Solar cell module and preparation method thereof and solar cell

By introducing an interface modification layer into the solar cell, the transport layer and active layer surface are passivated by carbonyl or a material that can ionize hydrogen ions, the interface defect problem is solved and the photoelectric conversion efficiency and performance of the solar cell are significantly improved.

CN118338694BActive Publication Date: 2024-11-15SUZHOU GUOXIAN INNOVATION TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410774246.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-17
Publication Date
2024-11-15
Estimated Expiration
2044-06-17

AI Technical Summary

Technical Problem

The interface defect problem of solar cells affects its performance improvement, especially when there are problems with the interface between the film layers, resulting in a decrease in efficiency.

Method used

Using an interface modification layer, the material molecular formula includes carbonyl or a material that can ionize hydrogen ions, which is used to passivate the surface of the first transport layer and the active layer, reduce the vacant ions on the surface through the interface modification layer, reduce interface defects, and improve the solar cell. performance.

Benefits of technology

Through the use of the interface modification layer, the open circuit voltage, short circuit current density and filling factor of the solar cell are significantly improved, the photoelectric conversion efficiency is improved, the interface defects are reduced, and the device performance is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118338694B_ABST
    Figure CN118338694B_ABST
Patent Text Reader

Abstract

The present application discloses a solar cell assembly, a preparation method thereof and a solar cell. The solar cell assembly includes a stacked substrate, a first transmission layer, an interface modification layer, an active layer and a second transmission layer. The first transmission layer, the active layer and the second transmission layer realize the photoelectric conversion function of the solar cell. The interface modification layer is arranged between the first transmission layer and the active layer, and the material of the interface modification layer is used to ionize hydrogen ions, so that the interface modification layer coordinates the free ions on the surface of the first transmission layer close to the active layer, reduces the vacancy ions on the surface of the first transmission layer, and realizes the passivation of the surface of the first transmission layer, and can coordinate the free ions on the surface of the active layer close to the first transmission layer, reduce the vacancy ions on the buried surface of the active layer, and realize the passivation of the buried surface of the active layer, thereby reducing the interface defects of the solar cell assembly and improving the device performance of the solar cell assembly.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of solar cells, and in particular to a solar cell assembly and a preparation method thereof, and a solar cell. Background Art

[0002] The development of semiconductor technology plays a vital role in the progress of the electronics industry. As a new type of semiconductor, perovskite has many advantages such as long carrier diffusion length, high defect tolerance, adjustable band gap, and large absorption coefficient. Compared with traditional organic and inorganic semiconductors, perovskite has a simple preparation process and low cost, which has great advantages in the semiconductor field. Up to now, the efficiency of perovskite solar cells has exceeded 26%, and T95 has exceeded thousands of hours. In addition, it has been studied and applied in light-emitting diodes, detectors, lasers, etc. As an emerging semiconductor material, perovskite shows great potential.

[0003] Solar cells are a path to green and low-carbon energy. Perovskite solar cells have the advantages of high photoelectric conversion efficiency, low cost, and environmentally friendly materials. They are gradually becoming a popular solar cell and a key development direction of the solar cell industry.

[0004] At present, there are still some problems between the interfaces of various film layers of solar cells, which affects the further improvement of solar cell performance. Summary of the invention

[0005] The embodiments of the present application provide a solar cell assembly and a method for preparing the same, and a solar cell, aiming to improve the interface defect problem of the solar cell.

[0006] A first aspect of the present application provides a solar cell assembly, comprising: a substrate; a first transmission layer, an interface modification layer, an active layer and a second transmission layer stacked in sequence on one side of the substrate, the first transmission layer being located on a side of the interface modification layer close to the substrate; wherein the interface modification layer is used to passivate a surface of the first transmission layer close to the active layer, the interface modification layer is used to passivate a surface of the active layer close to the first transmission layer, the molecular formula of the material of the interface modification layer includes a carbonyl group, and / or the material of the interface modification layer is used to ionize hydrogen ions.

[0007] According to an embodiment of the first aspect of the present application, the molecular formula of the material of the interface modification layer includes a carboxyl group.

[0008] According to any of the aforementioned embodiments of the first aspect of the present application, the material of the interface modification layer includes at least one of auxin or auxin-like substances.

[0009] According to any of the aforementioned embodiments of the first aspect of the present application, the auxin-like substances include 4-chloro-IAA, 5-hydroxy-IAA, and indolebutyric acid.

[0010] According to any of the aforementioned embodiments of the first aspect of the present application, the thickness of the interface modification layer is 1 nm to 20 nm.

[0011] According to any of the aforementioned embodiments of the first aspect of the present application, the thickness of the interface modification layer is 1 nm to 6 nm.

[0012] According to any of the aforementioned embodiments of the first aspect of the present application, the active layer includes a perovskite material.

[0013] According to any of the aforementioned embodiments of the first aspect of the present application, the material of the active layer includes at least one of auxin or auxin-like substances.

[0014] According to any of the aforementioned embodiments of the first aspect of the present application, it also includes: a first electrode layer and a second electrode layer, the first electrode layer is located between the substrate and the first transport layer, and the second electrode layer is located on the side of the second transport layer away from the substrate; the first electrode layer is a positive electrode, the first transport layer is a hole transport layer, the second transport layer is an electron transport layer, and the second electrode layer is a negative electrode.

[0015] According to any of the aforementioned embodiments of the first aspect of the present application, the material of the first transmission layer includes metal oxide.

[0016] According to any of the aforementioned embodiments of the first aspect of the present application, the material of the first transmission layer includes NiO x , SnO2, ZnO2.

[0017] According to any of the aforementioned embodiments of the first aspect of the present application, the thickness of the first transmission layer is 50 nm to 60 nm.

[0018] According to any of the aforementioned embodiments of the first aspect of the present application, the thickness of the first transmission layer is 5 nm to 40 nm.

[0019] According to any of the aforementioned embodiments of the first aspect of the present application, the thickness of the second transmission layer is 10 nm to 30 nm.

[0020] According to any of the aforementioned embodiments of the first aspect of the present application, the material of the second transmission layer includes metal oxide or carbon-based material.

[0021] According to any of the aforementioned embodiments of the first aspect of the present application, the material of the second transmission layer includes at least one of SnO2, ZnO2, fullerene or a fullerene derivative.

[0022] According to any of the aforementioned embodiments of the first aspect of the present application, the thickness of the active layer is 200 nm to 800 nm.

[0023] According to any of the aforementioned embodiments of the first aspect of the present application, the material of the first electrode layer includes a transparent conductive material.

[0024] According to any of the aforementioned embodiments of the first aspect of the present application, the material of the first electrode layer includes a transparent conductive oxide.

[0025] According to any of the aforementioned embodiments of the first aspect of the present application, the material of the first electrode layer includes indium tin oxide or fluorine-doped tin oxide.

[0026] According to any of the aforementioned embodiments of the first aspect of the present application, the material of the second electrode includes a conductive oxide or a conductive metal or a conductive carbon-based material.

[0027] According to any of the aforementioned embodiments of the first aspect of the present application, the thickness of the first electrode layer and / or the second electrode is 100 nm to 500 nm.

[0028] According to any of the aforementioned embodiments of the first aspect of the present application, it also includes: an auxiliary functional layer located between the second transmission layer and the second electrode layer.

[0029] According to any of the aforementioned embodiments of the first aspect of the present application, the material of the auxiliary functional layer includes organic small molecules, BCP, TPBI, SnO2, LiF, MgF2, and organic metal salts.

[0030] According to any of the aforementioned embodiments of the first aspect of the present application, the material of the auxiliary functional layer includes organic material or inorganic material.

[0031] According to any of the aforementioned embodiments of the first aspect of the present application, the thickness of the auxiliary functional layer is 2 nm to 60 nm.

[0032] According to any of the aforementioned embodiments of the first aspect of the present application, the thickness of the auxiliary functional layer is 2nm~40nm.

[0033] The second aspect of the present application provides a method for preparing a solar cell assembly, comprising:

[0034] Sequentially preparing a first electrode layer and a first transmission layer on a substrate;

[0035] preparing an interface modification layer on a side of the first transport layer away from the first electrode layer;

[0036] An active layer, a second transport layer and a second electrode layer are sequentially prepared on a side of the interface modification layer away from the first transport layer, wherein the interface modification layer is used to passivate the surface of the first transport layer close to the active layer, and the interface modification layer is used to passivate the surface of the active layer close to the first transport layer, the molecular formula of the material of the interface modification layer includes a carbonyl group, and / or the material of the interface modification layer is used to ionize hydrogen ions.

[0037] According to an embodiment of the second aspect of the present application, in the step of preparing an interface modification layer on a side of the first transmission layer away from the first electrode layer, the method further comprises:

[0038] preparing an auxin solution or an auxin-like solution;

[0039] Coating an auxin solution or an auxin-like solution on a side of the first transport layer facing away from the first electrode layer;

[0040] The auxin solution or the auxin-like solution is heated and annealed to form an interface modification layer.

[0041] According to any of the aforementioned embodiments of the second aspect of the present application, in the steps of sequentially preparing the first electrode layer and the first transport layer, the method further comprises:

[0042] preparing nanoparticle solutions;

[0043] coating a nanoparticle solution on one side of the first electrode layer;

[0044] The nanoparticle solution is heated and annealed to form a first transport layer.

[0045] According to any of the aforementioned embodiments of the second aspect of the present application, in the step of sequentially preparing the active layer, the second transport layer, and the second electrode layer on the side of the interface modification layer away from the first transport layer, the method further comprises:

[0046] Preparing a perovskite precursor solution;

[0047] coating a perovskite precursor solution on a side of the interface modification layer facing away from the first transport layer;

[0048] adding an antisolvent dropwise to the perovskite precursor solution;

[0049] The perovskite precursor solution is heated and annealed to form an active layer.

[0050] An embodiment of the third aspect of the present application provides a solar cell, which includes a solar cell component of any of the above-mentioned embodiments or a solar cell component prepared by a preparation method of any of the above-mentioned embodiments.

[0051] According to the solar cell assembly of the embodiment of the present application, the solar cell assembly includes a stacked substrate, a first transmission layer, an interface modification layer, an active layer and a second transmission layer. The first transmission layer, the active layer and the second transmission layer realize the photoelectric conversion function of the solar cell. The interface modification layer is arranged between the first transmission layer and the active layer, and the molecular formula of the material of the interface modification layer includes a carbonyl group, and / or the material of the interface modification layer is used to ionize hydrogen ions, so that the interface modification layer coordinates the free ions on the surface of the first transmission layer close to the active layer, reduces the vacancy ions on the surface of the first transmission layer, and realizes the passivation of the surface of the first transmission layer, and can coordinate the free ions on the surface of the active layer close to the first transmission layer, reduce the vacancy ions on the buried surface of the active layer, and realize the passivation of the buried surface of the active layer, thereby reducing the interface defects of the solar cell assembly and improving the device performance of the solar cell assembly. BRIEF DESCRIPTION OF THE DRAWINGS

[0052] Other features, objects and advantages of the present application will become more apparent by reading the following detailed description of non-limiting embodiments with reference to the accompanying drawings, in which the same or similar reference numerals represent the same or similar features and the accompanying drawings are not drawn to scale.

[0053] Figure 1 is a partial cross-sectional view of a solar cell assembly provided in an embodiment of the present application;

[0054] Figure 2 is a current-voltage curve diagram of a solar cell assembly provided in an embodiment of the present application;

[0055] Figure 3 is a partial cross-sectional view of a solar cell assembly in another embodiment;

[0056] Figure 4 It is a schematic flow chart of a method for preparing a solar cell module provided in an embodiment of the present application;

[0057] Figures 5 to 10 It is a schematic diagram of a preparation process of a solar cell module provided in an embodiment of the present application.

[0058] Description of reference numerals:

[0059] 10. Solar cell module; 11. Substrate;

[0060] 100. a first electrode layer;

[0061] 200, first transport layer;

[0062] 300, interface modification layer;

[0063] 400, active layer;

[0064] 500, second transport layer;

[0065] 600, second electrode layer;

[0066] 700. Auxiliary function layer. DETAILED DESCRIPTION

[0067] The features and exemplary embodiments of various aspects of the present application will be described in detail below. In order to make the purpose, technical solutions and advantages of the present application clearer, the present application will be further described in detail below in conjunction with the accompanying drawings and specific embodiments. It should be understood that the specific embodiments described herein are only configured to explain the present application and are not configured to limit the present application. For those skilled in the art, the present application can be implemented without the need for some of these specific details. The following description of the embodiments is only to provide a better understanding of the present application by illustrating the examples of the present application.

[0068] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the statement "include..." do not exclude the presence of other identical elements in the process, method, article or device including the elements.

[0069] It should be understood that when describing the structure of a component, when a layer or a region is referred to as being "on" or "over" another layer or another region, it may mean that it is directly on the other layer or another region, or that other layers or regions are included between it and the other layer or another region. Moreover, if the component is turned over, the layer or a region will be "below" or "beneath" another layer or another region.

[0070] The embodiments of the present application provide a solar cell and a method for manufacturing the same. The embodiments of the solar cell and the method for manufacturing the same are described below in conjunction with the accompanying drawings.

[0071] See also Figure 1 , Figure 1 It is a partial cross-sectional view of a solar cell assembly provided in an embodiment of the present application.

[0072] like Figure 1As shown, the first aspect of the present application provides a solar cell assembly 10, which includes a stacked substrate 11, a first transmission layer 200, an interface modification layer 300, an active layer 400 and a second transmission layer 500, wherein the first transmission layer 200 is located on a side of the interface modification layer 300 close to the substrate 11; wherein the interface modification layer 300 is used to passivate the surface of the first transmission layer 200 close to the active layer 400, the interface modification layer 300 is used to passivate the surface of the active layer 400 close to the first transmission layer 200, the molecular formula of the material of the interface modification layer 300 includes a carbonyl group, and / or the material of the interface modification layer 300 is used to ionize hydrogen ions.

[0073] According to the solar cell assembly 10 of the embodiment of the present application, the solar cell assembly 10 includes a stacked substrate 11, a first transmission layer 200, an interface modification layer 300, an active layer 400 and a second transmission layer 500. The first transmission layer 200, the active layer 400 and the second transmission layer 500 realize the photoelectric conversion function of the solar cell. The interface modification layer 300 is arranged between the first transport layer 200 and the active layer 400, and the molecular formula of the material of the interface modification layer 300 includes a carbonyl group (C=O), and / or the material of the interface modification layer 300 is used to ionize hydrogen ions, so that the interface modification layer 300 coordinates the free ions on the surface of the first transport layer 200 close to the active layer 400, reduces the vacancy ions on the surface of the first transport layer 200, and achieves passivation of the surface of the first transport layer 200, and can coordinate the free ions on the surface of the active layer 400 close to the first transport layer 200, reduce the vacancy ions on the buried surface of the active layer 400, and achieve passivation of the buried surface of the active layer 400, thereby reducing the interface defects of the solar cell module 10 and improving the device performance of the solar cell module 10.

[0074] For example, the O in the carbonyl group of the interface modification layer 300 can coordinate with the metal ions in the active layer 400, thereby reducing the vacant ions on the buried surface of the active layer 400, and passivating the buried surface of the active layer 400. The interface modification layer 300 can ionize hydrogen ions, and the hydrogen ions can coordinate with the vacant O in the first transport layer 200, thereby reducing the vacant O on the surface of the first transport layer 200, and passivating the surface of the first transport layer 200.

[0075] Optionally, the material of the active layer 400 includes a perovskite material. The general chemical formula of the perovskite active layer 400 is ABX3, wherein A is a monovalent metal cation or an organic cation, which can be selected from at least one of CH3NH3, C4H9NH3, NH2=CHNH2, and Cs; B is a divalent metal cation, which can be selected from at least one of Pb and Sn; X - is a monovalent anion, which can be selected from Cl - Br -or I - Halogen ions, SCN - At least one or more of the pseudo-halogen ions, such as multiple X ions, whose total ratio satisfies the general chemical formula of the perovskite active layer 400. For example, one or more of CsPbI3, CsPbI2Br, CsPbIBr2, CsPbBr3, CsSnI3, or organic-inorganic hybrid perovskites, such as one or more of FAPbI3, MAPbI3, FAPbBr3, MAPbBr3, or multi-system organic-inorganic-hybrid perovskites, such as Cs 0.05 FA 0.9 MA 0.05 Pb(I 0.95 Br 0.05 )3. Cs 0.05 FA 0.95 One or more of PbI3.

[0076] Optionally, the material molecular formula of the interface modification layer includes a carboxyl group (-COOH), which can include both a carbonyl group and ionize hydrogen ions, and the hydrogen ions are combined with the vacant O of the first transport layer 200 to reduce the number of vacant O in the first transport layer 200, thereby passivating the first transport layer 200. In addition, the O of the carbonyl group in the carboxyl group can coordinate with the vacant Pb ions or vacant Sn ions in the active layer 400 to reduce the number of vacant ions in the active layer 400, thereby passivating the buried interface of the active layer 400, thereby reducing the interface defects of the solar cell module 10 and improving the device performance of the solar cell module 10.

[0077] For example, in some optional embodiments, the material of the interface modification layer 300 includes at least one of auxin (IAA) or auxin-like substances.

[0078] In these optional embodiments, the carboxyl group of the auxin or auxin-like substances can ionize hydrogen ions, thereby combining with the vacant O in the first transmission layer 200 to reduce the number of vacant O in the first transmission layer 200, thereby passivating the first transmission layer 200. In addition, the carboxyl group (-COOH) of the auxin or auxin-like substances can coordinate with the vacant Pb ions or vacant Sn ions in the active layer 400 to reduce the number of vacant ions in the active layer 400, thereby passivating the buried interface of the active layer 400, thereby reducing the interface defects of the solar cell module 10 and improving the device performance of the solar cell module 10. Auxin is a natural product with a simple material structure, easy preparation, and low cost.

[0079] Alternatively, the chemical nature of the auxin is indoleacetic acid.

[0080] Optionally, the auxin-like substances include 4-chloro-IAA, 5-hydroxy-IAA, indolebutyric acid, and the like.

[0081] Please also read Figure 2 and Table 1, Figure 2 : is a current-voltage curve diagram of a solar cell assembly provided in an embodiment of the present application; the following table compares the characteristics of solar cell devices in the embodiment of the present application and the comparative example.

[0082] Table 1

[0083]

[0084] like Figure 2 As shown in Table 1, HTL is the hole transport layer, Voc is the device open circuit voltage, Jsc is the short circuit current density, FF is the fill factor, and PCE is the photoelectric conversion efficiency. It can be seen that in Example 1 of the present application, the interface modification layer 300 of IAA is added between the first transport layer 200 and the active layer 400, which is different from the case where only NiO is provided between the first electrode layer 100 and the active layer 400. x Compared with the comparative example, the device open circuit voltage and short circuit current density are significantly improved, and the device efficiency is significantly improved. In Example 2 of the present application, an interface modification layer 300 of 4-chloro-IAA is added between the first transmission layer 200 and the active layer 400, which is different from the case where only NiO is provided between the first electrode layer 100 and the active layer 400. x Compared with the comparative example, the device open circuit voltage and short circuit current density are significantly improved, and the device efficiency is significantly improved. In Example 3 of the present application, an interface modification layer 300 of 5-hydroxy-IAA is added between the first transmission layer 200 and the active layer 400, which is different from only NiO x Compared with the comparative example, the device open circuit voltage and short circuit current density are significantly improved, and the device efficiency is significantly improved. In Example 4 of the present application, an interface modification layer 300 of naphthaleneacetic acid (NAA) is added between the first transmission layer 200 and the active layer 400, which is different from only setting NiO x Compared with the control group, the device open circuit voltage and short circuit current density are significantly improved, and the device efficiency is significantly improved. 4-Chloro-IAA, 5-hydroxy-IAA, naphthylacetic acid (NAA), etc. all have the same structure as IAA, that is, they have a carboxyl group (-COOH), and have the same beneficial effects as IAA.

[0085] In some optional embodiments, the thickness of the interface modification layer 300 is 1 nm to 20 nm. For example, the thickness of the interface modification layer 300 is 1 nm, 2 nm, 3 nm, 6 nm, 20 nm, etc.

[0086] In these optional embodiments, the thickness of the interface modification layer 300 is greater than or equal to 1 nm, so as to avoid the problem that the preparation of the interface modification layer 300 is difficult due to the small thickness of the interface modification layer 300. The thickness of the interface modification layer 300 is less than or equal to 20 nm, so as to avoid the problem that the interface modification layer 300 is too large, so that the carriers cannot undergo quantum tunneling in the interface modification layer 300 (i.e., the quantum behavior of microscopic particles such as carriers being able to penetrate or cross potential barriers), i.e., the interface modification layer 300 is an insulating layer, and the device function of the solar cell module 10 cannot be realized.

[0087] Optionally, the thickness of the interface modification layer 300 is 1 nm to 6 nm. For example, the thickness of the interface modification layer 300 is 1 nm, 2 nm, 3 nm, 4 nm, 5 nm, 6 nm, etc. The interface modification layer 300 within this thickness range has a relatively low preparation difficulty and enables carriers to undergo quantum tunneling in the interface modification layer 300 to realize the device function of the solar cell module 10.

[0088] Optionally, the material of the active layer 400 includes auxin or auxin-like materials, that is, auxin or auxin-like materials are doped in the active layer 400, for example, auxin or auxin-like materials are doped in the perovskite active layer 400, so as to further enable vacant Pb ions or vacant Sn ions in the active layer 400 to coordinate with the carboxyl group (-COOH) of the auxin or auxin-like materials, thereby improving the device performance of the solar cell module 10. Optionally, the material of the active layer 400 includes auxin, which is a natural product, has a simple material structure, is easy to prepare, and has low cost.

[0089] Optionally, one of the first transport layer 200 and the second transport layer 500 is a hole transport layer, and the other is an electron transport layer. The active layer 400 is used to convert incident light into electric charge. The hole transport layer is used to transport holes generated by absorbing photons in the active layer 400; at the same time, the hole transport layer can also block the following electrons to reduce the recombination of holes and electrons. The electron transport layer is used to transport electrons generated by absorbing photons in the perovskite active layer 400, and at the same time, the electron transport layer can also block the above holes to reduce the recombination of holes and electrons. In this article, holes and electrons are collectively referred to as carriers.

[0090] Table 2

[0091]

[0092] Please refer to Table 2 above, which is a comparison of the different O1s peak area ratios in the XPS spectra of the sample film surfaces of the embodiments of the present application and the comparative examples.

[0093] As shown in Table 2 above, in Example 1, relative to bare NiO x Surface, NiOx The characteristic peak area of ​​uncoordinated O on the surface of IAA is significantly reduced, indicating that IAA has a significant effect on NiO x The surface defects play a passivation role, that is, the hydrogen ions ionized by IAA play a passivation role. That is, the auxin can ionize hydrogen ions, which can combine with the vacancies O in the first transport layer 200 to reduce the number of vacancies O in the first transport layer 200, thereby achieving passivation of the first transport layer 200. In Example 2, compared with bare NiO x Surface, NiO x / The characteristic peak area of ​​uncoordinated O on the surface of 4-chloro-IAA is significantly reduced, indicating that 4-chloro-IAA x Surface defects play a passivation role. In Example 3, compared with bare NiO x Surface, NiO x / The characteristic peak area of ​​uncoordinated O on the surface of 5-hydroxy-IAA is significantly reduced, indicating that 5-hydroxy-IAA x Surface defects play a passivation role. In Example 4, compared with bare NiO x Surface, NiO x The characteristic peak area of ​​uncoordinated O on the surface of NAA was significantly reduced, indicating that NAA x Surface defects play a passivating role.

[0094] Please refer to Table 3 below, which shows the different Pb characteristic peak positions in the XPS spectra of the sample film surfaces of the embodiments of the present application and the comparative examples.

[0095] Table 3

[0096]

[0097] As shown in Table 3 above, in Example 1, relative to the bare perovskite surface, the Pb 4f 7 / 2 Characteristic peak Pb4f 5 / 2 The characteristic peaks shifted, indicating that the carboxyl group of IAA and Pb 2+ The coordination occurs, which can passivate the uncoordinated Pb in the perovskite film. That is, the auxin has a carboxyl group (-COOH), which can coordinate with the vacant Pb ions or vacant Sn ions in the active layer 400 to reduce the number of vacant ions in the active layer 400 and achieve passivation of the buried interface of the active layer 400. In Example 2, relative to the bare perovskite surface, the Pb 4f 7 / 2 Characteristic peak Pb 4f 5 / 2 The characteristic peaks shifted, indicating that the carboxyl group of IAA and Pb 2+Coordination occurs, which can passivate the uncoordinated Pb in the perovskite film. In Example 3, relative to the bare perovskite surface, the Pb 4f 7 / 2 Characteristic peak Pb 4f 5 / 2 The characteristic peaks shifted, indicating that the carboxyl group of IAA and Pb 2+ Coordination occurs, which can passivate the uncoordinated Pb in the perovskite film. In Example 4, relative to the bare perovskite surface, the Pb 4f 7 / 2 Characteristic peak Pb 4f 5 / 2 The characteristic peaks shifted, indicating that the carboxyl group of IAA and Pb 2+ Coordination occurs, which can passivate the uncoordinated Pb in the perovskite film.

[0098] The solar cell assembly also includes a first electrode layer 100 and a second electrode layer 600, wherein the first electrode layer 100 is located between the substrate 11 and the first transmission layer 200, and the second electrode layer 600 is located on the side of the second transmission layer 500 away from the substrate 11; the first electrode layer 100 is a positive electrode, the first transmission layer 200 is a hole transmission layer, the second transmission layer 500 is an electron transmission layer, and the second electrode layer 600 is a negative electrode. That is, a solar cell assembly 10 with an inverse structure. When the solar cell assembly 10 is irradiated by sunlight, the active layer 400 absorbs photons to generate electron-hole pairs. Due to the difference in exciton binding energy of the active layer 400 materials, these carriers either become free carriers or form excitons. Moreover, because these active layer 400 materials often have a lower carrier recombination probability and a higher carrier mobility, the diffusion distance and life of the carriers are longer. Then, these uncombined electrons and holes are collected by the electron transport layer and the hole transport layer, respectively, that is, the electrons are transported from the active layer 400 to the electron transport layer, and finally absorbed by the first electrode layer 100 or the second electrode layer 600; the holes are transported from the perovskite layer to the hole transport layer, and finally collected by the first electrode layer 100 or the second electrode layer 600; the photocurrent is realized by connecting the first electrode layer 100 with the circuit of the first electrode layer 100. The first transport layer 200 is a hole transport layer, and the second transport layer 500 is an electron transport layer, then the electrons are transported from the active layer 400 to the second transport layer 500, and finally collected by the second electrode layer 600.

[0099] Optionally, the first transport layer 200 is an electron transport layer, and the second transport layer 500 is a hole transport layer, that is, a solar cell module 10 of a formal structure. In the solar cell module 10 of the formal structure, the interface modification layer 300 should be arranged between the active layer 400 and the second transport layer 500. During preparation, the interface modification layer 300 should be prepared on the surface of the active layer 400. However, when the interface modification layer 300 is IAA with a carboxyl group, the interface modification layer 300 is a polar material with good solubility in polar solvents, but polar solvents will destroy the active layer 400 of the perovskite material. And the second transport layer 500 is a metal oxide, and the raw material has good fluidity, and it is difficult to prepare on the active layer 400 of the perovskite material. Therefore, IAA is better applied to the solar cell module 10 of the trans structure.

[0100] Optionally, the material of the first transmission layer 200 includes metal oxide, such as NiO x , SnO2, ZnO2, etc. When the first transport layer 200 includes a metal oxide, there will be a large number of vacancies O on the surface of the first transport layer 200 close to the active layer 400. An interface modification layer 300 is arranged between the first transport layer 200 and the active layer 400. The hydrogen ions ionized from the interface modification layer 300 can coordinate with the vacancies O, thereby reducing the vacancies O on the surface of the first transport layer 200 and passivating the surface of the first transport layer 200.

[0101] Optionally, the thickness of the first transmission layer 200 is 5 nm to 60 nm. For example, the thickness of the first transmission layer 200 is 5 nm, 10 nm, 15 nm, 40 nm, 60 nm, etc.

[0102] In these optional embodiments, the thickness of the first transmission layer 200 is greater than or equal to 5 nm, so as to avoid the problem that the surface of the first transmission layer 200 is also rough and uneven after the first transmission layer 200 covers the first electrode layer 100 due to the thickness of the first transmission layer 200 being too small and the surface of the first electrode layer 100 being rough, thereby affecting the bonding effect between the first transmission layer 200 and the active layer 400. The thickness of the first transmission layer 200 is less than or equal to 60 nm, so as to avoid the problem that the transmission path of the carriers in the first transmission layer 200 is too long and the carrier transfer efficiency is reduced, that is, the conductivity of the first transmission layer 200 is reduced due to the thickness of the first transmission layer 200 being too large.

[0103] Optionally, the thickness of the first transmission layer 200 is 5 nm to 40 nm. For example, the thickness of the first transmission layer 200 is 5 nm, 10 nm, 15 nm, 20 nm, 30 nm, 40 nm, etc. Within this thickness range, the first transmission layer 200 can ensure both the flatness of the first transmission layer 200 and the carrier transfer efficiency.

[0104] Optionally, the second transmission layer is an electron transport layer, and electrons are transported from the active layer 400 to the second transmission layer 500 and finally collected by the second electrode layer 600 to realize the device function of the solar cell module 10.

[0105] Optionally, the thickness of the second transmission layer 500 is 10 nm to 30 nm. For example, the thickness of the second transmission layer 500 is 10 nm, 15 nm, 20 nm, 30 nm, etc.

[0106] In these optional embodiments, the thickness of the second transmission layer 500 is greater than or equal to 10 nm, which can avoid the problem that the resistance of the second transmission layer 500 is too large and it is difficult to transmit electrons due to the thickness of the second transmission layer 500 is too small. The thickness of the second transmission layer 500 is less than or equal to 30 nm, which can avoid the problem that the transmission distance of electrons is too large and the transmission efficiency of electrons is reduced due to the thickness of the second transmission layer 500 being too large.

[0107] Optionally, the material of the second transmission layer 500 includes metal oxide or carbon-based material. For example, the material of the second transmission layer 500 includes SnO2, ZnO2, fullerene (C60) or fullerene derivative (PCBM), etc., taking into account good conductivity and low cost. When the material of the second transmission layer 500 is fullerene (C60), it can be prepared by thermal evaporation, and when the material of the second transmission layer 500 is PCBM, it can be prepared by solution coating.

[0108] Optionally, the thickness of the active layer 400 is 200 nm to 800 nm, for example, the thickness of the active layer 400 is 200 nm, 300 nm, 500 nm, 800 nm, etc.

[0109] In these optional embodiments, the thickness of the active layer 400 is greater than or equal to 200 nm, so as to avoid the problem that the overall volume of the active layer 400 is reduced and the absorption of light is insufficient due to the thin thickness of the active layer 400, thereby reducing the photovoltaic conversion efficiency (PCE) of the solar cell. The thickness of the active layer 400 is less than or equal to 800 nm, so as to avoid the problem that when the thickness of the active layer 400 is too large, the active layer 400 is composed of multiple layers of crystals, and the carrier transmission efficiency between the interfaces between the crystals is low, that is, the carrier transmission efficiency of the active layer 400 is reduced.

[0110] Optionally, the material of the first electrode layer 100 includes a transparent conductive material, and the transparent first electrode layer 100 serves as the light incident side of the solar cell assembly 10 , so that light can pass through the first electrode layer 100 and the first transmission layer 200 to reach the active layer 400 .

[0111] Optionally, the material of the first electrode layer 100 includes a transparent conductive oxide, such as indium tin oxide (ITO) or fluorine-doped tin oxide (FTO), which has good light transmittance and conductivity.

[0112] Optionally, the material of the second electrode includes conductive oxides or conductive metals or conductive carbon-based materials, such as Au, Ag, Cu, Cr, Al, ITO, FTO, graphite, graphene, carbon nanotubes, etc. Conductive oxides or conductive metals have good conductivity, and conductive carbon-based materials have lower cost.

[0113] Optionally, the thickness of the first electrode layer 100 is 100 nm to 500 nm, for example, the thickness of the first electrode layer 100 is 100 nm, 200 nm, 300 nm, 500 nm, etc.

[0114] In these optional embodiments, the thickness of the first electrode layer 100 is greater than or equal to 100 nm, which can avoid the problem that the resistance of the first electrode layer 100 is large and the conductivity is reduced due to the thickness of the first electrode layer 100 being too small. The thickness of the first electrode layer 100 is less than or equal to 500 nm, which can avoid the problem that the transmittance of the first electrode layer 100 is reduced due to the thickness of the first electrode layer 100 being too large, the relationship of reaching the active layer 400 through the first electrode layer 100 is reduced, and the photoelectric conversion efficiency of the solar cell module 10 is reduced. It can also avoid the problem that the cost is increased due to the thickness of the first electrode layer 100 being too large.

[0115] Optionally, the thickness of the second electrode layer 600 is 100 nm to 500 nm, for example, the thickness of the second electrode layer 600 is 100 nm, 120 nm, 200 nm, 300 nm, 500 nm, etc.

[0116] In these optional embodiments, the thickness of the second electrode layer 600 is greater than or equal to 100 nm, which can avoid the problem of large resistance and reduced conductivity of the second electrode layer 600 due to the thickness of the second electrode layer 600 being too small. The thickness of the second electrode layer 600 is less than or equal to 500 nm, which can avoid the problem of increased material cost of the second electrode layer 600 due to the thickness of the second electrode layer 600 being too large.

[0117] See also Figure 3 , Figure 3 is a partial cross-sectional view of a solar cell module in another embodiment.

[0118] like Figure 3 As shown, in some optional embodiments, an auxiliary functional layer 700 is further included, and the auxiliary functional layer 700 is located between the second transmission layer 500 and the second electrode layer 600 .

[0119] In these optional embodiments, the material of the auxiliary functional layer 700 includes organic materials or inorganic materials. For example, organic small molecules, BCP (2,9-dimethyl-4,7-diphenyl-1,10-phenanthroline), TPBI, SnO2, LiF, MgF2, organic metal salts (MOF), etc. For example, BCP is arranged between the second transmission layer 500 and the second electrode layer 600, which can significantly improve the electron collection rate of the second electrode layer 600 and effectively improve the PCE of the solar cell module 10. When the material of the auxiliary functional layer 700 is an organic small molecule, it can be prepared by thermal evaporation. When the material of the auxiliary functional layer 700 is an inorganic material such as SnO2, it can be prepared by vacuum coating methods such as PVD and ALD.

[0120] Optionally, the thickness of the auxiliary functional layer 700 is 2 nm to 60 nm. For example, the thickness of the auxiliary functional layer 700 is 2 nm, 7 nm, 10 nm, 20 nm, 40 nm, 60 nm, etc.

[0121] In these optional embodiments, the thickness of the auxiliary functional layer 700 is greater than or equal to 2 mm, which can avoid the problem that the thickness of the auxiliary functional layer 700 is too small, resulting in an increased difficulty in preparing the auxiliary functional layer 700. The thickness of the auxiliary functional layer 700 is less than or equal to 40 nm, which avoids the problem that the carriers cannot undergo quantum tunneling in the auxiliary functional layer 700 due to the auxiliary functional layer 700 being too thick, that is, the interface modification layer 300 is an insulating layer, and the device function of the solar cell module 10 cannot be realized. For example, when the material of the auxiliary functional layer 700 is an organic small molecule, the thickness of the auxiliary functional layer 700 is 2 nm to 10 nm, and when the material of the auxiliary functional layer 700 is an inorganic material such as SnO2, the thickness of the auxiliary functional layer 700 is 10 nm to 40 nm.

[0122] Optionally, the thickness of the auxiliary functional layer 700 is 2nm~40nm. For example, the thickness of the auxiliary functional layer 700 is 2nm, 7nm, 10nm, 20nm, 30nm, 40nm, etc. Within this thickness range, the auxiliary functional layer 700 has a lower preparation difficulty and can ensure that carriers undergo quantum tunneling in the auxiliary functional layer 700, thereby realizing the device function of the solar cell module 10.

[0123] The structural design in this embodiment can be applied to other solar cell modules 10 , and the specific selection can be made according to actual conditions, and this application does not impose any specific restrictions on it.

[0124] Please also read Figures 4 to 10 , Figure 4 It is a schematic flow chart of a method for preparing a solar cell module provided in an embodiment of the present application; Figures 5 to 10It is a schematic diagram of a preparation process of a solar cell module provided in an embodiment of the present application.

[0125] like Figures 4 to 10 As shown, an embodiment of the second aspect of the present application provides a method for preparing a solar cell assembly, comprising:

[0126] Step S01: sequentially preparing a first electrode layer and a first transmission layer on a substrate.

[0127] Step S02: preparing an interface modification layer on a side of the first transmission layer away from the first electrode layer.

[0128] Step S03: preparing an active layer, a second transport layer and a second electrode layer in sequence on a side of the interface modification layer facing away from the first transport layer, wherein the interface modification layer is used to passivate the surface of the first transport layer close to the active layer, and the interface modification layer is used to passivate the surface of the active layer close to the first transport layer, the molecular formula of the material of the interface modification layer includes a carbonyl group, and / or the material of the interface modification layer is used to ionize hydrogen ions.

[0129] According to the preparation method of the second aspect of the present application, the solar cell assembly 10 includes a stacked substrate 11, a first electrode layer 100, a first transmission layer 200, an interface modification layer 300, an active layer 400, a second transmission layer 500, and a second electrode layer 600. The first electrode layer 100, the first transmission layer 200, the active layer 400, the second transmission layer 500, and the second electrode layer 600 realize the photoelectric conversion function of the solar cell. The interface modification layer 300 is arranged between the first transport layer 200 and the active layer 400, and the molecular formula of the material of the interface modification layer 300 includes a carbonyl group (C=O), and / or the material of the interface modification layer 300 is used to ionize hydrogen ions, so that the interface modification layer 300 coordinates the free ions on the surface of the first transport layer 200 close to the active layer 400, reduces the vacancy ions on the surface of the first transport layer 200, and achieves passivation of the surface of the first transport layer 200, and can coordinate the free ions on the surface of the active layer 400 close to the first transport layer 200, reduce the vacancy ions on the buried surface of the active layer 400, and achieve passivation of the buried surface of the active layer 400, thereby reducing the interface defects of the solar cell module 10 and improving the device performance of the solar cell module 10.

[0130] Optionally, in step S02, the method further includes:

[0131] preparing an auxin solution or an auxin-like solution;

[0132] Coating an auxin solution or an auxin-like solution on a side of the first transmission layer 200 facing away from the first electrode layer 100;

[0133] The auxin solution or the auxin-like solution is heated and annealed to form an interface modification layer 300 .

[0134] In these optional embodiments, the auxin or auxin-like solution is prepared by a solution method, for example, the IAA solution is an IAA ethanol solution, and the concentration is 0.1-10 mg / mL, for example, the concentration is 0.2 mg / mL, 0.5 mg / mL, 1 mg / mL, 10 mg / mL, etc. And the IAA ethanol solution is coated on the side of the first transmission layer 200 away from the first electrode layer 100 by any one of spin coating, scraping, dipping, slit coating, spraying, printing, vacuum deposition, and film drawing. For example, in the spin coating method, the rotation speed is 3000rpm-3500rpm, and the spin coating is 30s-60s. Finally, annealing is performed at 100℃-120℃ for 10min-20min to form a dry IAA film layer, i.e., the interface modification layer 300, on the surface of the first transmission layer 200.

[0135] Optionally, in the spin coating method, the rotation speed is 3000 rpm, the spin coating is 30 seconds, and finally annealing is performed at 100°C for 10 minutes, or, the rotation speed is 3200 rpm, the spin coating is 40 seconds, and finally annealing is performed at 110°C for 12 minutes, or, the rotation speed is 3500 rpm, the spin coating is 60 seconds, and finally annealing is performed at 120°C for 20 minutes.

[0136] Optionally, in step S01, the method further includes:

[0137] preparing nanoparticle solutions;

[0138] Coating a nanoparticle solution on one side of the first electrode layer 100;

[0139] The nanoparticle solution is heated and annealed to form the first transmission layer 200 .

[0140] In these optional embodiments, the nanoparticle solution is prepared by a solution method, and the nanoparticles may be NiO x , SnO2, ZnO2 and other metal oxide nanoparticles are coated on the surface of the first electrode layer 100 by PVD magnetron sputtering or nanoparticle solution coating, and can also be processed by spin coating, scraping, dipping, slit coating, spraying, printing, vacuum deposition, and film drawing. For example, a nanoparticle aqueous solution with a concentration of 10 mg / mL-20 mg / mL is prepared, and the rotation speed is set to 3000 rpm-3500 rpm for spin coating for 30s-60s, and finally annealed at 100℃-120℃ for 10min-20min to form a dry first transmission layer 200 on the surface of the first electrode layer 100.

[0141] Optionally, a nanoparticle aqueous solution with a concentration of 10 mg / mL is prepared, and the rotation speed is set to 3500 rpm for spin coating for 60 s, and finally annealing at 100°C for 10 min; or, a nanoparticle aqueous solution with a concentration of 15 mg / mL is prepared, and the rotation speed is set to 3200 rpm for spin coating for 35 s, and finally annealing at 120°C for 20 min; or, a nanoparticle aqueous solution with a concentration of 20 mg / mL is prepared, and the rotation speed is set to 3000 rpm for spin coating for 30 s, and finally annealing at 110°C for 10 min.

[0142] Optionally, in step S03, the method further includes:

[0143] Preparing a perovskite precursor solution;

[0144] Coating a perovskite precursor solution on a side of the interface modification layer 300 away from the first transmission layer 200;

[0145] adding an antisolvent dropwise to the perovskite precursor solution;

[0146] The perovskite precursor solution is heated and annealed to form an active layer 400 .

[0147] In these optional embodiments, a perovskite precursor solution is prepared, and the active layer 400 is prepared by a solution method such as slit coating, doctor blade coating, spray coating, inkjet printing, screen printing, or by a method such as vacuum thermal evaporation. For example, CsI (0.05-0.15 equiv), FAI (0.5-1 equiv), PbI2 (0.8-1.2 equiv), and MACl (0.2-0.4 equiv) are weighed in a molar ratio and dissolved in a DMF:DMSO=4:1 solution to prepare a perovskite precursor solution with a solution concentration of 1 mol / ml-1.4 mol / ml, and the perovskite precursor solution is spin-coated at a speed of 3000 rpm-3500 rpm for 30s-60s, and an ethyl acetate anti-solvent is added dropwise in the last 5s, and then annealed at 100°C-150°C for 30min-45min to form a dry active layer 400 on the side of the interface modification layer 300 away from the first transmission layer 200. The addition of an anti-solvent can increase the crystallization rate of the perovskite active material and improve the preparation efficiency. CsI ​​(0.1 equiv) means that the equivalent of CsI is 0.1. In other words, the molar proportion of CsI in the total solute is 0.1. For example, when the equivalent of CsI is 0.1 and the equivalent of PbI2 is 1, if PbI2 is 1 mol, then CsI is 0.1 mol, and the same applies to other materials.

[0148] Optionally, CsI (0.05 equiv), FAI (0.5 equiv), PbI2 (0.8 equiv), and MACl (0.2 equiv) are weighed in a molar ratio and dissolved in a solution of DMF:DMSO=4:1 to prepare a solution concentration of 1 mol / ml-1.4 mol / ml perovskite precursor solution; or, CsI (0.1 equiv), FAI (0.9 equiv), PbI2 (1.0 equiv), and MACl (0.35 equiv) are weighed in a molar ratio and dissolved in a solution of DMF:DMSO=4:1 to prepare a solution concentration of 1 mol / ml-1.4 mol / ml perovskite precursor solution; or, CsI (0.15 equiv), FAI (1 equiv), PbI2 (1.2 equiv), and MACl (0.4 equiv) and dissolved in a solution of DMF:DMSO=4:1 to prepare a perovskite precursor solution with a solution concentration of 1mol / ml-1.4mol / ml. The concentration of the perovskite precursor solution can be 1mol / ml, 1.1mol / ml, 1.3mol / ml, 1.4mol / ml.

[0149] The embodiment of the third aspect of the present application provides a solar cell, which includes the solar cell assembly 10 of any of the above-mentioned embodiments or the solar cell assembly 10 prepared by the preparation method of any of the above-mentioned embodiments. Since the solar cell provided by the embodiment of the third aspect of the present application includes the solar cell assembly 10 of any of the above-mentioned embodiments, the solar cell provided by the embodiment of the third aspect of the present application has the beneficial effects of the solar cell assembly 10 of any of the above-mentioned embodiments, which will not be repeated here.

[0150] According to the embodiments described above, these embodiments do not describe all the details in detail, nor do they limit the invention to the specific embodiments described. Obviously, many modifications and changes can be made based on the above description. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present application, so that those skilled in the art can make good use of the present application and the modifications based on the present application. The present application is limited only by the claims and their full scope and equivalents.

Claims

1. A solar cell module, It is characterized in that include: substrate; A first transmission layer, an interface modification layer, an active layer and a second transmission layer are sequentially stacked on one side of the substrate, wherein the first transmission layer is located on a side of the interface modification layer close to the substrate; The material of the interface modification layer includes at least one of auxin or auxin-like substances, the molecular formula of the material of the interface modification layer includes a carbonyl group, and the material of the interface modification layer is used to ionize hydrogen ions.

2. The solar cell module according to claim 1, It is characterized in that The auxin-like substances include 4-chloro-IAA, 5-hydroxy-IAA, and indolebutyric acid.

3. The solar cell module according to claim 1, It is characterized in that The thickness of the interface modification layer is 1 nm to 20 nm.

4. The solar cell module according to claim 3, It is characterized in that The thickness of the interface modification layer is 1 nm to 6 nm.

5. The solar cell module according to claim 1, It is characterized in that The active layer includes a perovskite material.

6. The solar cell module according to claim 5, It is characterized in that The material of the active layer includes at least one of auxin or auxin-like substances.

7. The solar cell module according to claim 1, It is characterized in that Also includes: A first electrode layer and a second electrode layer, the first electrode layer is located between the substrate and the first transport layer, and the second electrode layer is located on a side of the second transport layer away from the substrate; the first electrode layer is a positive electrode, the first transport layer is a hole transport layer, the second transport layer is an electron transport layer, and the second electrode layer is a negative electrode.

8. The solar cell module according to claim 1, It is characterized in that The material of the first transmission layer includes metal oxide.

9. The solar cell module according to claim 8, It is characterized in that The material of the first transmission layer includes NiO x , SnO 2 , ZnO 2 At least one of .

10. The solar cell module according to claim 1, It is characterized in that The thickness of the second transmission layer is 5nm-60nm.

11. The solar cell module according to claim 10, It is characterized in that The thickness of the first transmission layer is 5nm~40nm.

12. The solar cell module according to claim 1, It is characterized in that The thickness of the second transmission layer is 10nm-30nm.

13. The solar cell module according to claim 1, It is characterized in that The material of the second transmission layer includes metal oxide or carbon-based material.

14. The solar cell module according to claim 13, It is characterized in that The material of the second transmission layer includes SnO 2 , ZnO 2 , at least one of fullerene or a fullerene derivative.

15. The solar cell module according to claim 1, It is characterized in that The thickness of the active layer is 200nm~800nm.

16. The solar cell module according to claim 7, It is characterized in that The thickness of the first electrode layer and / or the second electrode is 100 nm to 500 nm.

17. The solar cell module according to claim 7, It is characterized in that Also includes: The auxiliary functional layer is located between the second transmission layer and the second electrode layer.

18. The solar cell module according to claim 17, It is characterized in that The material of the auxiliary functional layer includes organic material or inorganic material.

19. The solar cell module according to claim 18, It is characterized in that The materials of the auxiliary functional layer include organic small molecules, BCP, TPBI, SnO 2 、LiF、MgF 2 , organic metal salts.

20. The solar cell module according to claim 17, It is characterized in that The thickness of the auxiliary functional layer is 2nm~60nm.

21. The solar cell module according to claim 20, It is characterized in that The thickness of the auxiliary functional layer is 2nm-40nm.

22. A method for preparing a solar cell module, It is characterized in that include: Sequentially preparing a first electrode layer and a first transmission layer on a substrate; preparing an interface modification layer on a side of the first transmission layer away from the first electrode layer; An active layer, a second transport layer and a second electrode layer are sequentially prepared on a side of the interface modification layer away from the first transport layer, wherein the material of the interface modification layer includes at least one of auxin or auxin-like substances, the molecular formula of the material of the interface modification layer includes a carbonyl group, and the material of the interface modification layer is used to ionize hydrogen ions.

23. The preparation method according to claim 22, It is characterized in that In the step of preparing an interface modification layer on a side of the first transmission layer facing away from the first electrode layer, the method further comprises: preparing an auxin solution or an auxin-like solution; Coating the auxin solution or auxin-like solution on a side of the first transmission layer facing away from the first electrode layer; The auxin solution or the auxin-like solution is heated and annealed to form the interface modification layer.

24. The preparation method according to claim 22, It is characterized in that In the step of sequentially preparing the first electrode layer and the first transport layer, the method further comprises: preparing nanoparticle solutions; coating the nanoparticle solution on one side of the first electrode layer; The nanoparticle solution is heated and annealed to form the first transport layer.

25. The preparation method according to claim 22, It is characterized in that In the step of sequentially preparing an active layer, a second transport layer, and a second electrode layer on a side of the interface modification layer away from the first transport layer, the method further comprises: Preparing a perovskite precursor solution; Coating the perovskite precursor solution on a side of the interface modification layer away from the first transport layer; adding an anti-solvent dropwise to the perovskite precursor solution; The perovskite precursor solution is heated and annealed to form the active layer.

26. A solar cell, It is characterized in that It comprises the solar cell module according to any one of claims 1 to 21 or the solar cell module prepared by the preparation method according to any one of claims 22 to 25.