The composite electrode material La0.8Sr1.2FeO4+δ-xLa0.4Sr0.6FeO3-δ is synthesized through a one-pot method, which solves the problem of difficulty in balancing catalytic activity and stability of Ruddlesden-Popper type perovskite materials and achieves high stability. SOFC cathode materials with high resistance and high catalytic activity improve electrochemical and thermal cycle performance.
Patent Information
- Application Number
- CN202410463151.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-17
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2044-04-17
AI Technical Summary
It is difficult to combine high catalytic activity and high stability in Ruddlesden-Popper type perovskite-like materials with existing technology, and composite modification methods such as mechanical mixing and impregnation processes have problems with uniform distribution and difficulty in control.
The composite electrode material La0.8Sr1.2FeO4+δ-xLa0.4Sr0.6FeO3-δ is synthesized using a one-pot method. The composite electrode material powder is prepared by the citric acid-nitrate combustion method, and the introduction amount of the second phase material is controlled to achieve uniform distribution. and high stability.
It achieves high thermodynamic stability and uniform distribution of the composite electrode material, improves the catalytic activity and electrochemical stability of the SOFC cathode, and improves the output power and thermal cycle stability.
Smart Images

Figure CN118336003B_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to the technical field of electrode materials for solid oxide fuel cells, and in particular to a composite electrode material, a preparation method and application thereof, and a solid oxide fuel cell. Background Art
[0002] Energy plays a key role in human development, and the storage and conversion of energy are crucial. Traditional fossil fuels have limited reserves and serious environmental pollution problems, while renewable energy sources such as wind and solar energy also have limitations. Fuel cells have attracted much attention as an efficient and clean way of energy conversion, directly converting chemical energy into electrical energy. Solid oxide fuel cells (SOFCs) are an advanced energy conversion technology that is efficient and clean, converting chemical energy directly into electrical energy through electrochemical reactions. As one of the key materials of SOFC, the cathode has a very important influence on the overall performance of SOFC.
[0003] Ruddlesden-Popper (RP) type perovskite is a promising SOFC cathode material. Its chemical composition is similar to that of simple perovskite materials. The A position is usually an alkaline metal, alkaline earth metal or some rare earth metal cations (such as Na, K, Ca, La, Sr, Nd, etc.), the B position is a transition metal cation (such as Mn, Fe, Co, Ni, Cu, etc.), and O is a negatively charged oxygen ion. Structurally, it consists of an AO rock salt layer and an n-layer single perovskite ABO 3 The unique structure of RP-type perovskite materials makes them have great potential in high catalytic activity and high stability. 3 The larger gaps between single perovskite layers can accommodate interstitial oxygen, which makes some RP-type perovskite materials have higher ionic conductivity, oxygen surface exchange coefficient and volume exchange coefficient than traditional single perovskite materials. The gap between the single perovskite layer and the rock salt layer can also tolerate a part of the lattice expansion, which makes this type of material have a lower thermal expansion coefficient than the single perovskite material with the same chemical element composition. In addition, the rock salt layer of the RP-type perovskite material can also protect the perovskite layer, so it also has great potential in chemical stability. At present, the modification research on RP-type perovskite mainly focuses on the doping of elements at the A and B positions, but this method is difficult to compromise between catalytic activity and stability.
[0004] Among them, some composite modification methods for introducing second phase materials have some disadvantages. For example, although mechanical mixing can improve the performance of the electrode to a certain extent, it is difficult to achieve uniform distribution of the two phases by direct mechanical mixing, which will limit the contact interface between the two phases and is not conducive to charge transfer during the SOFC electrode reaction. In addition, impregnation is also an optional solution for introducing second phase materials. However, the impregnation process is relatively cumbersome, and it is difficult to control the amount of second phase material introduced by impregnation.
[0005] Therefore, we need to develop other methods to modify RP-type perovskites to obtain RP-structured SOFC cathodes with high catalytic activity and high stability. Summary of the invention
[0006] The present disclosure provides a composite electrode material, a preparation method and application thereof, and a solid oxide fuel cell, so as to at least solve one of the technical problems existing in the prior art.
[0007] According to a first aspect of the present disclosure, a composite electrode material is provided, wherein the general chemical formula of the composite electrode material is La 0.8 Sr 1.2 FeO 4+δ -xLa 0.4 Sr 0.6 FeO 3-δ , x = 10 ~ 50 mol%.
[0008] According to a second aspect of the present disclosure, there is provided a method for preparing a composite electrode material, comprising:
[0009] (1), according to the general formula La 0.8 Sr 1.2 FeO 4+δ -xLa 0.4 Sr 0.6 FeO 3-δ , weigh the stoichiometric ratio of La 2 O 3 、Sr(NO 3 ) 3 、Fe(NO 3 ) 3 , and then put the three into a dilute nitric acid aqueous solution to obtain a mixed solution;
[0010] (2) According to Sr 3+ The molar ratio of EDTA to EDTA is 1:1~1.1. Prepare EDTA and La 3+ with Fe 3+ The molar ratio of the sum of the two to CA is 1:2-2.2 to prepare CA, add EDTA and CA to the mixed solution, stir, adjust the pH value of the mixed solution to 7 with ammonia water, and then dry it in a water bath to a gel state;
[0011] (3) placing the gel at 250° C. and allowing it to self-propagate to burn to obtain a precursor powder, and then grinding the precursor powder and calcining it at 1100° C. for 9-11 hours to obtain the composite electrode material.
[0012] In one embodiment, the Sr 3+ The molar ratio of La to EDTA is 1:1; 3+ with Fe 3+ The molar ratio of the sum of the two to CA is 1:2.
[0013] In one embodiment, in step (1), the mass percentage of the solute in the dilute nitric acid aqueous solution is 15 wt% to 20 wt%.
[0014] According to a third aspect of the present disclosure, a solid oxide fuel cell is provided, comprising a cathode material, wherein the cathode material comprises the composite electrode material or the composite electrode material prepared by the preparation method.
[0015] According to a fourth aspect of the present disclosure, there is provided a composite electrode material or an application of the composite electrode material prepared by the preparation method in a solid oxide fuel cell.
[0016] In one possible implementation manner, the composite electrode material or the composite electrode material obtained by the preparation method is used as a cathode material for preparing a solid oxide fuel cell.
[0017] Compared with the prior art, the advantages of the present application are: 1) the composite electrode material of the present application has high thermodynamic stability, and the two phases of the composite electrode material are evenly distributed, which meets the requirements of the cathode material of the solid oxide fuel cell; 2) the present application adopts a one-pot method to synthesize the composite electrode material, wherein the composite electrode material powder is synthesized by the citric acid-nitrate combustion method, and the preparation process is simple, and only the raw material ratio needs to be changed to regulate the introduction amount of the second phase material, and the prepared composite electrode material has thermodynamic stability and evenly distributed two phases; 3) the composite electrode material of the present application has high stability and high catalytic activity when used as the cathode material of the solid oxide fuel cell, so that the prepared solid oxide fuel cell has high thermal cycle stability, electrochemical stability and high output power.
[0018] It should be understood that the content described in this section is not intended to identify the key or important features of the embodiments of the present disclosure, nor is it intended to limit the scope of the present disclosure. Other features of the present disclosure will become easily understood through the following description. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] The above and other objects, features and advantages of the exemplary embodiments of the present disclosure will become readily understood by reading the detailed description below with reference to the accompanying drawings. In the accompanying drawings, several embodiments of the present disclosure are shown in an exemplary and non-limiting manner, in which:
[0020] In the drawings, the same or corresponding reference numerals represent the same or corresponding parts.
[0021] Figure 1 The XRD pattern of the composite electrode material of the embodiment of the present disclosure is shown;
[0022] Figure 2 The SEM-EDX spectrum of the composite electrode material of the embodiment of the present disclosure is shown;
[0023] Figure 3 The cathode single cell IV power density curve of the embodiment of the present disclosure is shown;
[0024] Figure 4 The thermal cycle test and long-term discharge curve of the cathode cell according to the embodiment of the present disclosure are shown. DETAILED DESCRIPTION
[0025] In order to make the purpose, features, and advantages of the present disclosure more obvious and easy to understand, the technical solutions in the embodiments of the present disclosure will be clearly and completely described below in conjunction with the drawings in the embodiments of the present disclosure. Obviously, the described embodiments are only part of the embodiments of the present disclosure, not all of the embodiments. Based on the embodiments in the present disclosure, all other embodiments obtained by those skilled in the art without creative work are within the scope of protection of the present disclosure.
[0026] Solid oxide fuel cells (SOFCs) are all-solid-state systems that are easy to manage and can use a variety of fuels without the need for precious metal catalysts, and have commercial prospects. Exploring new cathode materials and structures is the key to improving the overall performance of SOFCs. Ruddlesden-Popper (RP)-type perovskites have the potential to be higher in catalytic activity and stability than traditional single perovskite materials, but current research always finds it difficult to achieve both high catalytic activity and high stability. An iron-based RP-type perovskite (La, Sr) 2 FeO 4+δ , which has good chemical stability, chemical compatibility with traditional electrolyte materials and thermal expansion compatibility, as well as economical raw materials. However, (La, Sr) 2 FeO 4+δ The catalytic activity is not enough and it is difficult to apply it to SOFC cathode.
[0027] This application aims to improve the catalytic activity of RP-type perovskite without destroying its stability. It proposes to synthesize RP-structure-perovskite composite cathode materials in one step by simply adjusting the raw material ratio. The introduction of cubic perovskite materials can expand the oxygen ion transmission channel. At the same time, perovskite materials are also good electrode materials, which can further improve the electrode catalytic activity. In addition, heterogeneous structural defects can be formed in situ and the oxygen reduction kinetics can be further improved.
[0028] Based on this, the composite electrode material prepared by the one-pot method in this application shows its potential as a SOFC cathode material, providing ideas for the research of SOFC cathode materials with high stability and high catalytic activity.
[0029] Specifically, according to one embodiment of the present disclosure, the present application provides a composite electrode material, the chemical formula of the composite electrode material is La 0.8 Sr 1.2 FeO 4+δ -xLa 0.4 Sr 0.6 FeO 3-δ , x = 10 to 50 mol%. That is, La 04 Sr 06 FeO 3-δ with La 08 Sr 12 FeO 4+δ The molar ratio is 10 to 50 mol%: 1. The minus sign (ie -δ) before δ indicates the number of oxygen defects, and the plus sign (ie +δ) before δ indicates the number of interstitial oxygen.
[0030] The composite electrode material provided in the present application has high thermodynamic stability, and the two phases of the composite electrode material are evenly distributed, meeting the requirements of cathode materials for solid oxide fuel cells.
[0031] The composite electrode material of the present application has high stability and high catalytic activity when used as a cathode material for a solid oxide fuel cell, so that the prepared solid oxide fuel cell has high thermal cycle stability, electrochemical stability and high output power.
[0032] For example, the preparation method of the composite electrode material comprises:
[0033] (1), according to the general formula La 0.8 Sr 1.2 FeO 4+δ -xLa 0.4 Sr 0.6 FeO 3-δ , weigh the stoichiometric ratio of La 2 O 3 、Sr(NO3 ) 3 、Fe(NO 3 ) 3 , and then put the three into a dilute nitric acid aqueous solution to obtain a mixed solution;
[0034] (2) According to Sr 3+ The molar ratio of EDTA to EDTA is 1:1~1.1. Prepare EDTA and La 3+ with Fe 3+ The molar ratio of the sum of the two to CA is 1:2-2.2 to prepare CA, add EDTA and CA to the mixed solution, stir, adjust the pH value of the mixed solution to 7 with ammonia water, and then dry it in a water bath to a gel state;
[0035] (3) The gel is placed at 250°C and allowed to self-propagate to burn to obtain a precursor powder, which is then ground and calcined at 1100°C for 9-11 hours to obtain a composite electrode material.
[0036] The present invention uses ethylenediaminetetraacetic acid (EDTA) and citric acid (CA) as complexing agents and adopts the citric acid-nitrate combustion method to synthesize La 0.8 Sr 1.2 FeO 4+δ -xLa 0.4 Sr 0.6 FeO 3-δ Composite powder.
[0037] Compared with the existing RP structural material modification method, the one-pot synthesis of composite electrode materials can produce thermodynamically stable and uniformly distributed two phases in a simple step, and the amount of the second phase material introduced can be regulated by simply changing the raw material ratio. The one-pot method of the present application has great potential to provide a large number of heterogeneous structural interfaces for composite cathode materials, which can enhance the oxygen reduction reaction kinetics of the electrode.
[0038] The present application introduces a single perovskite structure into the RP structure through a one-pot synthesis, thereby improving its catalytic activity without destroying its stability.
[0039] Preferably, Sr 3+ The molar ratio of La to EDTA is 1:1; 3+ with Fe 3+ The molar ratio of the sum of the two to CA is 1:2.
[0040] Preferably, in step (1), the mass percentage of the solute in the dilute nitric acid aqueous solution is 15wt% to 20wt%, that is, the solute-dilute nitric acid accounts for 15wt% to 20wt% of the entire dilute nitric acid aqueous solution.
[0041] In a second aspect, the present application also provides the use of the composite electrode material or the composite electrode material prepared by the above preparation method in a solid oxide fuel cell.
[0042] Preferably, the composite electrode material is used as a cathode material for preparing a solid oxide fuel cell.
[0043] For example, the solid oxide fuel cell includes a cathode material, and the cathode material includes a composite electrode material or a composite electrode material prepared by the above preparation method. The cathode material is prepared by preparing a cathode slurry with a mass ratio of 100:40:10:5 including the composite electrode material: dispersant: binder: pore former, and then screen-printing the cathode slurry on the surface of the electrolyte layer on the cathode side, drying, and sintering.
[0044] The present application is further described in detail below with reference to specific embodiments.
[0045] Example 1
[0046] A composite electrode material (La 0.8 Sr 1.2 FeO 4+δ -10mol%La 0.4 Sr 0.6 FeO 3-δ ), comprising:
[0047] (1) Based on the composite electrode material La 0.8 Sr 1.2 FeO 4+δ -10mol%La 0.4 Sr 0.6 FeO 3-δ , weigh the stoichiometric ratio of La 2 O 3 、Sr(NO 3 ) 3 、Fe(NO 3 ) 3 , and then placing the three in a dilute nitric acid aqueous solution to obtain a mixed solution; wherein the mass percentage of the solute in the dilute nitric acid aqueous solution is 18wt%;
[0048] (2) According to Sr 3+ The molar ratio of EDTA to EDTA is 1:1. 3+ with Fe 3+ CA was prepared at a molar ratio of 1:2 between the sum of the two and CA, EDTA and CA were added to the mixed solution, and after sufficient stirring, the pH value of the mixed solution was adjusted to 7 with ammonia water in a fume hood, and then dried in a water bath to a gel state;
[0049] (3) The gel was placed in a 250°C forced air oven to self-propagate combustion to obtain a precursor powder, and then the precursor powder was ground and calcined in a muffle furnace at 1100°C for 10 h to obtain a composite electrode material. The general chemical formula of the composite electrode material is La 0.8 Sr 1.2 FeO 4+δ -10mol%La 0.4 Sr 0.6 FeO 3-δ .
[0050] Example 2
[0051] The preparation of Example 2 is substantially the same as that of Example 1, except that the chemical formula of the composite electrode material prepared in Example 2 is La 0.8 Sr 1.2 FeO 4+δ -20mol%La 0.4 Sr 0.6 FeO 3-δ .
[0052] Example 3
[0053] The preparation of this embodiment 3 is substantially the same as that of embodiment 1, except that the chemical formula of the composite electrode material prepared in this embodiment 3 is La 0.8 Sr 1.2 FeO 4+δ -30 mol% La 0.4 Sr 0.6 FeO 3-δ .
[0054] Example 4
[0055] The preparation of this embodiment 4 is substantially the same as that of embodiment 1, except that the chemical formula of the composite electrode material prepared in this embodiment 4 is La 0.8 Sr 1.2 FeO 4+δ -40 mol% La 0.4 Sr 0.6 FeO 3-δ .
[0056] Example 5
[0057] The preparation of this embodiment 5 is substantially the same as that of embodiment 1, except that the chemical formula of the composite electrode material prepared in this embodiment 5 is La 0.8 Sr 1.2 FeO 4+δ -50 mol% La 0.4 Sr 0.6 FeO 3-δ .
[0058] Comparative Example 1
[0059] The preparation of this comparative example 1 is substantially the same as that of Example 1, except that the chemical formula of the electrode material prepared in this comparative example 1 is La 0.4 Sr 0.6 FeO 3-δ , referred to as LSF-P.
[0060] Comparative Example 2
[0061] The preparation of this comparative example 2 is substantially the same as that of Example 1, except that the chemical formula of the electrode material prepared in this comparative example 2 is La 0.8 Sr 1.2 FeO 4+δ , referred to as LSF-RP.
[0062] Performance Testing
[0063] 1: First, the cathode slurry is prepared by mixing the electrode material: dispersant: binder: pore-forming agent in a ratio of 100:40:10:5, wherein the dispersant is pine alcohol, the binder is ethyl cellulose, and the pore-forming agent is glutinous rice flour. Subsequently, the prepared cathode slurry is screen-printed on the surface of the electrolyte layer on the cathode side to obtain a semi-finished battery. After drying, the semi-finished battery is placed in a muffle furnace, heated at a heating rate of 3°C / min, and sintered at 1150°C for 2h to obtain a button-shaped solid oxide fuel cell (referred to as "button battery", the same below). Finally, we placed the packaged battery in a button battery test furnace and tested the various properties of the button battery through an electrochemical workstation.
[0064] For the power generation performance of a single cell (i.e., a button cell), we introduced 100 mL / min of humidified hydrogen into the anode side of the cell and recorded the output characteristics and impedance characteristics of the cell at different temperatures (650-850°C, with an interval temperature of 50°C).
[0065] For the thermal cycle stability of the single cell, a thermal cycle test was performed in the temperature range of 200°C to 800°C, with a thermal cycle heating and cooling rate of 10°C / min, and the OCV (open circuit voltage) of the single cell was recorded.
[0066] In addition, for the long-term stability of power generation of the single cell, we also introduced 100 mL / min of humidified hydrogen into the anode of the single cell and recorded the voltage-time relationship curve of the single cell under constant current.
[0067] According to the ratio of electrode material: dispersant: binder: pore-forming agent = 100:40:10:5, the composite electrode materials of Examples 1-5 and the electrode materials prepared in Comparative Examples 1-2 were used to prepare button batteries.
[0068] The dispersant may be replaced by fish oil or triethanolamine instead of pineol, the binder may be replaced by polyvinyl alcohol, polyvinyl butyral or acrylic emulsion instead of ethyl cellulose, and the pore-forming agent may be starch.
[0069] 2. The composite electrode materials prepared in the above examples 1-5 and the electrode materials prepared in the comparative examples 1-2 were subjected to XRD test. The results are as follows: Figure 1 shown.
[0070] from Figure 1 We can find that the diffraction patterns of the composite electrode materials with different proportions synthesized by the one-pot method are consistent with the standard JCPDS card 34-0641 (SrFeO 3-x ) and 29-1305(LaSrFeO 4 ) corresponds well. This shows that we have synthesized different proportions of La by one-pot method. 0.8 Sr 1.2 FeO 4+δ -xLa 0.4 Sr 0.6 FeO 3-δ Composite electrode materials.
[0071] 3. The composite electrode material La prepared in Example 1 0.8 Sr 1.2 FeO 4+δ -10mol%La 0.4 Sr 0.6 FeO 3-δ The microstructure and local distribution of elements were observed by scanning electron microscope (SEM-EDX). Figure 2 shown.
[0072] Figure 2 a shows the composite electrode material La 0.8 Sr 1.2 FeO 4+δ -10mol%La 0.4 Sr 0.6 FeO 3-δ SEM-EDX images of Figure 2 b shows the composite electrode material La 0.8 Sr 1.2 FeO 4+δ -10mol%La 0.4 Sr 0.6 FeO 3-δ The element distribution of Figure 2 We can find that the amount of Sr and O in the flake particles is higher than that in the small particles. 0.8 Sr 1.2FeO 4+δ The existence of SrO salt rock layer in the phase, the ratio of Sr and O elements is higher than that of La 0.4 Sr 0.6 FeO 3-δ Therefore, we speculate that Figure 2 The small particles in a represent La 0.4 Sr 0.6 FeO 3-δ phase, while the large flake-like particles represent La 0.8 Sr 1.2 FeO 4+δ From the overall SEM-EDX image, the two phases of the composite electrode material are evenly distributed and loose and porous, which meets the requirements of SOFC cathode materials.
[0073] 4. The composite electrode material prepared in Example 1 and the electrode material La prepared in Comparative Example 2 are 0.8 Sr 1.2 FeO 4+δ The "button batteries" were prepared respectively. The IV power density test of the "button batteries" was carried out, and the results were as follows Figure 3 shown.
[0074] Figure 3 a shows the electrode material La prepared in Comparative Example 2 0.8 Sr 1.2 FeO 4+δ is the single cell output power of the cathode material, Figure 3 b shows the composite electrode material La prepared in Example 1 0.8 Sr 1.2 FeO 4+δ -10mol%La 0.4 Sr 0.6 FeO 3-δ The single cell output power of the cathode material.
[0075] Figure 3 In a, as the temperature rises from 650℃ to 850℃, the output power also increases successively, and the output power increases from 88mw.cm -2 Increased to 579mw.cm -2 . Figure 3 In b, as the temperature rises from 650℃ to 850℃, the output power also increases successively, and the output power increases from 231mw.cm -2 Increased to 890mw.cm -2 It can be seen from this that the composite electrode material after composite modification of the present application has high catalytic activity, and the composite electrode material after composite modification of the present application has obviously higher output power when used in SOFC cells.
[0076] 5. The single cell prepared by the composite electrode material prepared in Example 1 was subjected to thermal cycle test and discharge test. The results are as follows: Figure 4 shown.
[0077] Figure 4 a shows the thermal cycle test curve of a composite cathode single cell (i.e., a single cell prepared with a composite electrode material as the cathode material). Figure 4 b shows the long-term discharge curve of the composite cathode single cell. Figure 4 a and Figure 4 In b, we can see that the OCV (open circuit voltage) of the composite cathode single cell has basically not decayed after 20 thermal cycles, and the voltage of the battery has remained stable during the 100h long-term constant current discharge test. This shows that the composite electrode material after the composite modification has good thermal cycle stability and electrochemical stability when used in solid oxide fuel cells.
[0078] It should be understood that the various forms of processes shown above can be used to reorder, add or delete steps. For example, the steps recorded in this disclosure can be executed in parallel, sequentially or in different orders, as long as the desired results of the technical solutions disclosed in this disclosure can be achieved, and this document does not limit this.
[0079] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Thus, a feature defined as "first" or "second" may explicitly or implicitly include at least one of the features. In the description of the present disclosure, the meaning of "plurality" is two or more, unless otherwise clearly and specifically defined.
[0080] The above is only a specific embodiment of the present disclosure, but the protection scope of the present disclosure is not limited thereto. Any person skilled in the art who is familiar with the technical field can easily think of changes or substitutions within the technical scope disclosed in the present disclosure, which should be included in the protection scope of the present disclosure. Therefore, the protection scope of the present disclosure should be based on the protection scope of the claims.
Claims
1. A composite electrode material, characterized in that: The chemical formula of the composite electrode material is La 0.8 Sr 1.2 FeO 4+δ -xLa 0.4 Sr 0.6 FeO 3-δ , x = 10~50mol%; among which, La 0.8 Sr 1.2 FeO 4+δ :xLa 0.4 Sr 0.6 FeO 3-δ =1: x, +δ represents the number of interstitial oxygen, -δ represents the number of oxygen defects; Wherein, the preparation method of the composite electrode material comprises: (1), according to the general formula La 0.8 Sr 1.2 FeO 4+δ -xLa 0.4 Sr 0.6 FeO 3-δ , weigh La2O3, Sr(NO3)3, and Fe(NO3)3 in a stoichiometric ratio, and then place the three in a dilute nitric acid aqueous solution to obtain a mixed solution; (2) According to Sr. 3+ The molar ratio of EDTA to EDTA is 1:1~1.
1. Prepare EDTA and La 3+ with Fe 3+ The molar ratio of the sum of the two to CA is 1:2-2.2 to prepare CA, add EDTA and CA to the mixed solution, stir, adjust the pH value of the mixed solution to 7 with ammonia water, and then dry it in a water bath to a gel state; (3) placing the gel at 250° C. and allowing it to self-propagate to burn to obtain a precursor powder, and then grinding the precursor powder and calcining it at 1100° C. for 9-11 hours to obtain the composite electrode material; wherein CA is citric acid.
2. The composite electrode material according to claim 1, characterized in that The Sr 3+ The molar ratio of La to EDTA is 1:1; 3+ with Fe 3+ The molar ratio of the sum of the two to CA is 1:
2.
3. The composite electrode material according to claim 1, characterized in that In the step (1), the mass percentage of the solute in the dilute nitric acid aqueous solution is 15wt%~20wt%.
4. A solid oxide fuel cell comprising a cathode material, characterized in that: The cathode material comprises the composite electrode material according to any one of claims 1 to 3.
5. Use of the composite electrode material according to any one of claims 1 to 3 in a solid oxide fuel cell.