Ultra-thin functional fabric for down jackets and preparation method thereof
By combining bamboo fiber into bamboo-like cotton fiber with elastic fiber and fluff, blending and electrostatic treatment, an ultra-thin functional fabric is prepared, which solves the problem of insufficient anti-drilling performance of traditional fabrics and improves the aesthetics and warmth of down jackets. sex while maintaining portability.
Patent Information
- Application Number
- CN202410715306.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-04
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-06-04
AI Technical Summary
Traditional down jacket fabrics have insufficient anti-down performance, which causes down to easily come out of the fabric, affecting the appearance and warmth of the garment. At the same time, increasing the thickness and weight of the fabric is detrimental to portability.
Bamboo fiber is expanded and mechanically processed to form bamboo-like cotton fiber, which is combined with elastic fiber and fluff. After blending, twisting and weaving, an ultra-thin functional fabric is prepared. Electrostatic charge is used to enhance the binding force between fluff and yarn to form Tightly woven construction to prevent down from poking through the fabric.
It achieves the effect of effectively preventing down from drilling out of the fabric, improving the aesthetics and warmth of the down jacket, while maintaining the lightness and comfort, and avoiding the increase in fabric thickness and weight.
Smart Images

Figure CN118272983B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of woven fabrics, and in particular to an ultra-thin functional fabric for down jackets and a preparation method thereof. Background Art
[0002] In the field of down jacket manufacturing, the selection and preparation technology of fabrics are crucial to the overall performance of down jackets. Traditional down jacket fabrics are often made of relatively thick materials. Although they can provide good warmth retention, they sacrifice the lightness and comfort of the clothing. At the same time, traditional fabrics have obvious deficiencies in anti-down drilling performance, which makes it easy for down to drill out of the fabric during use, affecting the appearance and warmth retention of the clothing.
[0003] In the prior art, in order to improve the anti-down drilling performance of down jackets, methods such as increasing fabric density, using coatings or laminations are usually adopted; however, while these methods enhance the anti-down drilling performance, they also often increase the thickness and weight of the fabric, which is not conducive to the portability of the clothing.
[0004] Therefore, a new technical solution is needed to solve the above existing problems. Summary of the invention
[0005] The invention overcomes the shortcomings of the prior art and provides an ultra-thin functional fabric for down jackets and a preparation method thereof.
[0006] To achieve the above object, the technical solution adopted by the present invention is: a method for preparing an ultra-thin functional fabric for down jackets, comprising the following steps:
[0007] S1, soaking the bamboo fiber in a dilute alkali solution with a mass concentration of 1-5% to expand the bamboo fiber;
[0008] S2, mechanically treating the expanded bamboo fibers to enhance curling and twisting effects, so that the bamboo fibers form a natural twisted shape similar to cotton fibers, thereby obtaining bamboo imitation cotton fibers;
[0009] S3, combining the bamboo-like cotton fiber with the base fiber to obtain a bamboo-like cotton base yarn, wherein the base fiber is an elastic fiber; twisting a plurality of strands of the bamboo-like cotton base yarn and sandwiching fluff to obtain a bamboo-like cotton composite yarn;
[0010] S4. The bamboo-like cotton composite yarn is woven into fabric through a weaving process to obtain an ultra-thin functional fabric for down jackets.
[0011] In a preferred embodiment of the present invention, in S1, the diluted alkali solution used is a NaOH solution; the mass ratio of bamboo fiber to the diluted alkali solution is 1:10-1:20, the temperature is controlled at 25-60°C, and the time is controlled at 60-120min.
[0012] In a preferred embodiment of the present invention, in S2, the preparation of bamboo imitation cotton fiber includes the following steps:
[0013] S21, crushing, cutting and combing the expanded bamboo fibers in sequence, so that the length of the bamboo fibers is controlled to be 5-16 cm and the diameter is controlled to be 15-30 μm;
[0014] S22, stretching and twisting the thinned bamboo fibers by a crimping machine, so that the bamboo fibers form a twisted shape similar to cotton fibers;
[0015] S23, heating the curled bamboo fiber at a temperature of 180-210° C. for 20-30 seconds, and cooling it to 25-30° C. within 10 seconds to achieve shaping, thereby obtaining a bamboo imitation cotton fiber;
[0016] In S22, the curling blade spacing is set at 5-10 mm, the curling roller speed is 200-300 m / min, the stretching ratio is 1.5-2.0 times, and the curling angle is set to 30°-45°, so that the curvature of the bamboo imitation cotton fiber is 100-120 pieces / 10 cm.
[0017] In a preferred embodiment of the present invention, in S3, the elastic fiber selected as the base fiber is polyester; the selected bamboo imitation cotton fiber is 20-30 parts, the polyester is 40-60 parts, and the fluff is 5-10 parts.
[0018] In a preferred embodiment of the present invention, in S3, a blending machine is used to combine the bamboo imitation cotton fiber with the base fiber to obtain the bamboo imitation cotton base yarn, wherein the blending ratio of the bamboo imitation cotton fiber to polyester is 1:1.5-1:2.
[0019] In a preferred embodiment of the present invention, in S3, a plurality of strands of bamboo imitation cotton fiber basic yarns are twisted by a twisting machine; wherein the number of strands twisted is 2-3 strands; and at the same time, when fluff is sandwiched in the twisting process, the fluff is interlaced with the adjacent plurality of bamboo imitation cotton fiber basic yarns.
[0020] In a preferred embodiment of the present invention, in S3, an electrostatic generator with an output power of 5-10W is used to apply electrostatic charge to the obtained bamboo-like cotton composite yarn, the voltage is controlled at 5-8kV, and the current is not greater than 1mA; in S3, the electrostatic generator is used to apply electrostatic charge to the obtained bamboo-like cotton composite yarn, which can make the fluff attract each other under the action of static electricity, and promote the bamboo-like cotton base yarns to get closer together, thereby improving the anti-down drilling performance of the obtained ultra-thin performance fabric for down jackets.
[0021] In a preferred embodiment of the present invention, in S4, the weaving process used is a weaving process, a plurality of bamboo-like cotton composite yarns are used as warp and weft respectively, and the weaving density is 250T-400T.
[0022] An ultra-thin functional fabric for down jackets is prepared by adopting the above-mentioned method for preparing the ultra-thin functional fabric for down jackets.
[0023] A down jacket comprises: an inner liner fabric, filling down arranged inside the inner liner fabric, and an outer shell fabric arranged on the outer layer of the inner liner fabric, characterized in that the material of the inner liner fabric and the outer shell fabric are both the ultra-thin functional fabric for down jackets.
[0024] The present invention solves the defects existing in the background technology and has the following beneficial effects:
[0025] (1) The present invention provides a method for preparing an ultra-thin functional fabric for a down jacket, wherein bamboo fiber is made into bamboo imitation cotton fiber, which is then combined with elastic fiber and fluff, and then blended, twisted and woven to finally obtain an ultra-thin functional fabric for a down jacket. The ultra-thin functional fabric can effectively prevent down from leaking out of the fabric, thereby improving the aesthetics and warmth retention of the down jacket. Compared with the prior art, the thickness and weight of the fabric itself are reduced, thereby ensuring the lightness and comfort of the down jacket.
[0026] (2) The present invention provides a method for preparing an ultra-thin functional fabric for a down jacket, wherein bamboo fiber is selected as fabric fiber, and through puffing and curling treatment, the bamboo fiber is formed into a twisted shape similar to cotton fiber, which can increase the friction and cohesion between fibers, reduce the gaps between fibers and other fibers, and form a tight interwoven structure, thereby effectively preventing down from drilling out of the fabric; in addition, compared with the natural twisted shape of naturally grown cotton fibers, the artificial twisted shape of the bamboo imitation cotton fiber can control its size and twist degree, which is beneficial to improving the uniformity of the fabric fibers and reducing the gaps between fibers, thereby further improving the anti-drilling down performance.
[0027] (3) The present invention provides an ultra-thin functional fabric for down jackets. During the preparation process, the length, diameter and curling degree of the fibers are precisely controlled to effectively control the uniformity of the fibers in the fabric. Furthermore, in the process of twisting the bamboo-like cotton basic yarn, fluff is added to make the fluff and the adjacent bamboo-like cotton basic yarns intertwine with each other, and the binding force between the fluff and the bamboo-like cotton basic yarn is increased by static electricity. This can not only improve the strength of the obtained bamboo-like cotton composite yarn, but also further reduce the gaps between the yarns inside the fabric, thereby avoiding an increase in the thickness of the fabric itself. On the basis of maintaining the light and thin characteristics, the anti-down drilling performance of the fabric is improved, so that the final down jacket is lighter when worn, which is beneficial to improving the portability and storage of the down jacket. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art are briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For those of ordinary skill in the art, other drawings can be obtained based on these drawings without creative work.
[0029] Figure 1 It is a step diagram of a method for preparing an ultra-thin functional fabric for down jackets according to a preferred embodiment of the present invention. DETAILED DESCRIPTION
[0030] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0031] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein. Therefore, the protection scope of the present invention is not limited to the specific embodiments disclosed below.
[0032] like Figure 1 As shown, a method for preparing an ultra-thin functional fabric for a down jacket comprises the following steps:
[0033] S1, soaking the bamboo fiber in a dilute alkali solution with a mass concentration of 1-5% to expand the bamboo fiber;
[0034] S2, mechanically treating the expanded bamboo fibers to enhance curling and twisting effects, so that the bamboo fibers form a natural twisted shape similar to cotton fibers, thereby obtaining bamboo imitation cotton fibers;
[0035] S3, combining the bamboo-like cotton fiber with the base fiber to obtain a bamboo-like cotton base yarn, wherein the base fiber is an elastic fiber; twisting a plurality of strands of the bamboo-like cotton base yarn and sandwiching fluff to obtain a bamboo-like cotton composite yarn;
[0036] S4. The bamboo-like cotton composite yarn is woven into fabric through a weaving process to obtain an ultra-thin functional fabric for down jackets.
[0037] It is worth explaining that the natural twisting form of cotton fiber is a torsional form with a directional spiral feature formed during the growth process of cotton fiber. It usually appears as a flat strip with positive and negative spiral twists, which is most obvious in the middle section of the fiber, and the degree of twist is usually expressed by the number of 180° twists per centimeter, that is, the degree of twist. The formation of the natural twisting form of cotton fiber is mainly due to the interaction force between cellulose molecules and the influence of the second law of thermodynamics. The two adjacent chair-type six-membered rings of the cellulose macromolecule are turned 180° to form its own twisting characteristics. The natural twisting form of cotton fiber is an important source of the good elasticity and resilience of cotton fiber. When the fiber is subjected to external force, this twisting form helps the cotton fiber to return to its original state. In addition, the twisting form can also reduce the gaps between fibers and reduce the possibility of fillers drilling out of the fabric, thereby enhancing the durability and warmth of the fabric. Therefore, the natural twisting form of cotton fiber is one of its unique and important physical properties, which has a positive effect on improving the performance of fibers and fabrics.
[0038] However, it is worth pointing out that due to the influence of various environmental factors during the growth process of cotton fibers, the natural twist morphologies of different cotton fibers are often quite different. Excessive differences will affect the neatness and uniformity of the fabric fibers, resulting in more gaps in the fabric, affecting the anti-down performance of the fabric. If the cotton fibers are regularized and screened, the cost required is too high, which is not conducive to the promotion of production. In addition, sea island cotton has the highest twist degree, followed by upland cotton, while Asian cotton and African cotton have the lowest twist degree. Cotton fibers with high twist degrees have better adhesion, and their spinning, web and strip forming performance are also better. However, correspondingly, sea island cotton has the lowest output, and therefore the cost is too high, making it difficult to promote and apply.
[0039] It is worth further explaining that, compared with the natural twisting form of naturally grown cotton fibers, the artificial twisting form of bamboo-like cotton fibers, which is similar to the natural twisting form of cotton fibers, is more advantageous in many aspects. First, the artificial twisting form is more controllable. In the production process of bamboo-like cotton fibers, the twisting degree and form of the fibers can be precisely adjusted by precisely controlling the process parameters such as fiber stretching, heating and cooling, so that the twisting form of bamboo-like cotton fibers is more consistent and stable, which is beneficial to the fiber arrangement and weaving in the subsequent textile processing. Secondly, the artificial twisting form is beneficial to improving the uniformity of fabric fibers. Due to the consistency and stability of the artificial twisted morphology, the bamboo-like cotton fiber can be more evenly distributed in the fabric during the weaving process, avoiding the problem of uneven fiber distribution caused by differences in fiber morphology. The uniform fiber distribution can make the fabric flatter and smoother, and improve the appearance quality and feel of the fabric. Finally, the artificial twisted morphology helps to reduce the gaps between the fabric fibers. By precisely controlling the artificial twisted morphology of the bamboo-like cotton fiber, the fibers can be made to fit more closely together and the gaps between the fibers can be reduced, which can not only improve the warmth and breathability of the fabric, but also enhance the wear resistance and anti-pilling properties of the fabric.
[0040] Therefore, it can be concluded that compared with the natural twisting form of naturally grown cotton fibers, the artificial twisting form of bamboo-like cotton fibers is more controllable, and this artificial twisting form has a positive effect on improving the uniformity of fabric fibers and reducing the gaps between fibers, which makes bamboo-like cotton fibers have a wider application prospect and market demand in textile manufacturing.
[0041] In addition, bamboo fiber is a renewable material, and using bamboo fiber as raw material is beneficial to environmental protection and sustainable development. At the same time, bamboo fiber has good air permeability and moisture absorption, which can improve the comfort of the fabric. Furthermore, bamboo fiber as raw material has good wear resistance, which can improve the wear resistance of the fabric, thereby extending the service life of the down jacket.
[0042] In S1, when the bamboo fiber is soaked in a dilute alkali solution, the dilute alkali solution is a NaOH solution; the mass ratio of the bamboo fiber to the dilute alkali solution is 1:10-1:20, the temperature is controlled at 25-60°C, and the time is controlled at 60-120min.
[0043] It is worth noting that the natural twisted morphology of cotton fiber is mainly formed by the arrangement and crystal structure of the cellulose molecular chains inside it; therefore, in order to imitate this morphology, the present invention uses a dilute alkali solution to treat bamboo fiber. Bamboo fiber contains a large amount of cellulose. When bamboo fiber is soaked in a dilute alkali solution, the hydroxide ions in the dilute alkali solution will react with the primary hydroxyl groups on the cellulose macromolecular chain. In this process, the hydroxide ions will replace the hydrogen atoms on the primary hydroxyl groups to form an intermediate product called alkali cellulose; this substitution reaction will cause the hydrogen bonds between the cellulose molecular chains to be destroyed, thereby making the originally regular crystal structure loose. When this loose structure is fixed in the subsequent processing process, the fiber will present a puffed state, and the puffed fiber will become more curly and twisted in shape, thereby imitating the natural twisted morphology of cotton fiber.
[0044] Specifically, in S1, when the bamboo fiber is puffed with NaOH solution, the concentration of the NaOH solution is preferably 1-3%, and the volume ratio of the bamboo fiber mass to the dilute alkali solution is preferably 1:13-1:15; after the bamboo fiber is soaked with NaOH solution, the bamboo fiber is fully washed with clean water until it is neutral, and the residual solution on the surface is washed away and then dried for use.
[0045] In S2, the preparation of bamboo imitation cotton fiber includes the following steps:
[0046] S21, crushing, cutting and combing the expanded bamboo fibers in sequence, so that the length of the bamboo fibers is controlled to be 5-16 cm and the diameter is controlled to be 15-30 μm;
[0047] S22, stretching and twisting the thinned bamboo fibers by a crimping machine, so that the bamboo fibers form a twisted shape similar to cotton fibers;
[0048] S23, heating the curled bamboo fiber at a temperature of 180-210° C. for 20-30 seconds, and cooling it to 25-30° C. within 10 seconds to achieve shaping, thereby obtaining bamboo imitation cotton fiber.
[0049] Specifically, in S21, the expanded bamboo fibers are first crushed using a crusher to initially reduce the length and diameter of the crushed bamboo fibers; then, the crushed bamboo fibers are sent to a cutting machine for cutting to further control their length within the range of 5-16 cm; finally, the cut bamboo fibers are combed using a combing machine to remove impurities during the combing process and control the diameter of the bamboo fibers within the range of 15-30 μm, thereby enabling the length and diameter of the bamboo fibers to be controlled within a selected range.
[0050] Specifically, in S22, the refined bamboo fibers are fed into a crimping machine, and the stretching and twisting functions of the crimping machine are used to make the bamboo fibers form a twisted shape similar to that of cotton fibers; during the curling process, the stretching force and twisting angle of the crimping machine are adjusted as needed to obtain the desired curling effect, that is, the desired curvature of the bamboo imitation cotton fibers; preferably, the curvature of the bamboo imitation cotton fibers is controlled to be 100-120 pieces / cm by using the crimping machine for multiple times.
[0051] Preferably, the specific steps of using a crimping machine to process the bamboo fiber include:
[0052] The first step is to pre-treat the bamboo fiber, control the temperature of the bamboo fiber at 80-100°C and the moisture content at 15%-20%;
[0053] The second step is to select the FA series crimping machine and set the working temperature to 90-110℃ to ensure that the fiber is in a softened state during the crimping process; the crimping knife spacing is set to 5-10mm, the crimping roller speed is 200-300m / min, the stretching ratio is 1.5-2.0 times, and the crimping angle is set to 30-45°. The crimping density is controlled by the crimping roller speed and the crimping knife spacing, and the curvature of the bamboo imitation cotton is controlled to 100-120 pieces / cm;
[0054] The third step is to use a microscope or other testing equipment to measure the curvature of the bamboo fiber after the curling treatment, screen out unqualified products, and ensure that it is within the range of 100-120 pieces / cm; at the same time, according to the test results, appropriately adjust the parameters of the crimping machine to optimize the treatment effect;
[0055] In actual use, the puffed bamboo fiber after combing is continuously fed into the crimping machine; first, it enters the area between the crimping knife and the crimping roller, and a certain stretching force is applied to make the bamboo fiber fully stretched, and the stretching ratio is usually set at 1.7 times; multiple crimping knives are arranged on the crimping machine, and there is a set spacing of 7mm between the crimping rollers. The crimping knives apply mechanical force to the bamboo fiber passing through, and the surface of the crimping roller has uneven textures. When it cooperates with the crimping knives, the bamboo fiber is sandwiched between the two; when the bamboo fiber passes between the crimping knife and the crimping roller, the fiber is repeatedly bent and compressed under the clamping and friction of the two, resulting in alternating positive and negative curling, forming a positive and negative spiral structure; in actual use, the crimping knife spacing determines the tightness and frequency of the curling, the crimping knife angle affects the curling morphology of the fiber, and the crimping roller speed determines the speed at which the fiber passes through the crimping area, thereby affecting the fineness of the curling. By controlling the parameters of the crimping machine, the fiber curvature can reach 100-120 pieces / cm.
[0056] It is worth mentioning that compared with the sea island cotton with the highest natural curvature, the curvature of sea island cotton is 80-120 / cm. The bamboo imitation cotton fiber produced by a crimping machine has a more stable curvature, which is conducive to industrial promotion. In addition, compared with the upland cotton with a curvature of 39-65 / cm, and the Asian cotton and African cotton with a curvature of 18-40 / cm, the curvature of bamboo imitation cotton has a significant advantage and can have better adhesion.
[0057] In S3, the elastic fiber selected as the base fiber is polyester; the selected bamboo imitation cotton fiber is 20-30 parts, the polyester is 40-60 parts, and the fluff is 5-10 parts; preferably, the selected polyester has a diameter of 20-35 μm; the selected fluff is cashmere wool, and the fiber diameter is 14-18 μm.
[0058] In S3, polyester is selected as the elastic fiber as the base fiber; 20-30 parts of bamboo imitation cotton fiber, 40-60 parts of polyester, and 5-10 parts of fluff are selected; a blending machine is used to combine the bamboo imitation cotton fiber with the base fiber to obtain a bamboo imitation cotton basic yarn, wherein the blending ratio of the bamboo imitation cotton fiber to the polyester is 1:1.5-1:2; a doubling machine is used to doubling and twisting a plurality of strands of the bamboo imitation cotton basic yarn; wherein the number of doubling and twisting strands is 2-3 strands; at the same time, when the fluff is sandwiched in the doubling and twisting process, the fluff is interlaced with the adjacent strands of the bamboo imitation cotton fiber basic yarn, that is, according to the bamboo imitation cotton basic yarn and cashmere basic yarn, the doubling and twisting ratio is 1:1.5-1:2. The cashmere wool is evenly distributed between the bamboo-like cotton fiber basic yarns through a feeding device in a ratio of 2:1-4:1, and the fibers made of the cashmere wool and the remaining bamboo-like cotton basic yarns are used to form new yarns through the operation of a twisting machine; subsequently, an electrostatic generator with an output power of 5-10W is used to apply electrostatic charge to the obtained bamboo-like cotton composite yarn, the voltage is controlled at 5-8kV, and the current is not more than 1mA, which can make the cashmere attract each other under the action of static electricity, and promote the bamboo-like cotton basic yarns to be further brought closer, thereby improving the anti-down drilling performance of the obtained ultra-thin performance fabric for down jackets.
[0059] It is worth mentioning that the high-curvature bamboo-like cotton fiber makes the fibers more tightly bonded, the high-elastic polyester makes the ultra-thin performance fabric more elastic, and the fluff is used to attract each other under the action of static electricity, further reducing the gap between the fibers. The combination of the three can produce ultra-thin functional fabrics with good anti-down performance.
[0060] Specifically, in S4, the weaving process adopted is the weaving process, and a number of bamboo-like cotton composite yarns are used as warp and weft respectively, and the weaving density is 250T-400T; it is worth noting that the woven fabric is formed by interlacing the yarns in the warp and weft directions through a loom in the form of shuttle, and has the characteristics of compact structure, high strength, good wear resistance, etc. As a down jacket fabric, it can provide basic warmth and protection functions.
[0061] An ultra-thin functional fabric for down jackets is prepared by the above-mentioned method for preparing an ultra-thin functional fabric for down jackets; it is worth noting that according to actual needs, the required weaving process can be selected to weave the bamboo imitation cotton composite yarn into an ultra-thin functional fabric for down jackets, preferably using a weaving process.
[0062] A down jacket comprises: an inner liner fabric, filling down arranged inside the inner liner fabric, and an outer shell fabric arranged on the outer layer of the inner liner fabric; the materials of the inner liner fabric and the outer shell fabric are both ultra-thin functional fabrics for down jackets; the down jacket made of the ultra-thin functional fabric for down jackets provided by the present invention not only has good lightness, but also can effectively prevent down from drilling out, thereby effectively improving the warmth retention and durability of the down jacket, and has good application prospects.
[0063] Embodiment 1
[0064] The first embodiment of the present invention is based on the above-mentioned method for preparing the ultra-thin functional fabric for down jackets, and specifically comprises the following steps:
[0065] A1. Select bamboo fiber as the source of bamboo fiber and as fabric fiber, expand the bamboo fiber, soak it in 1% NaOH solution, the volume ratio of bamboo fiber mass to dilute alkali solution is 1:13, and soak it at 55℃ for 60min;
[0066] A2. Use a crusher, a cutter and a carding machine to crush, cut and card the expanded bamboo fiber in sequence, so that the length of the bamboo fiber is controlled at 5 cm and the diameter is controlled at 15 μm; use a crimping machine to crimp the bamboo fiber, so that the average curvature of the bamboo fiber is controlled at 110 / cm; use a hot air blower to heat the curled bamboo fiber at 180°C for 20 seconds and then quickly cool and shape it to obtain bamboo imitation cotton fiber; specifically, select a FA series crimping machine, set the working temperature to 100°C, the crimping knife spacing to 7mm, the crimping roller speed to 250m / min, the stretching ratio to 1.7 times, and the crimping angle to 40°;
[0067] A4, 20 parts of the obtained bamboo imitation cotton fiber are selected and blended with 40 parts of polyester using a blending machine with a blending speed of 150 turns / min to obtain a bamboo imitation cotton basic yarn; a doubling machine with a doubling speed of 150 turns / min is used to doubling and twisting the obtained bamboo imitation cotton basic yarn with three strands as the number of strands, with an S twist direction, and 5 parts of cashmere wool are sequentially added between adjacent bamboo imitation cotton basic yarns during the doubling and twisting process, that is, fibers made of cashmere wool are sandwiched between any two strands of bamboo imitation cotton basic yarns, and the fibers made of cashmere wool are combined with the remaining bamboo imitation cotton yarns through the operation of the doubling and twisting machine. The imitation cotton basic yarn is combined with the new yarn to obtain the bamboo imitation cotton composite yarn; the diameter of the selected polyester is 20-35 μm, the selected wool is cashmere wool, and the fiber diameter is 14-18 μm; an electrostatic generator with an output power of 10 W is used, the voltage is controlled at 5 kV, the current is 1 mA, and the ambient humidity is 50%-55% and the ambient temperature is 25-30° C. The processing time is controlled at 15 s, and an electrostatic charge is applied to the obtained bamboo imitation cotton composite yarn, so that the wool attracts each other under the action of electrostatics, and the bamboo imitation cotton basic yarns are further brought closer together;
[0068] A5. The bamboo-like cotton composite yarn was woven by a weaving process using a loom at a speed of 300 rpm, and the bamboo-like cotton composite yarn was used as warp and weft respectively. The weaving density, i.e., the T number was 400T, and an ultra-thin functional fabric sample 1 was obtained.
[0069] Embodiment 2
[0070] Based on Example 1, the raw materials of the bamboo-like cotton composite yarn in Example 1 were used in different proportions to prepare fabric samples, and sample 2, sample 3, sample 4, sample 5, and sample 6 were prepared respectively.
[0071] Control group 1
[0072] Based on Example 1, the difference is that natural Asian cotton fiber is directly used as the fabric fiber, blended with polyester, and fluff is sandwiched in the twisting process after blending, and finally sample 7 is obtained by weaving.
[0073] Control group 2
[0074] Based on Example 1, the difference is that natural Asian cotton fiber is directly used as the fabric fiber, blended with polyester, and no fluff is inserted in the twisting process after blending, and sample 8 is directly produced by weaving.
[0075] Control group three
[0076] Based on Example 1, the difference is that after the bamboo imitation cotton basic yarn is prepared, no fluff is added in the subsequent twisting process, and the bamboo imitation cotton composite yarn is directly obtained. At the same time, no electrostatic treatment is performed, and finally sample 9 is obtained by weaving.
[0077] Control group 4
[0078] Based on Example 1, the difference is that: the ultra-thin functional fabric finally prepared is coated by using a wet coating method, polyurethane is added to the fabric at a standard of 150g / ㎡, and sample 10 is obtained after drying for 8 hours, wherein the ratio of the paint to the curing agent of the polyurethane coating is 1:1.
[0079] According to the obtained samples, the thinness and anti-down performance of these samples are tested respectively;
[0080] Specifically, for the lightness and thinness of the fabric, choose to weigh and measure the thickness, which is reflected by the weight per unit area and the thickness of the fabric;
[0081] Specifically, for the anti-down drilling performance of the fabric, the garment transfer method is adopted, 2㎡ of the above samples are selected respectively, 90% white goose down is selected as the filling down, 150 grams are weighed, the down is evenly filled into each compartment of the down jacket, and the M-size down jacket is cut to be used as the sample, and the number of down, feathers and down fibers drilled out from the inside of the sample per unit relative area is used for evaluation, that is, the amount of down escape; Specifically, first, a box-type anti-down drilling test machine is prepared; then, according to the GB / T31907 standard, the length, chest circumference, sleeve length, sleeve width and other dimensions of the sample are measured, and the clothing surface area of the sample is calculated; then, the whole sample is placed in the rotary box of the box-type anti-down drilling test machine, and 15 After that, the test machine was started, the rotation number was set to 1440 times, the speed was set to 42r / min, and the silicone rubber shaped ball was brought to a certain height through the constant speed rotation of the rotary box, and then impacted the sample in the box, thereby simulating the various squeezing, rubbing, collision and other effects that the tested sample was subjected to during use; after the test process was completed, the number of down, feathers, down fibers and other materials drilled out from the inside of the sample was collected; based on the collected data, the number of down, feathers, down fibers and other materials drilled out from the inside of the sample per unit relative area was calculated, that is, the amount of down escaped = (number of down escaped) / (surface area of clothing); finally, the anti-down drilling performance of the sample was evaluated, and the amount of down escaped was 0-1 root / 10cm 2 The down-proof performance of the sample is excellent, and the amount of down leakage is 2-5 pieces / 10cm 2 The down-proof performance of the sample is average, and the amount of down escaped is greater than 5 pieces / 10cm 2 The anti-down drilling property of the sample is poor;
[0082] The test results obtained according to the selected test methods for thinness and anti-down performance are shown in Table 1:
[0083] Table 1. Test results of sample thinness and anti-downfall performance
[0084]
[0085]
[0086] According to the data in Table 1, it can be concluded that compared with samples 7 and 8 directly using cotton fibers, samples 1-6 using bamboo fibers all exhibit better anti-down properties, because the natural curvature of cotton fibers is not as controllable as the artificial curvature of bamboo-like cotton fibers made from bamboo fibers, which makes the structure looser and causes the down to escape easily; it is worth noting that when the amount of polyester increases, the anti-down property decreases, because the increase in polyester reduces the proportion of bamboo-like cotton fibers, making the fabric structure relatively loose, and more bamboo fibers, that is, more bamboo-like cotton fibers, can better hold the fibers together, thereby making the fabric more comfortable. The structure is tighter; in addition, by comparing sample 7 and sample 8, it can be concluded that the use of down can further improve the down-proof performance of the fabric, because the fibers in the fabric can be more tightly combined under the electrostatic effect of the charged down; in addition, by changing the weight of the fabric raw materials, the various samples obtained are different in weight and thickness, because the density and volume of different raw materials are different, but compared with sample 10 treated with traditional coating, samples 1-6 obtained by the method of the present invention do not need to add additional coating, thus avoiding excessive increase in weight and thickness, which is beneficial to improving the lightness of the down jacket.
[0087] In addition, it is worth mentioning that in the preparation method provided by the present invention, by controlling the length, diameter and curvature of the bamboo fiber, the uniformity of the fabric fiber can be improved, which is beneficial to improving the performance of the fabric.
[0088] Control group five
[0089] Based on Example 1, the difference is that the expanded bamboo fibers are not crushed, cut and combed, that is, the uniformity of the bamboo imitation cotton fibers is not controlled, and the curling treatment and subsequent steps are directly performed to prepare sample 11.
[0090] Control group 6
[0091] Based on control group one, the difference is that the general fiber length of natural Asian cotton is 15-24mm, and the fiber diameter is 23-26μm. Therefore, a crusher, a cutter and a carding machine are used to crush, cut and card the natural Asian cotton fibers in sequence, so that the length of the natural Asian cotton fibers is controlled at 20mm and the diameter is controlled at 25μm; no curling treatment is performed, and then blending with polyester is performed, and subsequent treatment is performed to prepare sample 12.
[0092] Control group seven
[0093] Based on control group six, the difference is that the general fiber length of natural sea island cotton is 35-50mm, and the fiber diameter is 15-20μm, so the natural Asian cotton fiber is replaced by natural sea island cotton fiber, and the natural Asian sea island cotton fiber is crushed, cut and combed in sequence using a crusher, a cutter and a combing machine to control the length of the natural Asian cotton fiber to 45mm and the diameter to 20μm; no curling treatment is performed, and then it is blended with polyester, and subsequent treatment is performed to prepare sample 13.
[0094] For samples 11, 12 and 13, the uniformity and flatness of the fabric were tested in combination with samples 1 and 7.
[0095] Specifically, the uniformity detection method for the fabric is as follows: each sample is cut into a size of 20cm*20cm; a microscope or surface analyzer is used to fix the sample on the microscope platform to ensure that the sample is flat and close to the platform, and 5 points are randomly selected in the central area of the sample, in an area of 10cm*10cm, and high-resolution images are collected at each point to calculate the number of fibers therein and obtain the fiber density of each point; the image analysis software is used to calculate the uniformity of fiber distribution at each point, and the result is expressed as a uniformity index in the range of 0-1, and the closer the value is to 1, the better the uniformity; specifically, uniformity index = 1-(fiber density standard deviation) / (average fiber density); the uniformity index of each sample is recorded; the uniformity test results are shown in Table 2.
[0096] Table 2. Sample uniformity test results
[0097]
[0098] According to the analysis in Table 2, compared with sample 11 which also uses bamboo imitation cotton but is not combed, the uniformity index of sample 1 is significantly improved. Similarly, compared with sample 7 which is not combed, the uniformity index of sample 12 is also improved, indicating that the fibers after crushing and combing are more evenly distributed in the fabric, that is, crushing and combing can effectively improve the uniformity of the fabric; at the same time, the artificial curvature of sample 11 is greater than the natural curvature of sample 12, and less than the natural curvature of sample 13, and the uniformity index also shows corresponding characteristics. Therefore, the high curvature of the fiber has a positive effect on improving the uniformity of the fabric; however, after combing, sample 13, which has the highest natural curvature, has a worse uniformity than sample 1. This is because the curvature of the artificially made bamboo imitation cotton fiber is more controllable, and it has better stability than the natural sea island cotton fiber, which can better improve the uniformity of the fabric.
[0099] Specifically, the flatness test method for the fabric is as follows: cut each sample into a size of 20cm*20cm to ensure that there are no obvious wrinkles on the sample surface; use a flatness tester, such as a surface profiler, to lay the sample flat on the test platform and fix the four sides with clamps to make the sample surface as flat as possible; start the flatness tester, set the scanning area to a 10cm*10cm central area, the scanning interval to 1mm, record the value of the sample surface undulation in μm, and the measurement results include the maximum height difference, the average height difference and the standard deviation; the flatness test results are shown in Table 3.
[0100] Table 3. Flatness test results of samples
[0101] Sample No. Maximum height difference / μm Average height difference / μm Standard deviation / μm Sample 1 20 5 3 Sample 7 60 25 15 Sample 11 40 15 10 Sample 12 30 10 7 Sample 13 25 8 5
[0102] According to the analysis in Table 3, similar to the results obtained from the uniformity analysis in Table 2, compared with sample 11 which also uses bamboo imitation cotton but is not combed, the maximum height difference and the average height difference of sample 1 are greatly reduced. Similarly, compared with sample 7 which is not combed, the standard deviation of sample 12 is also reduced. The fibers whose surfaces have been crushed and combed can make the fabric smoother; at the same time, the artificial curvature of sample 11 is greater than the natural curvature of sample 12, and less than the natural curvature of sample 13, and the flatness test results also show corresponding characteristics. Therefore, the high curvature of the fiber has a significant effect on improving the flatness; however, after combing, sample 13, which has the highest natural curvature, has a worse flatness performance than sample 1. This is because the curvature of the artificially made bamboo imitation cotton fiber is more controllable, and has better stability than the natural sea island cotton fiber, which can better improve the flatness of the fabric.
[0103] Therefore, it can be concluded that in the preparation method provided by the present invention, by controlling the length, diameter and curvature of the bamboo fibers, the uniformity and regularity of the fabric fibers can be effectively improved, thereby improving the overall quality of the fabric.
[0104] Furthermore, in the preparation method provided by the present invention, a curling machine is used to increase the curvature of the expanded and combed bamboo fiber. During the curling process, the parameters of the curling machine have different effects on the processing of the bamboo fiber. Experiments are conducted to further verify the description. The specific experimental steps are: first, several groups of bamboo fibers are soaked in a 1% NaOH solution with a fiber to solution volume ratio of 1:13 at 55°C for 60 minutes, and the expanded bamboo fiber is processed to a length of 5 cm and a diameter of 15 μm using a crusher, a cutter and a combing machine; then, five key parameters of the curling machine are selected for adjustment. The working temperature, curling knife spacing, curling roller speed, stretching ratio and curling angle are respectively adjusted. Several groups of bamboo fibers are divided into 5 corresponding groups, and each group of bamboo fibers is curled based on different parameters; finally, a microscope is used to take images of each group of fibers and the image analysis software is used to calculate the curvature of the fibers, and the average curvature and standard deviation of each group are calculated; the working temperature is 100℃, the curling knife spacing is 7mm, the curling roller speed is 250m / min, the stretching ratio is 1.7 and the curling angle is 40° as the standard group, and the experimental results obtained by changing the other parameters are shown in Tables 4, 5, 6, 7 and 8.
[0105] Table 4. Effect of the working temperature of the crimping machine on the curvature
[0106] Temperature / ℃ Degree of curvature / piece / cm Standard Deviation 90 90 6 100 110 5 110 95 7
[0107] Table 5. Effect of the crimping knife spacing of the crimping machine on the curvature
[0108] Curling knife spacing / mm Degree of curvature / piece / cm Standard Deviation 5 85 7 7 110 5 9 95 6
[0109] Table 6. Effect of the curling roller speed of the curling machine on the curvature
[0110]
[0111]
[0112] Table 7. Effect of the stretch ratio of the crimping machine on the curvature
[0113] Stretch ratio Degree of curvature / piece / cm Standard Deviation 1.5 80 7 1.7 110 5 2.0 100 8
[0114] Table 8. Effect of curling angle of curling machine on curvature
[0115] Curl angle / ° Degree of curvature / piece / cm Standard Deviation 30 85 6 40 110 5 50 95 7
[0116] According to the analysis of Tables 4 to 8, it can be concluded that too high temperature will reduce the curvature because it will damage the fiber to a certain extent, while too low temperature will reduce the curvature because the bamboo fiber is not fully softened; too small a curling knife spacing will cause the curvature of the bamboo fiber to interfere with each other, thereby reducing the curvature, while too large a curling knife spacing will result in insufficient curling processing; too fast a curling roller speed will damage the fiber, while too low a speed will result in insufficient processing; too large a stretching ratio will also damage the fiber, while too small a stretching ratio will make it impossible to fully curl the bamboo fiber; too large a curling angle will also cause the fiber to bend excessively, while too small a curling angle will make it difficult to retain the curvature formed by torsion; therefore, an operating temperature of 100°C, a curling knife spacing of 7mm, a curling roller speed of 250m / min, a stretching ratio of 1.7 times and a curling angle of 40° are the best parameters for optimizing the curvature of bamboo imitation cotton fiber. The curvature of bamboo imitation cotton fiber under these parameter combinations reaches 110 pieces / cm, which is significantly higher than other parameter combinations; at the same time, the standard deviation is also smaller, which means that the resulting curvature is more stable. It can be concluded that in the preparation method provided by the present invention, a crimping machine is used to increase the curvature of the expanded and combed bamboo fibers, and the processing parameters used are conducive to stably and significantly improving the curvature of the bamboo fibers.
[0117] In summary, the present invention provides an ultra-thin functional fabric for down jackets and a preparation method thereof. By selecting corresponding weight portions of bamboo fiber, polyester and fluff within a given range, the bamboo fiber can be processed into bamboo-spun cotton fiber with artificial curvature after puffing, mechanical curling and the like. The bamboo imitation cotton fiber is blended with polyester to obtain a bamboo imitation cotton basic yarn with a tight structure, which can achieve the anti-down effect of the fabric. Furthermore, by sandwiching fluff in the twisting process and performing electrostatic treatment, a bamboo imitation cotton composite yarn with a tighter structure can be formed, thereby further reducing the gaps between fibers inside the fabric, thereby further improving the anti-down drilling performance. At the same time, compared with the processing and production of traditional anti-down drilling fabrics in the prior art, the method provided by the present invention does not require the addition of additional coatings, thereby avoiding excessive increase in fabric weight and thickness, and can maintain the lightness of the fabric in addition to improving the anti-down drilling performance of the fabric, which is beneficial to improving the comfort and lightness of down jackets, and has good application prospects.
[0118] The above is based on the ideal embodiment of the present invention. Through the above description, relevant personnel can make various changes and modifications without departing from the technical concept of the present invention. The technical scope of the present invention is not limited to the content in the specification, and the technical scope must be determined according to the scope of the claims.
Claims
1. A method for preparing an ultra-thin functional fabric for down jackets, characterized in that: The following steps are involved: S1, soaking the bamboo fiber in a dilute alkali solution with a mass concentration of 1-5% to expand the bamboo fiber; S2, mechanically treating the expanded bamboo fibers to enhance curling and twisting effects, so that the bamboo fibers form a natural twisted shape similar to cotton fibers, thereby obtaining bamboo imitation cotton fibers; S3, combining the bamboo-like cotton fiber with the base fiber to obtain a bamboo-like cotton base yarn, wherein the base fiber is an elastic fiber; twisting a plurality of strands of the bamboo-like cotton base yarn and sandwiching fluff to obtain a bamboo-like cotton composite yarn; S4. The bamboo-like cotton composite yarn is woven into fabric through a weaving process to obtain an ultra-thin functional fabric for down jackets.
2. The method for preparing an ultra-thin functional fabric for down jackets according to claim 1, characterized in that: In S1, the dilute alkali solution is a NaOH solution; the mass ratio of bamboo fiber to the dilute alkali solution is 1:10-1:20, the temperature is controlled at 25-60° C., and the time is controlled at 60-120 min.
3. The method for preparing an ultra-thin functional fabric for down jackets according to claim 1, characterized in that: In S2, the preparation of bamboo imitation cotton fiber includes the following steps: S21, crushing, cutting and combing the expanded bamboo fibers in sequence, so that the length of the bamboo fibers is controlled to be 5-16 cm and the diameter is controlled to be 15-30 μm; S22, stretching and twisting the thinned bamboo fibers by a crimping machine, so that the bamboo fibers form a twisted shape similar to cotton fibers; S23, heating the curled bamboo fiber at a temperature of 180-210° C. for 20-30 seconds, and cooling it to 25-30° C. within 10 seconds to achieve shaping, thereby obtaining a bamboo imitation cotton fiber; In S22, the curling blade spacing is set at 5-10 mm, the curling roller speed is 200-300 m / min, the stretching ratio is 1.5-2.0 times, and the curling angle is set to 30°-45°, so that the curvature of the bamboo imitation cotton fiber is 100-120 pieces / 10 cm.
4. The method for preparing an ultra-thin functional fabric for down jackets according to claim 1, characterized in that: In S3, the elastic fiber selected as the base fiber is polyester; the selected bamboo imitation cotton fiber is 20-30 parts, the polyester is 40-60 parts, and the fluff is 5-10 parts.
5. The method for preparing an ultra-thin functional fabric for down jackets according to claim 4, characterized in that: In S3, a blending machine is used to combine the bamboo imitation cotton fiber with the base fiber to obtain the bamboo imitation cotton base yarn, wherein the blending ratio of the bamboo imitation cotton fiber to the polyester is 1:1.5-1:
2.
6. The method for preparing an ultra-thin functional fabric for down jackets according to claim 4, characterized in that: In S3, a plurality of strands of bamboo imitation cotton fiber basic yarns are twisted by a twisting machine; wherein the number of strands twisted is 2-3 strands; and at the same time, when fluff is sandwiched in the twisting process, the fluff is interlaced with the adjacent plurality of bamboo imitation cotton fiber basic yarns.
7. The method for preparing an ultra-thin functional fabric for down jackets according to claim 4, characterized in that: In S3, an electrostatic generator with an output power of 5-10W is used to apply electrostatic charge to the obtained bamboo-like cotton composite yarn, the voltage is controlled at 5-8kV, and the current is not greater than 1mA.
8. The method for preparing an ultra-thin functional fabric for down jackets according to claim 1, characterized in that: In S4, the weaving process adopted is a machine weaving process, a plurality of bamboo-like cotton composite yarns are used as warp and weft respectively, and the weaving density is 250T-400T.
9. An ultra-thin functional fabric for down jackets, characterized in that: The ultra-thin functional fabric for down jackets is prepared by the preparation method of any one of claims 1 to 8.
10. A down jacket, comprising: An inner liner fabric, filling down arranged inside the inner liner fabric, and an outer shell fabric arranged on the outer layer of the inner liner fabric, characterized in that the material of the inner liner fabric and the outer shell fabric are both the ultra-thin functional fabric for down jackets as described in claim 9.