A double-layer protective layer for lithium anodes, its preparation method and application
By preparing a double-layer protective layer for lithium anodes using electrospinning technology, the problem of dendrite growth in lithium metal anodes was solved, resulting in long cycle life and stability of lithium batteries.
Patent Information
- Application Number
- CN202410353094.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-26
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2044-03-26
AI Technical Summary
Safety issues and side reactions caused by dendrite growth in lithium metal anodes during charging and discharging affect battery stability and cycle life.
A double-layer protective layer for lithium anodes, consisting of PVDF-HA and a PVDF-HA/gelatin layer, was prepared using electrospinning technology to form a fiber network structure, thereby regulating the uniform deposition and growth of lithium.
It effectively suppresses lithium dendrite growth, improves the cycle stability and interface stability of lithium metal anodes, and extends battery life.
Smart Images

Figure CN118315541B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of lithium metal secondary electrode materials, and particularly relates to a lithium anode double-layer protective layer, its preparation method and application. Background Technology
[0002] The development of high-energy-density secondary battery systems with a specific energy greater than 500Wh / kg is an important measure to further promote implementation.
[0003] Lithium metal is known for its high theoretical specific capacity (3680 mAh g). -1 Low density (0.534g cm³) -3 With its low voltage and the lowest electrode potential (-3.04V vs standard hydrogen electrode), lithium batteries using metallic lithium as the negative electrode material are a promising next-generation energy storage system.
[0004] However, during the charge-discharge cycle of a battery, the continuous stripping and deposition of lithium can cause dendrite growth, leading to short circuits and thermal runaway, thus causing safety issues. Furthermore, side reactions between lithium metal and the electrolyte, and the formation of dead lithium, can also cause problems such as low battery coulombic efficiency, volume expansion, and structural damage.
[0005] The aforementioned problems severely restrict the commercialization of lithium metal anodes. Therefore, it is crucial to develop a highly stable lithium metal anode system with long cycle life that can mitigate dendrite growth, suppress side reactions, and alleviate dendrite growth.
[0006] Currently, the main methods used to improve the stability of lithium metal anodes are: (1) introducing an artificial protective layer; (2) optimizing the composition of the electrolyte; and (3) designing novel lithium anode structures.
[0007] Among them, modifying the surface of lithium metal with an artificial protective layer can leverage the advantages of the structure and functional components of the artificial protective layer to enable lithium to be uniformly deposited on the negative electrode surface and suppress the occurrence of side reactions, thereby improving the cycle life of the lithium negative electrode. Summary of the Invention
[0008] The technical problem solved by this invention: This invention aims to provide a method for preparing a lithium anode protective layer, which obtains a double-layer protective layer with a fiber network structure through electrospinning technology, and can effectively improve the cycle life of the lithium anode.
[0009] In view of the technical problems existing in the prior art, the present invention designs a lithium anode double-layer protective layer, its preparation method and application.
[0010] To solve the aforementioned technical problems, the present invention adopts the following solution:
[0011] A method for preparing a double-layer protective layer for a lithium anode, characterized by comprising the following steps:
[0012] Step 1: Preparation of the first protective layer PVDF-HA layer of the lithium anode;
[0013] Step 2: Preparation of the second protective layer PVDF-HA / gelatin layer of the lithium anode, thus obtaining the double protective layer of the lithium anode;
[0014] The total thickness of the lithium anode double-layer protective layer is 200μm-500μm.
[0015] Furthermore, step 1: the preparation of the first protective layer PVDF-HA layer of the lithium anode specifically involves:
[0016] 1.1 Prepare a 5%-8% (w / w) polyvinylidene fluoride (PVDF) solution using the first solvent and set it aside for later use;
[0017] 1.2 Add nano-hydroxyapatite (HA) to the prepared polyvinylidene fluoride (PVDF) solution according to the mass ratio of polyvinylidene fluoride (PVDF) to nano-hydroxyapatite (HA) of 2:1-5:1, and stir thoroughly to obtain a polyvinylidene fluoride solution with nano-hydroxyapatite uniformly dispersed.
[0018] 1.3 Take 2ml-5ml of the prepared polyvinylidene fluoride solution with uniformly dispersed nano-hydroxyapatite using a syringe. Under room temperature conditions, use electrospinning technology to spin the polyvinylidene fluoride solution with uniformly dispersed nano-hydroxyapatite onto one side of the aluminum foil to obtain the first protective layer of lithium anode, PVDF-HA layer.
[0019] 1.4 After electrospinning, the first protective layer PVDF-HA of the lithium anode is dried at 50-70℃ for 20-30h to obtain the dried first protective layer PVDF-HA of the lithium anode, which is ready for use.
[0020] Further, step 2: the preparation of the second protective layer PVDF-HA / gelatin layer of the lithium anode specifically involves:
[0021] 2.1 Prepare a gelatin solution with a mass fraction of 6%-15% using a second solvent at a preparation temperature of 50-70℃, and set aside for later use;
[0022] 2.2 Take 2ml-5ml of the prepared gelatin solution with a syringe while it is still hot, and spin the gelatin solution onto the surface of the dried lithium anode first protective layer PVDF-HA layer prepared in step 1 using electrospinning technology at 50-70℃.
[0023] 2.3 After electrospinning, continue drying at 50-70℃ for 20-30h to obtain the lithium anode double protective layer PVDF-HA / gelatin layer adhered to the aluminum foil;
[0024] 2.4 Remove the prepared PVDF-HA / gelatin layer, which is adhered to the aluminum foil, from the aluminum foil to obtain a double protective layer for the lithium anode.
[0025] Further, the first solvent mentioned in step 1.1 is N-methylpyrrolidone (NMP) or dimethylformamide (DMF);
[0026] The thorough mixing mentioned in step 1.2 refers to magnetic stirring for 10-15 hours.
[0027] Furthermore, the parameters in the electrospinning technology described in step 1.3 are set as follows:
[0028] Spinning voltage: 12kV; needle specification: 20G; distance from needle to receiver: 20cm; receiver rotation speed: 120r / min; solution temperature during PVDF spinning: room temperature; syringe injection speed: 3mL / h.
[0029] Furthermore, the second solvent mentioned in step 2.1 is deionized water or trifluoroethanol.
[0030] Further, the electrospinning parameters described in step 2.2 are set as follows:
[0031] Spinning voltage: 12kV; needle specification: 20G; distance from needle to receiver: 20cm; receiver rotation speed: 120r / min; solution temperature during gelatin spinning: 50-70℃; syringe injection speed: 3mL / h.
[0032] This invention also protects a lithium anode double-layer protective layer.
[0033] This invention also protects the application of a lithium anode double-layer protective layer in the field of lithium battery materials.
[0034] In this invention, a double-layer protective layer for lithium anodes is prepared by electrospinning technology to form a double-layer film with a fiber network structure, which is used as a protective layer for lithium metal anodes.
[0035] In this invention, the fiber network structure formed by electrospinning can regulate the uniform migration and deposition of metallic lithium. In particular, the abundant N and O heteroatoms in gelatin and the large number of hydroxyl groups (-OH) in nano-HA are all polar lithiumophilic groups, providing numerous active sites for lithium nucleation. This guides uniform deposition of metallic lithium, alleviates lithium dendrite growth, and extends cycle life. Furthermore, the rigidity of nano-HA can also inhibit lithium dendrite growth to a certain extent through physical action.
[0036] In this invention, the method overcomes the problems of gelatin and PVDF being difficult to mix and use and HA being unable to be electrospun into a film. It integrates gelatin, PVDF and HA into an organic-inorganic composite film with a double-layer structure and uses it for the protection of lithium anodes.
[0037] It should be noted that, in this invention, unless otherwise specified, the specific meaning of "comprising" in relation to composition definition and description includes both open-ended meanings such as "comprising," "including," etc., and closed-ended meanings such as "composed of," etc., and similar meanings.
[0038] This invention provides a lithium anode double-layer protective layer, its preparation method, and its application, which have the following beneficial effects:
[0039] (1) The lithium anode double-layer protective layer of this invention is prepared by electrospinning to create a double-layer film with a fiber network structure, which is used as a protective layer for the lithium metal anode. A lithium-lithium symmetric battery assembled using this double-layer protective lithium metal anode achieves a 1 mA cm⁻¹ performance. -2 Current density, 1mAh cm -2 At the given areal capacity, it can cycle stably for 500 hours and has a small polarization voltage, indicating that the double protective layer can effectively improve the cycle stability of the lithium metal anode.
[0040] (2) The preparation method of this invention is simple, fast, low-cost, and easy to control. By electrospinning twice, the problems of gelatin and PVDF being difficult to mix and HA being unable to be electrospinned into a film are overcome. Gelatin, PVDF and HA are integrated into an organic-inorganic composite film with a double-layer structure, which is used for the protection of lithium anodes. This provides theoretical guidance for the mechanism of action of achieving long life of lithium metal anodes and inhibiting the growth of lithium dendrites.
[0041] (3) The double protective layer of the present invention can effectively improve the interface stability of the lithium metal anode, and the assembled lithium-lithium symmetric battery has a long cycle life.
[0042] This demonstrates that the lithium anode double-layer protective layer designed using this invention has broad application prospects in the field of lithium metal secondary batteries. Attached Figure Description
[0043] Figure 1 This is a schematic diagram of the cycle performance of a lithium-lithium symmetric battery made using a lithium anode with a double protective layer in Embodiment 1 of the present invention. Detailed Implementation
[0044] The present invention will be further described below with reference to specific embodiments and accompanying drawings:
[0045] Example 1
[0046] Step 1: Preparation of the double-layer protective layer for lithium anode
[0047] Step 1: Preparation of the first protective layer PVDF-HA layer of the lithium anode
[0048] 1.1 Prepare a 6% (w / w) polyvinylidene fluoride (PVDF) solution using N-methylpyrrolidone (NMP) as the solvent.
[0049] 1.2 Add nano-hydroxyapatite to the prepared PVDF solution at a mass ratio of 2:1 for polyvinylidene fluoride (PVDF) to nano-hydroxyapatite (HA), and stir magnetically for 12 hours to ensure thorough mixing and obtain a polyvinylidene fluoride solution with uniformly dispersed nano-hydroxyapatite.
[0050] 1.3 Take 3 mL of the prepared polyvinylidene fluoride solution with uniformly dispersed nano-hydroxyapatite using a syringe. Under room temperature conditions, use electrospinning technology to spin the polyvinylidene fluoride solution with uniformly dispersed nano-hydroxyapatite onto one side of the aluminum foil to obtain the first protective layer PVDF-HA layer of the lithium anode.
[0051] 1.4 After electrospinning, the first protective layer PVDF-HA of the lithium anode is dried at 60℃ for 24h to obtain the dried first protective layer PVDF-HA of the lithium anode, which is ready for use.
[0052] Step 2: Preparation of the second protective layer PVDF-HA / gelatin layer for the lithium anode
[0053] 2.1 Prepare an 8% gelatin solution using trifluoroethanol as a solvent at a preparation temperature of 60℃, and set aside for later use;
[0054] 2.2 Take 3 mL of the prepared gelatin solution while it is still hot using a syringe, and spin the gelatin solution onto the surface of the first protective layer PVDF-HA layer of the lithium anode prepared in step 1 using electrospinning technology at 60℃.
[0055] 2.3 After electrospinning, the material was dried at 60°C for 24 hours to obtain a lithium anode double protective layer PVDF-HA / gelatin layer adhered to the aluminum foil.
[0056] 2.4 Remove the prepared PVDF-HA / gelatin layer, which is attached to the aluminum foil, from the aluminum foil to obtain a double protective layer for the lithium anode, which is a PVDF-HA / gelatin layer.
[0057] The parameters for the electrospinning technology in steps 1.3 and 2.2 are set as follows:
[0058] Spinning voltage: 12kV; Needle specifications: 20G (i.e., inner diameter 0.61mm, outer diameter 0.91mm); distance from needle to receiver: 20cm; receiver rotation speed: 120r / min;
[0059] The solution temperature for gelatin spinning is 60℃, and the solution temperature for PVDF spinning is room temperature, i.e., 25℃; the syringe injection rate is 3mL / h.
[0060] Step 2: Assembly and Cycle Performance Testing of Lithium-Lithium Symmetric Batteries
[0061] The obtained lithium anode double protective layer PVDF-HA / gelatin layer is cut into a circular piece with a diameter of 19mm.
[0062] Then, a layer containing PVDF and HA is placed facing the lithium metal, and a layer containing gelatin is placed facing the separator.
[0063] A lithium-lithium symmetric battery was assembled using a Celgard 2025 separator, 60 μL of electrolyte (DOL; DME = 1:1 vol%, 1 M LiTFSI, 0.4 M LiNO3), and a lithium metal sheet (15.6 mm in diameter and 0.2 mm in thickness). Its cycle performance was tested after standing for 12 hours.
[0064] Electrochemical performance was tested using a charge-discharge tester. The test was conducted at a current density of 1 mA cm⁻¹. -2 The surface capacity is 1mAh cm -2 Cyclic performance tests were conducted under the specified conditions, and the results are as follows: Figure 1 As shown.
[0065] from Figure 1 As can be seen from the data, the lithium-lithium symmetric battery assembled with a lithium metal anode using a double-layer protective layer performs well at 1 mA / cm². -2 Current density, 1mAh cm -2 At its surface capacity, it can cycle stably for 500 hours and has a small polarization voltage.
[0066] Comparative Example 1
[0067] In Comparative Example 1, the negative electrode of the battery is a common lithium negative electrode without a protective layer, and the other battery assembly and testing methods are the same as in Example 1.
[0068] Example 2
[0069] Step 1: Preparation of the double-layer protective layer for lithium anode
[0070] Step 1: Preparation of the first protective layer PVDF-HA layer of the lithium anode
[0071] 1.1 Prepare an 8% (w / w) polyvinylidene fluoride (PVDF) solution using N-methylpyrrolidone (NMP) as the solvent.
[0072] 1.2 Add nano-hydroxyapatite to the prepared PVDF solution at a mass ratio of 5:1 (PVDF to nano-hydroxyapatite). Stir magnetically for 15 hours to ensure thorough mixing and obtain a PVDF solution with uniformly dispersed nano-hydroxyapatite.
[0073] 1.3 Take 5 mL of the prepared polyvinylidene fluoride solution with uniformly dispersed nano-hydroxyapatite using a syringe. Under room temperature conditions, use electrospinning technology to spin the polyvinylidene fluoride solution with uniformly dispersed nano-hydroxyapatite onto one side of the aluminum foil to obtain the first protective layer PVDF-HA layer of the lithium anode.
[0074] 1.4 After electrospinning, the first protective layer PVDF-HA of the lithium anode is dried at 70℃ for 20h to obtain the dried first protective layer PVDF-HA of the lithium anode, which is ready for use.
[0075] Step 2: Preparation of the second protective layer PVDF-HA / gelatin layer for the lithium anode
[0076] 2.1 Prepare a 6% gelatin solution using trifluoroethanol as solvent at a preparation temperature of 50℃, and set aside for later use;
[0077] 2.2 Take 2 mL of the prepared gelatin solution while it is still hot using a syringe, and spin the gelatin solution onto the surface of the first protective layer PVDF-HA layer of the lithium anode prepared in step 1 using electrospinning technology at 50°C.
[0078] 2.3 After electrospinning, the material was dried at 50°C for 30 hours to obtain a lithium anode double protective layer PVDF-HA / gelatin layer adhered to the aluminum foil.
[0079] 2.4 Remove the prepared PVDF-HA / gelatin layer, which is attached to the aluminum foil, from the aluminum foil to obtain a double protective layer for the lithium anode, which is a PVDF-HA / gelatin layer.
[0080] The parameters for the electrospinning technology in steps 1.3 and 2.2 are set as follows:
[0081] Spinning voltage: 12kV; Needle specifications: 20G (i.e., inner diameter 0.61mm, outer diameter 0.91mm); distance from needle to receiver: 20cm; receiver rotation speed: 120r / min;
[0082] The solution temperature for gelatin spinning is 50℃, and the solution temperature for PVDF spinning is room temperature, i.e., 25℃; the syringe injection rate is 3mL / h.
[0083] Step 2: Assembly and Cycle Performance Testing of Lithium-Lithium Symmetric Batteries
[0084] The obtained lithium anode double protective layer PVDF-HA / gelatin layer is cut into a circular piece with a diameter of 19mm.
[0085] Then, a layer containing PVDF and HA is placed facing the lithium metal, and a layer containing gelatin is placed facing the separator.
[0086] A lithium-lithium symmetric battery was assembled using a Celgard 2025 separator, 60 μL of electrolyte (DOL; DME = 1:1 vol%, 1 M LiTFSI, 0.4 M LiNO3), and a lithium metal sheet (15.6 mm in diameter and 0.2 mm in thickness). Its cycle performance was tested after standing for 12 hours.
[0087] The results show that the symmetrical cell operates at 1 mA cm⁻¹ -2 Current density, 1mAh cm -2 At its surface capacity, it can cycle stably for 500 hours.
[0088] Example 3
[0089] Step 1: Preparation of the double-layer protective layer for lithium anode
[0090] Step 1: Preparation of the first protective layer PVDF-HA layer of the lithium anode
[0091] 1.1 Prepare a 5% (w / w) polyvinylidene fluoride (PVDF) solution using dimethylformamide (DMF) as the solvent;
[0092] 1.2 Add nano-hydroxyapatite to the prepared PVDF solution at a mass ratio of 3:1 for polyvinylidene fluoride (PVD) to nano-hydroxyapatite (HA), stir magnetically for 10 hours, and stir thoroughly to obtain a polyvinylidene fluoride solution with nano-hydroxyapatite uniformly dispersed.
[0093] 1.3 Take 3 mL of the prepared polyvinylidene fluoride solution with uniformly dispersed nano-hydroxyapatite using a syringe. Under room temperature conditions, use electrospinning technology to spin the polyvinylidene fluoride solution with uniformly dispersed nano-hydroxyapatite onto one side of the aluminum foil to obtain the first protective layer PVDF-HA layer of the lithium anode.
[0094] 1.4 After electrospinning, the first protective layer PVDF-HA of the lithium anode is dried at 50°C for 30 hours to obtain the dried first protective layer PVDF-HA of the lithium anode, which is ready for use.
[0095] Step 2: Preparation of the second protective layer PVDF-HA / gelatin layer for the lithium anode
[0096] 2.1 Prepare a 15% gelatin solution using deionized water as solvent at a preparation temperature of 70℃, and set aside for later use;
[0097] 2.2 Take 2 mL of the prepared gelatin solution while it is still hot using a syringe, and spin the gelatin solution onto the surface of the first protective layer PVDF-HA layer of the lithium anode prepared in step 1 using electrospinning technology at 70℃.
[0098] 2.3 After electrospinning, the material was dried at 70°C for 20 hours to obtain a lithium anode double protective layer PVDF-HA / gelatin layer adhered to the aluminum foil.
[0099] 2.4 Remove the prepared PVDF-HA / gelatin layer, which is attached to the aluminum foil, from the aluminum foil to obtain a double protective layer for the lithium anode, which is a PVDF-HA / gelatin layer.
[0100] The parameters for the electrospinning technology in steps 1.3 and 2.2 are set as follows:
[0101] Spinning voltage: 12kV; Needle specifications: 20G (i.e., inner diameter 0.61mm, outer diameter 0.91mm); distance from needle to receiver: 20cm; receiver rotation speed: 120r / min;
[0102] The solution temperature for gelatin spinning is 70℃, and the solution temperature for PVDF spinning is room temperature, i.e., 25℃; the syringe injection rate is 3mL / h.
[0103] Step 2: Assembly and Cycle Performance Testing of Lithium-Lithium Symmetric Batteries
[0104] The resulting lithium anode double-layer protective layer is cut into a circular piece with a diameter of 19mm.
[0105] Then, a layer containing PVDF and HA is placed facing the lithium metal, and a layer containing gelatin is placed facing the separator.
[0106] A lithium-lithium symmetric battery was assembled using a Celgard 2025 separator, 60 μL of electrolyte (DOL; DME = 1:1 vol%, 1 M LiTFSI, 0.4 M LiNO3), and a lithium metal sheet (15.6 mm in diameter and 0.2 mm in thickness). Its cycle performance was tested after standing for 12 hours.
[0107] The results show that the symmetrical cell operates at 1 mA cm⁻¹ -2 Current density, 1mAh cm -2 At its surface capacity, it can cycle stably for 500 hours.
[0108] The preparation method of this invention is simple, rapid, low-cost, and easy to control. By performing two electrospinning processes, it overcomes the problems of gelatin and PVDF being difficult to mix and HA being unable to be electrospinned into a film. It integrates gelatin, PVDF, and HA into an organic-inorganic composite film with a double-layer structure, which is used to protect the lithium anode. This can extend the lifespan of the lithium metal anode and simultaneously inhibit the growth of lithium dendrites.
[0109] The present invention has been described above by way of example with reference to the embodiments and accompanying drawings. Obviously, the implementation of the present invention is not limited to the above-described manner. Any improvements made by adopting the inventive concept and technical solution of the present invention, or the direct application of the inventive concept and technical solution of the present invention to other occasions without modification, are all within the protection scope of the present invention.
Claims
1. A method for preparing a lithium-lithium symmetric battery including a lithium anode double-layer protective layer, characterized in that, Includes the following steps: Step 1: Preparation of the first protective layer PVDF-HA layer of the lithium anode, specifically as follows: 1.1 Prepare a 5%-8% (w / w) polyvinylidene fluoride (PVDF) solution using the first solvent and set it aside for later use; 1.2 Add nano-hydroxyapatite HA to the prepared polyvinylidene fluoride PVDF solution according to the mass ratio of polyvinylidene fluoride PVDF to nano-hydroxyapatite HA of 2:1-5:1, and stir thoroughly to obtain a polyvinylidene fluoride solution with nano-hydroxyapatite uniformly dispersed. 1.3 Take 2ml-5ml of the prepared polyvinylidene fluoride solution with uniformly dispersed nano-hydroxyapatite using a syringe. Under room temperature conditions, use electrospinning to spin the polyvinylidene fluoride solution with uniformly dispersed nano-hydroxyapatite onto one side of the aluminum foil to obtain the first protective layer PVDF-HA layer of the lithium anode. 1.4 After electrospinning, the first protective layer PVDF-HA of the lithium anode is dried at 50-70℃ for 20-30h to obtain the dried first protective layer PVDF-HA of the lithium anode, which is ready for use. Step 2: Preparation of the second protective layer of the lithium anode, specifically: 2.1 Prepare a gelatin solution with a mass fraction of 6%-15% using a second solvent at a preparation temperature of 50-70℃, and set aside for later use; 2.2 Take 2ml-5ml of the prepared gelatin solution with a syringe while it is still hot, and spin the gelatin solution onto the surface of the dried lithium anode first protective layer PVDF-HA layer prepared in step 1 using an electrospinning method at 50-70℃. 2.3 After electrospinning, continue drying at 50-70℃ for 20-30h to obtain a double-layer protective layer of lithium anode adhering to aluminum foil; 2.4 Remove the prepared second protective layer of lithium anode that is adhered to the aluminum foil from the aluminum foil to obtain a double protective layer of lithium anode; The obtained lithium anode double protective layer is cut into a disc, with the layer containing PVDF-HA facing the lithium metal and the layer containing gelatin facing the separator, and then a lithium-lithium symmetric battery is assembled. The first solvent mentioned in step 1.1 is N-methylpyrrolidone or dimethylformamide; The thorough mixing mentioned in step 1.2 refers to magnetic stirring for 10-15 hours; The total thickness of the lithium anode double protective layer is 200μm-500μm.
2. The method for preparing a lithium-lithium symmetric battery including a lithium anode double-layer protective layer according to claim 1, characterized in that, The parameters in the electrospinning method described in step 1.3 are set as follows: Spinning voltage: 12kV; needle specification: 20G; distance from needle to receiver: 20cm; receiver rotation speed: 120r / min; solution temperature during PVDF spinning: room temperature; syringe injection speed: 3mL / h.
3. The method for preparing a lithium-lithium symmetric battery including a lithium anode double-layer protective layer according to claim 1, characterized in that: The second solvent mentioned in step 2.1 is deionized water or trifluoroethanol.
4. The method for preparing a lithium-lithium symmetric battery including a lithium anode double-layer protective layer according to claim 1, characterized in that, The electrospinning parameters described in step 2.2 are set as follows: Spinning voltage: 12kV; needle specification: 20G; distance from needle to receiver: 20cm; receiver rotation speed: 120r / min; solution temperature during gelatin spinning: 50-70℃; syringe injection speed: 3mL / h.
5. A lithium-lithium symmetric battery comprising a lithium anode double-layer protective layer, prepared by the preparation method according to any one of claims 1-4.
Citation Information
Patent Citations
Battery and electronic equipment
CN218783212U