is scrap steel and / or ferroalloys.
3. The preparation method according to claim 1, characterized in that, In the electric furnace or converter steelmaking process, the slag-forming agent used includes lime and dolomite, whose main chemical components are CaO+SiO2+MgO.
4. The preparation method according to claim 1, characterized in that, In the electric furnace or converter steelmaking process, the steel is tapped after the C content in the molten steel is 0.05~0.10wt% and the P content is ≤0.015wt%. The tapping temperature of the molten steel is 1600~1700℃. During the tapping process, refining slag and lime are added to form slag, and Al ingots are added for precipitation deoxidation and some Si, Mn and Cr alloys are added.
5. The preparation method according to claim 1, characterized in that, The refining process includes, but is not limited to, LF furnace refining; And / or, in the refining process, Al particles are used for diffusion deoxidation, and the composition of the molten steel is adjusted to the range of alloy element content required for the bainitic non-quenched and tempered steel; And / or, in the refining process, the refining temperature is 1600~1650℃.
6. The preparation method according to claim 1, characterized in that, The degassing is performed under RH vacuum degassing at a vacuum level below 67 Pa for at least 15 minutes.
7. The preparation method according to claim 1, characterized in that, The casting temperature for continuous casting is 1515~1535℃.
Citation Information
Patent Citations
Bainite non-quenched and tempered steel and profiles and articles made therefrom
CN117701996A