A composite coating on the surface of a carbon-based material and its preparation method and application

By depositing carbon/silicon carbide gradient coating and silicon carbide coating on graphite base, the problem of poor binding strength between graphite base and CVD SiC coating is solved, and the stability and life of the product are improved, which is suitable for industrial production.

CN118291947BActive Publication Date: 2024-11-12湖南德智新材料股份有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410424266.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-09
Publication Date
2024-11-12
Estimated Expiration
2044-04-09

AI Technical Summary

Technical Problem

In the prior art, the thermal expansion coefficient between the graphite base and the CVD SiC coating does not match, resulting in poor binding force between the coating and the substrate, which easily leads to the coating falling off, affecting the stability and life of the product.

Method used

By depositing n-layer gradient coating on the surface of carbon-based material, the carbon element content of each layer is reduced from 2 to 40 wt%, and the silicon carbide coating is deposited on the side of the silicon carbide coating to improve Interface adaptability and bonding.

Benefits of technology

It effectively improves the bonding force between graphite and silicon carbide coating, reduces stress concentration and crack formation, extends the service life of the product, and is suitable for large-scale industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118291947B_ABST
    Figure CN118291947B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of composite materials, and provides a composite coating on the surface of a carbon-based material, and a preparation method and application thereof, wherein the composite coating comprises a carbon / silicon carbide gradient coating and a silicon carbide coating containing n layers of gradient coatings combined on the surface of the carbon-based material; n>1; along the direction from the surface of the carbon-based material to the silicon carbide coating, the carbon content of each layer of the carbon / silicon carbide gradient coating is 2 to 40wt%, and decreases successively, and the difference in carbon content between the first layer of gradient coating and the nth layer of gradient coating is not less than 3wt%; along the direction from the surface of the carbon-based material to the silicon carbide coating, the average grain size of each layer of the carbon / silicon carbide gradient coating is smaller than that of the silicon carbide coating, and increases successively. The present invention introduces a carbon / silicon carbide gradient coating between the graphite-based and silicon carbide coatings, improves the interface adaptability between the two, can reduce stress concentration and crack formation, and improves the stability and service life of the product.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of composite materials, and in particular to a composite coating on the surface of a carbon-based material, a method for preparing the composite coating on the surface of a carbon-based material, a composite coating on the surface of a carbon-based material prepared by the preparation method, a composite material and their applications. Background Art

[0002] GaN material is a new type of semiconductor material for the development of microelectronic devices and optoelectronic devices. The mainstream technology for the epitaxial growth of GaN thin films is MOCVD. Among them, graphite, as the supporting base for the epitaxial growth of GaN thin films, is an important component in the reaction chamber of MOCVD equipment. Since the gas used in the epitaxial growth process is ammonia, graphite is very susceptible to ammonia corrosion at high temperatures, and hydrocarbons will be released during the corrosion process, causing graphite to fall off and contaminate the GaN film. Therefore, it is necessary to coat the surface of the MOCVD graphite base.

[0003] Chemical vapor deposition is a commonly used coating preparation technology. It decomposes the gaseous precursor into solid materials at high temperature and makes them grow on the substrate surface. Currently, SiC coatings deposited by CVD are mostly used as coatings on the surface of graphite bases. However, there is a mismatch in thermal expansion coefficients between graphite and CVD SiC coatings, which leads to poor bonding between the coating and the substrate. This makes it easy for the coating to fall off during the epitaxial production process of the product, causing wafer failure and the product life not meeting the design requirements.

[0004] Therefore, developing a new product that can effectively improve the bonding force between graphite and silicon carbide coating and improve the stability and performance of the product is an urgent problem to be solved by technicians in this field. Summary of the invention

[0005] The purpose of the present invention is to solve the above-mentioned problems existing in the prior art, to provide a composite coating on the surface of a carbon-based material, and to provide a preparation method and related products of the composite coating on the surface of a carbon-based material, wherein the composite coating can effectively improve the bonding force between the graphite and silicon carbide coatings, and improve the stability and performance of the product.

[0006] In order to achieve the above-mentioned object, the first aspect of the present invention provides a composite coating on the surface of a carbon-based material, wherein the composite coating comprises a carbon / silicon carbide gradient coating bonded to the surface of the carbon-based material and a silicon carbide coating bonded to the other side of the carbon / silicon carbide gradient coating;

[0007] The carbon / silicon carbide gradient coating comprises n layers of gradient coating, n>1;

[0008] Along the direction from the surface of the carbon-based material to the silicon carbide coating, the carbon content in each layer of the carbon / silicon carbide gradient coating is 2 to 40 wt % and decreases successively, and the difference in carbon content between the first layer of the gradient coating combined on the surface of the carbon-based material and the nth layer of the gradient coating combined on one side of the silicon carbide coating is not less than 3 wt %;

[0009] Along the direction from the surface of the carbon-based material to the silicon carbide coating, the average grain size of each layer of the carbon / silicon carbide gradient coating is smaller than that of the silicon carbide coating and increases successively.

[0010] A second aspect of the present invention provides a method for preparing a composite coating on the surface of a carbon-based material, the method comprising:

[0011] (1) depositing a carbon / silicon carbide gradient coating comprising n layers of gradient coating on the surface of a carbon-based material, wherein n>1, and the deposition method is such that the carbon content of each layer of the carbon / silicon carbide gradient coating is 2 to 40 wt% along the direction from the surface of the carbon-based material to the silicon carbide coating, and decreases successively, and the difference in carbon content between the first layer of gradient coating combined on the surface of the carbon-based material and the nth layer of gradient coating combined on one side of the silicon carbide coating is not less than 3 wt%; at the same time, along the direction from the surface of the carbon-based material to the silicon carbide coating, the average grain size of each layer of the carbon / silicon carbide gradient coating is smaller than that of the silicon carbide coating, and increases successively;

[0012] (2) Depositing a silicon carbide coating on the surface of the carbon / silicon carbide gradient coating to obtain a composite coating.

[0013] A third aspect of the present invention provides a composite coating on the surface of a carbon-based material prepared by the method described above.

[0014] A fourth aspect of the present invention provides a composite material, the composite material comprising a carbon-based material and a composite coating bonded to the surface of the carbon-based material;

[0015] Wherein, the composite coating is the composite coating on the surface of the carbon-based material as described above.

[0016] A fifth aspect of the present invention provides the use of the above-mentioned carbon-based material surface composite coating or the above-mentioned composite material in the semiconductor field.

[0017] The present invention adopts the above technical solution to achieve the following beneficial effects:

[0018] (1) The present invention introduces a carbon / silicon carbide gradient coating between the graphite base and the silicon carbide coating, thereby improving the interface adaptability between the two, reducing stress concentration and crack formation, and improving product stability and service life;

[0019] (2) The preparation method provided by the present invention is simple and effective, suitable for large-scale industrial production, and has high process repeatability.

[0020] The endpoints and any values ​​of the range disclosed in this article are not limited to the precise range or value, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article. Herein, in the absence of special instructions, data ranges include endpoints. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 The figure shows an electron microscope image of the composite material prepared in Example 1 of the present invention, wherein 100 is a graphite substrate; 200 is a first gradient coating layer; 300 is a second gradient coating layer; 400 is a third gradient coating layer; and 500 is a silicon carbide coating layer. DETAILED DESCRIPTION

[0022] The specific embodiments of the present invention are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.

[0023] Unless otherwise defined, all scientific and technical terms used in the present invention have the same meanings as commonly understood by one of ordinary skill in the art to which the present invention relates.

[0024] A first aspect of the present invention provides a composite coating on the surface of a carbon-based material, the composite coating comprising a carbon / silicon carbide gradient coating bonded to the surface of the carbon-based material and a silicon carbide coating bonded to the other side of the carbon / silicon carbide gradient coating;

[0025] The carbon / silicon carbide gradient coating comprises n layers of gradient coating, n>1;

[0026] Along the direction from the surface of the carbon-based material to the silicon carbide coating, the carbon content in each layer of the carbon / silicon carbide gradient coating is 2wt% to 40wt% (for example, it can be 2wt%, 5wt%, 10wt%, 15wt%, 20wt%, 25wt%, 30wt%, 35wt%, 40wt% and any range between any two values), and decreases successively, and the carbon content difference between the first layer of gradient coating combined on the surface of the carbon-based material and the nth layer of gradient coating combined on one side of the silicon carbide coating is not less than 3wt% (for example, it can be 3wt%, 4wt%, 6wt%, 8wt%, 10wt%, 12wt%, 14wt%, 16wt%, 18wt% and any range between any two values);

[0027] Along the direction from the surface of the carbon-based material to the silicon carbide coating, the average grain size of each layer of the carbon / silicon carbide gradient coating is smaller than that of the silicon carbide coating and increases successively.

[0028] In some embodiments, the thermal expansion coefficient of the carbon-based material is 4×10 -6 ~7.5×10 -6 / k, density is 1.7~2.2g / cm 3 , the porosity is 5-25%, and the grain size is less than 20μm.

[0029] In some embodiments, the carbon-based material is selected from isostatic graphite and / or carbon fiber reinforced carbon, which can be commercially available.

[0030] In some embodiments, the thickness of the composite coating is 80 μm to 150 μm, for example, 80 μm, 100 μm, 120 μm, 140 μm, 150 μm, and any range between any two values.

[0031] In some embodiments, in the composite coating, the thickness of the carbon / silicon carbide gradient coating is 20% to 45% of the total thickness, for example, it can be 20%, 25%, 30%, 32%, 34%, 36%, 38%, 40%, 42%, 44%, 45% and any range between any two values.

[0032] In some embodiments, the thickness of each layer of the carbon / silicon carbide gradient coating is 5 μm to 25 μm, for example, 5 μm, 10 μm, 15 μm, 20 μm, 25 μm, and any range between any two values.

[0033] In some embodiments, n≥3, the content of carbon in the first layer of gradient coating is 12wt% to 40wt%, for example, it can be 12wt%, 14wt%, 16wt%, 18wt%, 20wt%, 22wt%, 24wt%, 26wt%, 28wt%, 30wt%, 32wt%, 34wt%, 36wt%, 38wt%, 40wt% and any range between any two values, and the content of carbon in the nth layer of gradient coating is 2wt% to 12wt%, for example, it can be 2wt%, 4wt%, 6wt%, 8wt%, 10wt%, 12wt% and any range between any two values.

[0034] In some embodiments, the average grain size of the first layer of gradient coating is 50nm to 150nm, for example, it can be 50nm, 60nm, 70nm, 80nm, 90nm, 100nm, 150nm and any range between any two values, and the average grain size of the nth layer of gradient coating is 300nm to 700nm, for example, it can be 300nm, 350nm, 400nm, 450nm, 500nm, 550nm, 600nm, 650nm, 700nm and any range between any two values.

[0035] In some embodiments, the carbon content difference between each layer is 1wt% to 12wt%, for example, it can be 1wt%, 2wt%, 4wt%, 6wt%, 8wt%, 10wt%, 12wt% and any range between any two values.

[0036] In some embodiments, the average grain size of the silicon carbide coating is 500nm to 1500nm, for example, 500nm, 600nm, 800nm, 1000nm, 1200nm, 1400nm, 1500nm and any range between any two values, preferably 800nm ​​to 1200nm.

[0037] In some embodiments, n>3, the carbon content in the first layer of gradient coating is 12wt%~40wt%, and the carbon content in the nth layer of gradient coating is 2wt%~12wt%; the average grain size of the first layer of gradient coating is 50~150nm, and the average grain size of the nth layer of gradient coating is 300~700nm.

[0038] In some preferred embodiments, n is 3, and the content of carbon in the first layer of the gradient coating is 12wt% to 40wt%, for example, it can be 12wt%, 14wt%, 16wt%, 18wt%, 20wt%, 22wt%, 24wt%, 26wt%, 28wt%, 30wt%, 32wt%, 34wt%, 36wt%, 38wt%, 40wt% and any range between any two values; the content of carbon in the second layer of the gradient coating is 10wt% to 15wt%, for example, it can be 10wt%, 12wt%, 14wt%, 15wt% and any range between any two values; the content of carbon in the third layer of the gradient coating is 2wt% to 10wt%, for example, it can be 2wt%, 4wt%, 6wt%, 8wt%, 10wt% and any range between any two values.

[0039] In some preferred embodiments, the average grain size of the first layer of gradient coating is 50nm~150nm, for example, it can be 50nm, 60nm, 70nm, 80nm, 90nm, 100nm, 150nm and any range between any two values, the average grain size of the second layer of gradient coating is 100nm~500nm, for example, it can be 100nm, 150nm, 200nm, 250nm, 300nm, 350nm, 400nm, 450nm, 500nm and any range between any two values, the average grain size of the third layer of gradient coating is 300nm~700nm, for example, it can be 300nm, 350nm, 400nm, 450nm, 500nm, 550nm, 600nm, 650nm, 700nm and any range between any two values.

[0040] In the present invention, the carbon content is determined by D-sims, and the average grain size is determined by EBSD.

[0041] A second aspect of the present invention provides a method for preparing a composite coating on the surface of a carbon-based material, the method comprising:

[0042] (1) depositing a carbon / silicon carbide gradient coating comprising n layers of gradient coating on the surface of a carbon-based material, wherein n>1, and the deposition method is such that the carbon content of each layer of the carbon / silicon carbide gradient coating is 2wt% to 40wt% along the direction from the surface of the carbon-based material to the silicon carbide coating, and decreases successively, and the difference in carbon content between the first layer of gradient coating combined on the surface of the carbon-based material and the nth layer of gradient coating combined on one side of the silicon carbide coating is not less than 3wt%; at the same time, along the direction from the surface of the carbon-based material to the silicon carbide coating, the average grain size of each layer of the carbon / silicon carbide gradient coating is smaller than that of the silicon carbide coating, and increases successively;

[0043] (2) Depositing a silicon carbide coating on the surface of the carbon / silicon carbide gradient coating to obtain a composite coating.

[0044] In some embodiments, the method further comprises pre-treating the carbon-based material before depositing the carbon-based material surface. Impurities on the surface of the carbon-based material are removed by pre-treatment. Preferably, the pre-treatment method is to pickle the carbon-based material. The pickling acid can be a conventional acid in the art, such as hydrofluoric acid, hydrochloric acid and sulfuric acid, and the concentration of the acid can be selected in a wide range, such as 40wt% to 60wt%, and the pickling time is 0.5h to 2h.

[0045] It should be understood that the pretreatment is also accompanied by operations such as rinsing, and the carbon-based material after the acid washing treatment can be used in the subsequent deposition process after drying. The drying method can be a conventional drying method, such as using a vacuum dryer or air blast drying (it can be dried at 100°C to 500°C for more than 2 hours).

[0046] The deposition method can be CVD deposition, and the deposition equipment used is a CVD vapor deposition furnace. The graphite substrate can be placed horizontally in the deposition reaction chamber, the furnace door is closed, the reaction chamber is evacuated to a vacuum below 200 Pa, and then the temperature is increased to the deposition temperature at 3°C / min to 6°C / min.

[0047] In some embodiments, in step (1), the deposition method is such that the carbon / silicon carbide gradient coating includes at least three gradient coating layers. That is, in step (1), the deposition method is such that the carbon / silicon carbide gradient coating includes n gradient coating layers, n>3 or n is 3.

[0048] In some embodiments, the deposition method of the first layer of gradient coating includes: introducing gas containing trichloromethylsilane (MTS), argon and hydrogen, the deposition temperature is 1020°C to 1150°C, for example, it can be 1020°C, 1040°C, 1060°C, 1080°C, 1100°C, 1120°C, 1140°C, 1150°C and any range between any two values, the deposition pressure is 15kPa to 25kPa, for example, it can be 15kPa, 16kPa, 18kPa, 20kPa, 22kPa, 24kPa, 25kPa and any range between any two values, The deposition time is 2h~5h, for example, it can be 2h, 3h, 4h, 5h and any range between any two values; the flow ratio of trichloromethylsilane and hydrogen is 1:(1.5~5), for example, it can be 1:1.5, 1:1.6, 1:1.8, 1:2, 1:2.5, 1:3, 1:3.5, 1:4, 1:4.5, 1:5 and any range between any two values; the flow ratio of hydrogen and argon is 1:(1~2), for example, it can be 1:1, 1:1.2, 1:1.4, 1:1.6, 1:1.8, 1:2 and any range between any two values.

[0049] In some embodiments, the deposition method of the nth layer of gradient coating includes: introducing gas containing trichloromethylsilane, argon and hydrogen, the deposition temperature is 1250°C to 1400°C, for example, it can be 1250°C, 1260°C, 1270°C, 1280°C, 1290°C, 1300°C, 1310°C, 1320°C, 133°C, 1340°C, 1350°C, 1360°C, 1370°C, 1380°C, 1390°C, 1400°C and any range between any two values, and the deposition pressure is 10kPa to 20kPa, for example, it can be 10kPa, 11kPa, 12kPa, 13kPa, 14kPa, 15kPa a, 16kPa, 17kPa, 18kPa, 19kPa, 20kPa and any range between any two values, the deposition time is 2h to 5h, such as 2h, 3h, 4h, 5h and any range between any two values; the flow ratio of trichloromethylsilane and hydrogen is 1:(4-9), such as 1:4, 1:5, 1:6, 1:7, 1:8, 1:9 and any range between any two values; the flow ratio of hydrogen and argon is 1:(1-2), such as 1:1, 1:1.2, 1:1.4, 1:1.6, 1:1.8, 1:2 and any range between any two values. The inventors of the present invention found during the experiment that if the temperature is too low during the nth layer of gradient coating, the coating cannot be formed.

[0050] In some embodiments, the deposition method of the 2nd to n-1st layers of gradient coating includes: the introduction gas contains trichloromethylsilane, argon and hydrogen, the deposition time is 2h to 5h, for example, it can be 2h, 3h, 4h, 5h and any range between any two values; the flow ratio of hydrogen and argon is 1:(1~2), for example, it can be 1:1, 1:1.2, 1:1.4, 1:1.6, 1:1.8, 1:2 and any range between any two values, and at least one condition of the deposition temperature, deposition pressure and the flow ratio of trichloromethylsilane and hydrogen varies within the range of deposition conditions for forming the 1st layer of gradient coating and the nth layer of gradient coating.

[0051] In some embodiments, in step (1), the deposition method is such that the carbon / silicon carbide gradient coating includes three layers of gradient coating, that is, n is 3. The deposition method of the second layer of gradient coating includes: introducing gas comprising trichloromethylsilane, argon and hydrogen, the deposition temperature is 1100°C to 1250°C, for example, it can be 1100°C, 1120°C, 1140°C, 1160°C, 1180°C, 1200°C, 1220°C, 1240°C, 1250°C and any range between any two values, and the deposition pressure is 10kPa to 20kPa, for example, it can be 10kPa, 11kPa, 12kPa, 13kPa, 14kPa, 15kPa, 16kPa, 17kPa, 18kPa, 19kPa, 20kPa and any range between any two values. The deposition time is 2h~5h, for example, 2h, 3h, 4h, 5h and any range between any two values; the flow ratio of trichloromethylsilane to hydrogen is 1:(3~7), for example, 1:3, 1:3.5, 1:4, 1:4.5, 1:5, 1:5.5, 1:6, 1:6.5, 1:7 and any range between any two values; the flow ratio of hydrogen to argon is 1:(1~2), for example, 1:1, 1:1.2, 1:1.4, 1:1.6, 1:1.8, 1:2 and any range between any two values.

[0052] If not otherwise specified, in the present invention, the temperature can be raised to the target temperature at 3-6°C / min, and can be lowered to the target temperature at 10-15°C / min.

[0053] In some embodiments, the deposition rate is between 3 μm / h and 15 μm / h.

[0054] In some embodiments, the deposition rate of the first gradient coating is 3 μm / h to 5 μm / h, for example, 3 μm / h, 3.5 μm / h, 4 μm / h, 4.5 μm / h, 5 μm / h, and any range between any two values; the deposition rate of the second gradient coating is 5 to 8 μm / h, for example, 5 μm / h, 6 μm / h, 7 μm / h, 8 μm / h, and any range between any two values; the deposition rate of the third gradient coating is 5 to 8 μm / h, for example, 5 μm / h, 6 μm / h, 7 μm / h, 8 μm / h, and any range between any two values; The deposition rate of the coating is 5 to 10 μm / h, for example, 5 μm / h, 6 μm / h, 7 μm / h, 8 μm / h, 9 μm / h, 10 μm / h and any range between any two values. The deposition rate of the silicon carbide coating is 10 to 15 μm / h, for example, 10 μm / h, 11 μm / h, 12 μm / h, 13 μm / h, 14 μm / h, 15 μm / h and any range between any two values.

[0055] In some embodiments, in step (1), the method further comprises: after each layer of gradient coating is deposited, stopping the introduction of trichloromethylsilane and hydrogen, and performing annealing treatment.

[0056] In some embodiments, the annealing conditions include: a temperature 50-150°C higher than the deposition temperature of the first gradient coating, such as 50°C, 60°C, 70°C, 80°C, 90°C, 100°C, 110°C, 120°C, 130°C, 140°C, 150°C, and any range between any two values, and a time of 1-2h, such as 1h, 1.2h, 1.4h, 1.6h, 1.8h, 2h, and any range between any two values. It should be understood that the annealing conditions for each gradient coating layer may be different.

[0057] In some embodiments, in step (2), the deposition method includes: introducing gas comprising trichloromethylsilane, argon and hydrogen, the deposition temperature is 1250°C to 1400°C, for example, it can be 1250°C, 1260°C, 1280°C, 1300°C, 1320°C, 1340°C, 1360°C, 1380°C, 1400°C and any range between any two values, and the deposition pressure is 10kPa to 30kPa, for example, it can be 10kPa, 12kPa, 14kPa, 16kPa, 18kPa, 20kPa, 20kPa, 22kPa, 24kPa, 26kPa, 28kPa kPa, 30kPa and any range between any two values, the deposition time is 2h~5h, for example, it can be 2h, 3h, 4h, 5h and any range between any two values; the flow ratio of trichloromethylsilane and hydrogen is 1:(8~20), for example, it can be 1:8, 1:10, 1:12, 1:14, 1:16, 1:18, 1:20 and any range between any two values; the flow ratio of hydrogen and argon is 1:(1~2), for example, it can be 1:1, 1:1.2, 1:1.4, 1:1.6, 1:1.8, 1:2 and any range between any two values.

[0058] After the deposition is completed, a vacuum cooling operation can be performed. The specific operation method can be a conventional operation method in the art. For example, after stopping the introduction of gas, the furnace can be evacuated to below 200Pa, and the temperature can be gradually reduced by 400℃-600℃ at a cooling rate of 6-10℃ / min, and then cooled to room temperature with the furnace, and then N2 is introduced to adjust the pressure to normal pressure, and then the furnace is opened to take out the product.

[0059] A third aspect of the present invention provides a composite coating on the surface of a carbon-based material prepared by the method described above.

[0060] The structure and properties of the composite coating can be found in the first aspect and will not be elaborated here.

[0061] A fourth aspect of the present invention provides a composite material, the composite material comprising a carbon-based material and a composite coating bonded to the surface of the carbon-based material;

[0062] Wherein, the composite coating is the composite coating on the surface of the carbon-based material as described above.

[0063] For the description of carbon-based materials, see the first aspect.

[0064] A fifth aspect of the present invention provides the use of the above-mentioned carbon-based material surface composite coating or the above-mentioned composite material in the semiconductor field.

[0065] The composite coating can be combined with the surface of the carbon-based material to obtain the composite material, and the composite material can be used as a supporting base in the MOCVD process, for example.

[0066] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0067] Unless otherwise specified, the materials and reagents used in the following examples can be obtained from commercial sources.

[0068] The present invention is described in detail below in conjunction with specific embodiments, which are used to understand but not to limit the present invention.

[0069] In the following examples, the carbon content was determined by D-sims, and the average grain size was determined by EBSD.

[0070] The graphite matrix is ​​8516 static pressed graphite purchased from SGL.

[0071] Example 1

[0072] This example is used to illustrate the preparation method of the carbon-based material surface composite coating and the composite material described in the present invention.

[0073] (1) Graphite substrate pretreatment

[0074] The graphite substrate was soaked in 20wt% hydrochloric acid for 2 hours, then rinsed with deionized water for 2 minutes, and ultrasonically soaked at 20Hz for 30 minutes. After being taken out, the sample surface was rinsed with deionized water for 2 minutes, and then dried in a vacuum dryer at 200°C for 1 hour.

[0075] (2) Deposition of carbon / silicon carbide gradient coating

[0076] The pretreated graphite substrate was placed horizontally in the deposition reaction chamber of the CVD vapor deposition furnace, the furnace door was closed, the reaction chamber was evacuated to below 200 Pa, the temperature was raised to 1050 ° C, and MTS, H2 and Ar were continuously introduced for 10 minutes, wherein, according to the flow meter, MTS: H2 was 1: 2, Ar: H2 was 1.5: 1, MTS steam flow was 25 L / min; the deposition pressure was 20 kPa; the deposition time was 3 hours, and the first layer of gradient coating with a carbon content of about 20wt%, an average grain size of about 80nm, and a thickness of about 7μm was obtained. Then, the introduction of MTS and H2 was stopped, and the temperature was raised to 1150 ° C and maintained for 60 minutes for annealing.

[0077] After annealing, the temperature was stabilized at 1150°C, and MTS and H2 (volume ratio of 1:4) were continued to be introduced, the volume ratio of hydrogen and Ar remained unchanged, the MTS steam flow rate was 25L / min, the deposition pressure was 15kPa, and the deposition time was 3h, and the second layer of gradient coating with a carbon content of about 15wt%, an average grain size of about 250nm, and a thickness of about 10μm was obtained. The temperature was raised to 1250°C and maintained for 60min for annealing.

[0078] Then the temperature was raised at a heating rate of 5°C / min and stabilized at 1300°C, and MTS and H2 (volume ratio of 1:6) were continuously introduced, the volume ratio of hydrogen and Ar remained unchanged, the MTS steam flow rate was 25L / min, the deposition pressure was 15kPa, and the deposition time was 3h, and the third layer of gradient coating with a carbon content of about 10wt%, an average grain size of about 400nm, and a thickness of about 15μm was obtained. The temperature was raised to 1400°C and maintained for 60min for annealing.

[0079] (3) Deposition of silicon carbide coating

[0080] The temperature was lowered to 1300°C and stabilized for 10 minutes. MTS, H2 and Ar (volume ratio of 1:10) were continued to be introduced. The volume ratio of hydrogen and Ar remained unchanged. The MTS steam flow rate was 25L / min. The temperature was maintained at 1300°C. The deposition pressure was 25kPa. The deposition time was 5 hours. A silicon carbide coating with an average grain size of about 1μm and a thickness of about 70μm was obtained, that is, a composite material containing a composite coating was obtained.

[0081] The electron microscope image of the obtained composite material is shown in Figure 1 As shown, 100 is a graphite substrate; 200 is a first gradient coating layer; 300 is a second gradient coating layer; 400 is a third gradient coating layer; and 500 is a silicon carbide coating.

[0082] Example 2

[0083] This example is used to illustrate the preparation method of the carbon-based material surface composite coating and the composite material described in the present invention.

[0084] (1) Graphite substrate pretreatment

[0085] The treatment was carried out according to the method described in Example 1.

[0086] (2) Deposition of carbon / silicon carbide gradient coating

[0087] The pretreated graphite substrate was placed horizontally in the deposition reaction chamber of the CVD vapor deposition furnace, the furnace door was closed, the reaction chamber was evacuated to a vacuum pressure below 200 Pa, and the temperature was increased to 1100° C. at a rate of 5° C. / min.

[0088] MTS, H2 and Ar were introduced, wherein, by flow meter, MTS:H2 was 1:2.5, Ar:H2 was 1.5:1, and the MTS steam flow rate was 30 L / min; the deposition pressure was 20 kPa; the deposition time was 3 h, and the first gradient coating with a carbon content of about 15 wt%, an average grain size of about 60 nm, and a thickness of about 9 μm was obtained. Then, the introduction of MTS and H2 was stopped, and the temperature was raised to 1200°C and maintained for 60 min for annealing.

[0089] After annealing, the temperature was stabilized at 1200°C, and MTS and H2 (volume ratio of 1:5) were continued to be introduced, the volume ratio of hydrogen and Ar remained unchanged, the deposition pressure was 15kPa, the deposition time was 3h, and the second gradient coating with a carbon content of about 10wt%, an average grain size of about 220nm, and a thickness of about 13μm was obtained. The temperature was raised to 1300°C and maintained for 60min for annealing.

[0090] Then the temperature was raised at a heating rate of 5°C / min and stabilized at 1350°C for 10 minutes, and MTS and H2 (volume ratio of 1:7) were continuously introduced, the volume ratio of hydrogen and Ar remained unchanged, the deposition pressure was 15kPa, the deposition time was 3h, and the third layer of gradient coating with a carbon content of about 5wt%, an average grain size of about 500nm, and a thickness of about 18μm was obtained. The temperature was raised to 1450°C and maintained for 60 minutes for annealing.

[0091] (3) Deposition of silicon carbide coating

[0092] The method described in Example 1 was followed to prepare a composite material containing a composite coating.

[0093] Example 3

[0094] This example is used to illustrate the preparation method of the carbon-based material surface composite coating and the composite material described in the present invention.

[0095] (1) Graphite substrate pretreatment

[0096] The treatment was carried out according to the method described in Example 1.

[0097] (2) Deposition of carbon / silicon carbide gradient coating

[0098] The pretreated graphite substrate was placed horizontally in the deposition reaction chamber of the CVD vapor deposition furnace, the furnace door was closed, the reaction chamber was evacuated to below 200 Pa, the temperature was raised to 1050 ° C at 5 ° C / min and kept for 10 minutes, MTS, H2 and Ar were introduced, wherein, according to the flow meter, MTS: H2 was 1: 4, Ar: H2 was 1.5: 1, MTS steam flow was 25L / min; deposition pressure was 20kPa; deposition time was 3h, and the first layer of gradient coating with a carbon content of about 18wt%, an average grain size of about 100nm, and a thickness of about 6μm was obtained. Then stop the introduction of MTS and H2, raise the temperature to 1150 ° C and keep it for 60 minutes for annealing.

[0099] After annealing, the temperature was stabilized at 1150°C, and MTS and H2 (volume ratio of 1:6) were continued to be introduced, the volume ratio of hydrogen and Ar remained unchanged, the deposition pressure was 15kPa, the deposition time was 3h, and the second gradient coating with a carbon content of about 12wt%, an average grain size of about 400nm, and a thickness of about 8μm was obtained. The temperature was raised to 1250°C and maintained for 60min for annealing.

[0100] Then the temperature was raised at a heating rate of 5°C / min and stabilized at 1300°C, and MTS and H2 (volume ratio of 1:8) were continuously introduced, the volume ratio of hydrogen and Ar remained unchanged, the deposition pressure was 15kPa, the deposition time was 3h, and the third gradient coating with a carbon content of about 7wt%, an average grain size of about 500nm, and a thickness of about 12μm was obtained. The temperature was raised to 1400°C and maintained for 60min for annealing.

[0101] (3) Deposition of silicon carbide coating

[0102] The method described in Example 1 was followed to prepare a composite material containing a composite coating.

[0103] Example 4

[0104] This group of examples is used to illustrate the effect of changing the carbon content of the gradient coating on the effect.

[0105] The operation was carried out in accordance with the method described in Example 1, except that the flow ratio of MTS and H2 was changed during the coating deposition process. Specifically, based on the flow meter, the MTS:H2 ratio was 1:1 during the deposition of the first gradient coating layer, and the first gradient coating layer had a carbon content of 35 wt%, an average grain size of 70 nm, and a thickness of 15 μm.

[0106] Finally, a composite material was prepared.

[0107] Example 5

[0108] This group of examples is used to illustrate the influence of the change of coating grain size on the effect.

[0109] The method described in Example 1 was followed, except that the deposition temperatures of the coatings were changed respectively, specifically:

[0110] Example 5a: The deposition temperature of the second gradient coating layer is 1100° C., and a second gradient coating layer having a carbon content of 15 wt %, an average grain size of 300 nm, and a thickness of 15 μm is obtained;

[0111] Example 5b: The deposition temperature of the third gradient coating layer is 1200° C., and the third gradient coating layer is obtained with a carbon content of 10 wt %, an average grain size of 600 nm and a thickness of 20 μm.

[0112] Finally, composite materials were obtained.

[0113] Comparative Example 1

[0114] This comparative example is used to illustrate the preparation method of the reference carbon-based material surface composite coating and the composite material.

[0115] (1) Graphite substrate pretreatment

[0116] The treatment was carried out according to the method described in Example 1.

[0117] (2) Deposition of carbon / silicon carbide coating

[0118] The pretreated graphite substrate was placed horizontally in the deposition reaction chamber of the CVD vapor deposition furnace, the furnace door was closed, the reaction chamber was evacuated to below 200 Pa, the temperature was raised to 1200 ° C at 5 ° C / min and kept for 10 minutes, MTS, H2 and Ar were introduced, wherein, according to the flow meter, MTS: H2 was 1: 0.5, Ar: H2 was 1.5: 1, and the MTS steam flow rate was 25L / min; the deposition pressure was 15kPa; the deposition time was 3h, and a gradient coating with a carbon content of 40wt%, an average grain size of 50nm, and a thickness of about 30μm was obtained. Then stop the introduction of MTS and H2, raise the temperature to 1300 ° C and keep it for 60min for annealing.

[0119] (3) Deposition of silicon carbide coating

[0120] The method described in Example 1 was followed to prepare a composite material containing a composite coating.

[0121] Comparative Example 2

[0122] This comparative example is used to illustrate the preparation method of the reference carbon-based material surface composite coating and the composite material.

[0123] The method described in Example 1 is followed, except that the carbon / silicon carbide gradient coating is not deposited, but the silicon carbide coating is deposited directly on the graphite substrate, and the deposition time is controlled during the deposition of the silicon carbide coating to prepare a silicon carbide coating with a thickness of about 100 μm, that is, a composite material containing a composite coating is obtained.

[0124] Comparative Example 3

[0125] This comparative example is used to illustrate the preparation method of the reference carbon-based material surface composite coating and the composite material.

[0126] The method described in Example 1 was followed, except that the flow ratios of MTS and H2 during the coating deposition process were changed, specifically:

[0127] Comparative Example 3a: According to the flow meter, during the deposition of the second gradient coating, MTS:H2 is 1:2, and a second gradient coating having a carbon content of about 25wt%, an average grain size of about 230nm, and a thickness of about 20μm is obtained. At this time, the content of the second gradient coating (about 25wt%) is greater than the contents of the first and third gradient coatings (about 20wt% and about 10wt%, respectively);

[0128] Comparative Example 3b: According to the flow meter, the MTS:H2 ratio during the deposition of the third gradient coating was 1:3, and the third gradient coating had a carbon content of about 18wt%, an average grain size of 350nm, and a thickness of 20μm. At this time, the content of the second gradient coating (about 15wt%) was less than the contents of the first and third gradient coatings (about 20wt% and about 18wt%).

[0129] Finally, composite materials were obtained.

[0130] Comparative Example 4

[0131] This comparative example is used to illustrate the preparation method of the reference carbon-based material surface composite coating and the composite material.

[0132] The operation was carried out according to the method described in Example 1, except that the deposition temperature of the coating was changed. Specifically, the deposition temperature of the first gradient coating was about 1000°C, and a first gradient coating with a carbon content of about 20wt%, an average grain size of about 100nm, and a thickness of about 6μm was obtained (the color of the crystals in this layer was light yellow, and the grains were loose and disordered). At this time, the average grain size of the second gradient coating (about 250nm) was smaller than the average grain size of the third gradient coating (about 400nm). The surface of the prepared composite material was uneven and loose and porous under an electron microscope.

[0133] Test Example 1

[0134] The composite materials prepared in the examples and comparative examples were heated to 600°C and kept warm for 30 minutes, then the samples were directly put into 25°C water and cooled to room temperature. The cycle was repeated several times until the coating on the samples fell off. The number of cycles when the samples were damaged was recorded. The results are shown in Table 1.

[0135] Table 1

[0136] serial number Cycle times / times Example 1 45 Example 2 46 Example 3 41 Example 4 34 Example 5a 38 Example 5b 30 Comparative Example 1 20 Comparative Example 2 15 Comparative Example 3a 26 Comparative Example 3b 28 Comparative Example 4 27

[0137] It should be noted that, in this article, the terms "comprise", "include" or any other variant thereof are intended to cover non-exclusive inclusion, so that the process, method, article or device including a series of elements includes not only those elements, but also includes other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "comprise one..." do not exclude the presence of other identical elements in the process, method, article or device including the element. In addition, it should be pointed out that the scope of the methods and devices in the embodiments of the present application is not limited to performing functions in the order shown or discussed, and may also include performing functions in a substantially simultaneous manner or in reverse order according to the functions involved, for example, the described method may be performed in an order different from that described, and various steps may also be added, omitted, or combined. In addition, the features described with reference to certain examples may be combined in other examples.

[0138] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A composite coating on the surface of a carbon-based material, characterized in that: The composite coating includes a carbon / silicon carbide gradient coating bonded to a surface of a carbon-based material and a silicon carbide coating bonded to the other side of the carbon / silicon carbide gradient coating; The carbon / silicon carbide gradient coating comprises n layers of gradient coating; Along the direction from the surface of the carbon-based material to the silicon carbide coating, the carbon content in each layer of the carbon / silicon carbide gradient coating is 2wt% to 25wt% and decreases successively, and the difference in carbon content between the first layer of the gradient coating combined on the surface of the carbon-based material and the nth layer of the gradient coating combined on one side of the silicon carbide coating is not less than 3wt%; Along the direction from the surface of the carbon-based material to the silicon carbide coating, the average grain size of each layer of the carbon / silicon carbide gradient coating is smaller than that of the silicon carbide coating and increases successively; The thickness of each layer of carbon / silicon carbide gradient coating is 5 μm to 25 μm; The average grain size of the silicon carbide coating is 500nm to 1500nm; When n>3, the carbon content in the first gradient coating is 12wt% to 25wt%, and the carbon content in the nth gradient coating is 2wt% to 12wt%; the average grain size of the first gradient coating is 50nm to 150nm, and the average grain size of the nth gradient coating is 300nm to 700nm; When n is 3, the carbon content in the first layer of gradient coating is 12wt%~25wt%, the carbon content in the second layer of gradient coating is 10wt%~15wt%, and the carbon content in the third layer of gradient coating is 2wt%~10wt%; the average grain size of the first layer of gradient coating is 50nm~150nm, the average grain size of the second layer of gradient coating is 100nm~500nm, and the average grain size of the third layer of gradient coating is 300nm~700nm.

2. The carbon-based material surface composite coating according to claim 1, characterized in that: The thickness of the composite coating is 80 μm to 150 μm; and / or In the composite coating, the thickness of the carbon / silicon carbide gradient coating is 20% to 45% of the total thickness.

3. The carbon-based material surface composite coating according to claim 1 or 2, characterized in that: The carbon content difference between each layer is 4wt% to 8wt%.

4. A method for preparing a composite coating on the surface of a carbon-based material, characterized in that: The method includes: (1) depositing a carbon / silicon carbide gradient coating comprising n layers of gradient coating on the surface of a carbon-based material, wherein n>1, and the deposition method is such that the carbon content of each layer of the carbon / silicon carbide gradient coating is 2 to 40 wt% along the direction from the surface of the carbon-based material to the silicon carbide coating, and decreases successively, and the difference in carbon content between the first layer of gradient coating combined on the surface of the carbon-based material and the nth layer of gradient coating combined on one side of the silicon carbide coating is not less than 3 wt%; at the same time, along the direction from the surface of the carbon-based material to the silicon carbide coating, the average grain size of each layer of the carbon / silicon carbide gradient coating is smaller than that of the silicon carbide coating, and increases successively; (2) depositing a silicon carbide coating on the surface of the carbon / silicon carbide gradient coating to obtain a composite coating; In step (1), the deposition method is such that the carbon / silicon carbide gradient coating comprises n layers of gradient coating, n>3; the deposition method of the first layer of gradient coating comprises: the inlet gas comprises trichloromethylsilane, argon and hydrogen, the deposition temperature is 1020°C to 1150°C, the deposition pressure is 15kPa to 25kPa, and the deposition time is 2h to 5h; the flow ratio of trichloromethylsilane to hydrogen is 1:(1.5 to 5); the flow ratio of hydrogen to argon is 1:(1 to 2); the deposition method of the nth layer of gradient coating comprises: the inlet gas comprises trichloromethylsilane, argon and hydrogen, the deposition temperature is 1250 ~1400℃, deposition pressure of 10kPa~20kPa, deposition time of 2h~5h; flow ratio of trichloromethylsilane to hydrogen is 1:(4~9); flow ratio of hydrogen to argon is 1:(1~2); deposition method of the second to n-1 layers of gradient coating includes: introducing gas containing trichloromethylsilane, argon and hydrogen, deposition time of 2h~5h; flow ratio of hydrogen to argon is 1:(1~2), at least one condition of deposition temperature, deposition pressure and flow ratio of trichloromethylsilane to hydrogen is changed within the deposition condition formation range of the first layer of gradient coating and the nth layer of gradient coating; or In step (1), the deposition method makes the carbon / silicon carbide gradient coating contain n layers of gradient coating, n is 3; the deposition method of the second layer of gradient coating includes: the inlet gas contains trichloromethylsilane, argon and hydrogen, the deposition temperature is 1100~1250℃, the deposition pressure is 10kPa~20kPa, and the deposition time is 2h~5h; the flow ratio of trichloromethylsilane and hydrogen is 1:(3~7); the flow ratio of hydrogen and argon is 1:(1~2).

5. The preparation method according to claim 4, characterized in that: In step (1), the method further comprises: after each layer of gradient coating is deposited, stopping the introduction of trichloromethylsilane and hydrogen, and performing annealing treatment; The temperature of the annealing treatment is 50-150° C. higher than the deposition temperature of the corresponding gradient coating, and the time is 1-2 hours.

6. The preparation method according to claim 4 or 5, characterized in that: In step (2), the deposition method of the silicon carbide coating includes: the inlet gas contains trichloromethylsilane, argon and hydrogen, the deposition temperature is 1250-1400°C, the deposition pressure is 10kPa-30kPa, and the deposition time is 2h-5h; the flow ratio of trichloromethylsilane to hydrogen is 1:(8-20); the flow ratio of hydrogen to argon is 1:(1-2).

7. A composite coating on the surface of a carbon-based material prepared by the method according to any one of claims 4 to 6.

8. A composite material, characterized in that The composite material comprises a carbon-based material and a composite coating bonded to the surface of the carbon-based material; Wherein, the composite coating is a composite coating on the surface of a carbon-based material as described in any one of claims 1-3 and 7.

9. Use of the carbon-based material surface composite coating according to any one of claims 1 to 3 and 7 or the composite material according to claim 8 in the semiconductor field.