High efficiency and high comprehensive performance welding method for sea pipes under the shaking of pipe-laying vessels

Through ultra-short arc GMAW welding with low heat input and narrow gap U-shaped bevel multi-layer single-channel process, the fatigue and corrosion problems of deep water steel catenary risers in complex marine environments are solved, and the stability and high level of marine pipe welding are achieved Performance, meet service requirements under alternating loads.

CN118342065BActive Publication Date: 2024-11-01TIANJIN UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410648135.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-23
Publication Date
2024-11-01
Estimated Expiration
2044-05-23

AI Technical Summary

Technical Problem

In complex marine environments, deep-water steel catenary risers are prone to shorten their life due to fatigue damage and corrosion and fracture, and the shaking of the pipe laying ship makes it more difficult to weld the sea pipe, resulting in frequent welding instability and defects.

Method used

The ultra-short arc GMAW full-position welding method with low heat input is adopted to optimize the GMAW waveform parameters, and combined with the multi-layer single-channel welding process of narrow gap U-shaped bevels to ensure welding stability and reduce stress concentration, and avoid turbulence of the molten pool metal.

Benefits of technology

It improves the fatigue resistance and corrosion resistance of sea pipes, ensures welding stability, reduces the fatigue performance optimization of joints, avoids unfusion defects, meets the service requirements under alternating loads, and meets the NACE0177 standard through corrosion SSC test.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118342065B_ABST
    Figure CN118342065B_ABST
Patent Text Reader

Abstract

The present application belongs to the field of welding technology, and specifically discloses a high-efficiency and high-comprehensive-performance welding method for sea pipes under the shaking of a pipe-laying vessel, the welding method being: ultra-short arc GMAW full-position welding of sea pipes within the range of heat input of 0.2kJ / mm to 0.3kJ / mm, while setting the peak current in the GMAW waveform to 285A to 370A, the peak current drop rate to 50A / ms to 70A / ms, and the necking time to 3ms to 7ms. The present application can form a welding effect of overall low heat input and local high heat input, and ensure the stability of sea pipe full-position welding, thereby achieving stable sea pipe welding under the condition of the shaking of the pipe-laying vessel, and improving the fatigue resistance and corrosion resistance of the sea pipe.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the field of welding technology, and more specifically, relates to a high-efficiency and high-comprehensive-performance welding method for a subsea pipeline under the shaking of a pipe-laying vessel. Background Art

[0002] Since the first application of Steel Catenary Riser (SCR) in the Auger tension leg platform in the Gulf of Mexico in 1994, it has gained favor in deepwater development due to its strong resistance to high temperature and high pressure, relatively simple manufacturing process, and low cost. However, the complex marine environment and growing production demand have brought more challenges to the design and manufacture of deepwater steel catenary risers.

[0003] As the water depth increases and the length of the riser increases, the marine environment becomes more severe. The generation of underwater vortex-induced oscillations will cause violent vibrations at right angles to the water flow and the axis of the cylinder. At the same time, the steel catenary riser will be connected to the platform through a joint, which will multiply the effect of the alternating load. The riser in this state for a long time will have a shorter life due to frequent operation, which will cause fatigue damage. On the other hand, during the service life of the pipeline, the root weld is in direct contact with the internal gas or liquid. There is great pressure and strong corrosion inside the pipeline. Cracks will be generated from the root defects, which will cause the pipeline to break. At the same time, due to the frequent waves, the pipe-laying ship shakes, which seriously affects the full-position welding process of the sea pipe, thereby further increasing the difficulty of sea pipe welding. Summary of the invention

[0004] In view of the defects of the prior art, the present application provides a high-efficiency and high-comprehensive-performance welding method for subsea pipes under the shaking of a pipe-laying vessel, aiming to solve the problem that subsea pipes are prone to fatigue damage and corrosion fracture, and it is difficult to weld subsea pipes under the shaking of a pipe-laying vessel.

[0005] According to one aspect of the present application, a high-efficiency and high-comprehensive-performance welding method for submarine pipes under shaking of a pipe-laying vessel is provided, which is specifically: ultra-short arc GMAW full-position welding of the submarine pipe is performed within the range of heat input of 0.2kJ / mm to 0.3kJ / mm, and at the same time, the peak current in the GMAW waveform is set to 285A to 370A, the peak current drop rate is set to 50A / ms to 70A / ms, and the necking time is set to 3ms to 7ms, thereby forming an overall low heat input and local high heat input welding effect, thereby ensuring the stability of submarine pipe all-position welding under shaking conditions.

[0006] Compared with the prior art, the above technical solution conceived by the present application adopts low heat input for ultra-short arc GMAW all-position welding and optimizes the parameters in the GMAW waveform, thereby ensuring the stability of all-position welding of subsea pipelines.

[0007] As a further preferred embodiment, during the welding process, the root excess height is ensured to be less than or equal to 0.5 mm.

[0008] As a further preference, a multi-layer single-pass welding process with a narrow gap U-shaped groove is used for welding.

[0009] As a further preferred embodiment, the parameters of the narrow gap U-shaped groove are: blunt edge thickness 1.0 mm to 1.6 mm, arc transition radius 2.4 mm to 3.2 mm, and single-side groove angle 2.5° to 3.5°.

[0010] As a further preferred embodiment, when the sea pipe is welded using the ultra-short arc GMAW technology, the welding current is 160A-200A, the welding voltage is 12V-15V, and the welding speed is 450mm / min-700mm / min.

[0011] As a further preference, the arc length of the ultra-short arc is 1.5 mm to 2.5 mm.

[0012] According to another aspect of the present application, a submarine pipe weld joint prepared by the above welding method is provided.

[0013] In general, the above technical solutions conceived by this application have the following technical advantages compared with the prior art:

[0014] 1. The present application performs ultra-short arc GMAW full-position welding on the subsea pipeline under the condition of low heat input. At the same time, by optimizing the parameters in the GMAW waveform, it can form a welding effect of overall low heat input and local high heat input, and ensure the stability of the full-position welding of the subsea pipeline, thereby achieving stable welding of the subsea pipeline under the condition of the shaking of the pipe-laying ship, and improving the fatigue resistance and corrosion resistance of the subsea pipeline;

[0015] 2. In particular, the present application ensures that the root excess height is less than or equal to 0.5 mm during the welding process, which can reduce the stress concentration at the root of the joint and optimize the fatigue performance of the joint;

[0016] 3. In addition, the present application adopts a multi-layer single-pass welding process with a narrow gap U-shaped groove to replace the multi-layer multi-pass welding process with a V-shaped groove in conventional technology, and makes use of the compression and attraction of the side walls on both sides of the groove on the arc and the restraining effect on the flow range of the molten pool metal to avoid the turbulence of the molten pool metal under the condition of hull shaking, which causes unfused defects on the side walls, between passes and between layers. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 It is the arc shape in Example 1 of the present invention;

[0018] Figure 2 is a schematic diagram of the groove design in embodiments 1 to 5 of the present invention;

[0019] Figure 3 This is the macroscopic morphology of the joint in Example 1 of the present invention;

[0020] Figure 4 1 is the microstructure of the joint in Example 1 of the present invention, wherein (a) is the coarse grain area (CG) diagram of the heat affected zone at the 0-point position, (b) is the CG diagram at the 3-point position, (c) is the CG diagram at the 6-point position, (d) is the weld (WM) diagram at the 0-point position, (e) is the WM diagram at the 3-point position, and (f) is the WM diagram at the 6-point position;

[0021] Figure 5 is the microhardness distribution of the joint in Example 1 of the present invention;

[0022] Figure 6 is the SN curve of the joint fatigue test in Example 1 of the present invention;

[0023] Figure 7 is the surface morphology of the joint after SSC test in Example 1 of the present invention;

[0024] Figure 8 1 is the side morphology of the joint after SSC test in Example 1 of the present invention, wherein (a) is the 0 o'clock position, (b) is the 3 o'clock position, and (c) is the 6 o'clock position;

[0025] Fig. 9 This is the arc shape in Comparative Examples 1 and 2 of the present invention;

[0026] Fig.10 This is the macroscopic morphology of the joint in Comparative Example 1 of the present invention;

[0027] Fig.11 It is the microstructure of the joint in Comparative Example 1 of the present invention, wherein (a) is the coarse and fine zone (CG) diagram of the heat affected zone at the 0-point position, (b) is the CG diagram at the 3-point position, (c) is the CG diagram at the 6-point position, (d) is the weld (WM) diagram at the 0-point position, (e) is the WM diagram at the 3-point position, and (f) is the WM diagram at the 6-point position;

[0028] Fig.12 It is the microhardness distribution of the joint in Comparative Example 1 of the present invention;

[0029] Fig.13 It is the crack propagation of the welded joint at the 0 point position after the SSC test of the joint in Comparative Example 1 of the present invention, wherein (a) is the crack morphology near the coarse grain zone of the heat affected zone, (b) is an enlarged view of the crack morphology in (a), and (c) and (d) are enlarged views of the circled part in (b);

[0030] Fig.143. The crack propagation of the welded joint at three positions after the SSC test of the joint in Comparative Example 1 of the present invention, wherein (a) is the crack morphology near the coarse grain zone of the heat affected zone, (b) is an enlarged view of the crack morphology in (a), (c) is an enlarged view of the red frame part in (b), (d) is an enlarged view of the yellow frame part in (b), and (e) is an enlarged view of the blue frame part in (b);

[0031] Fig.15 It is the crack propagation of the welded joint at 6 points after the SSC test of the joint in Comparative Example 1 of the present invention, wherein (a) is the crack morphology near the coarse grain zone of the heat affected zone, (b) is an enlarged view of the red frame part in (a), (c) is an enlarged view of the yellow frame part in (a), and (d) is an enlarged view of the blue frame part in (a);

[0032] Fig.16 It is a surface morphology image of the joint after SSC test in Comparative Example 2 of the present invention. DETAILED DESCRIPTION

[0033] In order to make the purpose, technical solution and advantages of the present application more clearly understood, the present application is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.

[0034] According to one aspect of the present application, a high-efficiency and high-comprehensive-performance welding method for submarine pipes under shaking of a pipe-laying vessel is provided. Specifically, the submarine pipe is subjected to ultra-short arc GMAW full-position welding within a heat input range of 0.2 kJ / mm to 0.3 kJ / mm, and at the same time, the peak current in the GMAW waveform is set to 285A to 370A, the peak current drop rate is set to 50A / ms to 70A / ms, and the necking time is set to 3ms to 7ms, thereby forming an overall low heat input and local high heat input welding effect, thereby ensuring the stability of the submarine pipe in all positions under shaking conditions, and achieving SSC (hydrogen sulfide stress corrosion cracking) performance improvement.

[0035] The heat input in conventional GMAW welding is usually in the range of 0.8kJ / mm to 1.5kJ / mm. In the GMAW waveform, the peak current is 250A to 300A, the peak current drop rate is 250A / ms to 300A / ms, and the necking time is 1.5ms to 2.5ms. Considering that the conventional GMAW process has excessive heat input, its root forming (excessive root excess height and too small transition radius) is one of the key factors leading to stress concentration and fatigue failure. In order to improve the fatigue resistance of the submarine pipeline, the present application improves the root forming by reducing the heat input. However, under low heat input conditions, the electromagnetic force and arc pressure generated by arc welding in all positions, especially at the overhead welding position, are insufficient to ensure the stability of the welding process. The influence of the gravity of the molten pool metal causes the magnetic field on the side walls on both sides of the groove to be uneven, resulting in arc deflection. At the same time, under this condition, due to the rapid cooling of the molten pool metal, a martensitic structure is formed, and the sulfur-induced stress corrosion cracking performance of the joint is insufficient. Therefore, the present application adopts two methods of improving the GMAW waveform and ultra-short arc technology under low heat input. One is to increase the arc pressure by increasing the peak current, and to avoid the current mutation caused by the wire withdrawal by reducing the peak current drop rate, and to extend the necking time to increase the duration of the arc force on the molten droplet. The second is to use ultra-short arc technology to generate a greater electromagnetic force to overcome the influence of the anti-gravity of the molten droplet.

[0036] Specifically, the GMAW waveform is adjusted under low heat input conditions to increase the peak current, reduce the peak current drop rate and extend the necking time; the increase in peak current can significantly increase the arc pressure, offset part of the gravity of the molten pool metal, and allow more molten pool liquid metal to be discharged to the rear of the molten pool, thereby extending the time the molten drop exists on the welding wire; the reduction in the peak current drop rate can effectively avoid the current mutation caused by the wire withdrawal; the extension of the necking time increases the duration of the arc force on the molten drop, and the time required for the molten drop to fall off is longer. The continuous electromagnetic force can offset part of the gravity on the molten pool. The combination of the above factors ensures the stability of all-position welding of the sea pipe. In addition, the increase in peak current increases the average current and heat input, which is beneficial to reduce the joint hardness and improve the SSC performance of the joint. At the same time, in combination with the ultra-short arc technology, on the one hand, it can generate a greater electromagnetic force than conventional GMAW technology to overcome the influence of the anti-gravity of the molten droplet, promote the short-circuit transition of the molten droplet, and combine with the waveform adjustment to jointly ensure the stability of the full-position welding process of the submarine pipeline; on the other hand, it can reduce the effect of the arc on the side wall, prompting the arc heat to be locally compressed in the molten pool area, forming an overall low heat input and local high heat input effect, combined with the increase in peak current, the reduction in the peak current drop rate and the extension of the necking time, to jointly improve the stability of the molten droplet transition under the shaking of the pipe-laying ship hull, avoid the generation of unfused defects under low heat input, and achieve the maximum Vickers hardness of the joint ≤248HV10 and the corrosion SSC test to meet the NACE0177 standard.

[0037] Furthermore, during the welding process, the root excess height is ensured to be less than or equal to 0.5 mm to reduce stress concentration at the root of the joint, ensure that the fatigue performance of the joint can meet the service requirements of the subsea pipeline under alternating loads, and avoid fatigue damage.

[0038] Furthermore, for the all-position welding process of the sea pipe, the pipe-laying vessel shakes due to frequent sea waves. If the conventional multi-layer multi-pass GMAW welding process based on the V-shaped groove is used, the molten pool metal will have obvious turbulence under the condition of hull shaking. On the one hand, the molten pool metal cannot achieve good fusion with the side wall. On the other hand, after flowing to the next weld area, it affects the welding quality of the next weld and the next layer, and easily induces the side wall, inter-pass and inter-layer unfused defects. Therefore, it is preferred to use the multi-layer single-pass welding process based on the narrow gap U-shaped groove for welding. Due to the compression and attraction of the side walls on both sides of the groove on the arc and the constraint on the flow range of the molten pool metal, the molten pool metal can still be maintained in the center of the groove under the condition of hull shaking, avoiding the turbulence of the molten pool metal under the condition of hull shaking, which causes the unfused defects of the side wall, inter-pass and inter-layer. At the same time, the parameters of the narrow gap U-shaped groove are preferably: blunt edge thickness 1.0mm~1.6mm, arc transition radius 2.4mm~3.2mm, single-side groove angle 2.5°~3.5°, under which multi-layer single-pass welding can be achieved.

[0039] Furthermore, when the ultra-short arc GMAW technology is used to weld the sea pipe, the welding current is 160A to 200A, the welding voltage is 12V to 15V, and the welding speed is 450mm / min to 700mm / min.

[0040] Furthermore, the arc length of the ultra-short arc is 1.5 mm to 2.5 mm. At this arc length, a greater electromagnetic force can be generated to overcome the influence of the anti-gravity of the molten droplet, promote the short-circuit transition of the molten droplet, and promote the local compression of the arc heat in the molten pool area, thereby improving the arc stability.

[0041] Furthermore, the present application can use robots to achieve fully automatic welding of the 5G position of the subsea pipeline, and can also use a rail trolley to achieve fully automatic welding of the subsea pipeline.

[0042] According to another aspect of the present application, a sea pipe welded joint prepared by the above welding method is provided, and the sea pipe fatigue performance of the sea pipe welded joint is better than the BS7608D and E grade acceptance curves, the fatigue strength is about 40% higher than the BS7608E curve, the maximum Vickers hardness of the joint is ≤248HV10, and the corrosion SSC test meets the NACE0177 standard. Therefore, the sea pipe prepared by the welding method provided by the present application can meet the service requirements under alternating loads.

[0043] The technical solution provided in this application is further described below based on specific embodiments.

[0044] Example 1

[0045] The material to be welded in this embodiment is a 12-inch API 5L X65 riser, and the narrow gap U-shaped groove is as follows: Figure 2 As shown in the figure, the backing welding process parameters are welding current 185A, welding voltage 13.5V, welding speed 500mm / min, heat input 0.24kJ / mm. The peak current in the GMAW waveform is 360A, the peak current drop rate is 60A / ms, the necking time is 4.8ms, and the arc length is 2mm.

[0046] The welding process is stable, the molten metal pool is located in the center of the groove, and the arc is not deflected. Figure 1 As shown; no unfused defects were found in the macroscopic morphology of the joint, such as Figure 3 As shown in the figure, in terms of microstructure, the structure of the coarse-grained heat-affected zone at the 0-point position is mainly composed of lath bainite, ferrite and chain MA components, and the structure of the coarse-grained zone at the 3-point and 6-point positions is mainly composed of granular bainite, ferrite and chain MA components. There is no brittle hard structure such as martensite at each position. Figure 4 As shown; the maximum hardness value is less than 235HV10, all appear in the heat affected zone, such as Figure 5 As shown; the SN curve with a 95% confidence interval shows that no fatigue failure occurs after reaching the runout value at medium and low stress levels. At a high stress level of 172MPa, fatigue fracture failure occurs, and the fatigue performance is better than the BS7608D and E grade acceptance curves, and the fatigue strength is 38% higher than the BS7608E curve. Figure 6 As shown in the figure, after 720 hours of testing, the tensile surface of the SSC sample was inspected under a low-power microscope with a magnification of ×10. There was no crack or fissure on the tensile surface. Figure 7 As shown, it shows that the sample is not sensitive to sulfur-induced stress corrosion cracking or stress-induced hydrogen cracking under the above test conditions, and meets the DNV-OS-F101 standard; after the sample is cut and the root section is observed, no microcracks are found, such as Figure 8 shown.

[0047] Example 2

[0048] In this embodiment, the material to be welded is a 12-inch API 5L X65 riser, and a narrow gap U-shaped groove is used. The bottom welding process parameters are welding current 160A, welding voltage 15V, welding speed 450mm / min, and heat input 0.26kJ / mm. The peak current in the GMAW waveform is 285A, the peak current drop rate is 65A / ms, the necking time is 6ms, and the arc length is 1.5mm.

[0049] Example 3

[0050] In this embodiment, the material to be welded is a 12-inch API 5L X65 riser, and a narrow gap U-shaped groove is used. The bottom welding process parameters are welding current 170A, welding voltage 12V, welding speed 500mm / min, and heat input 0.23kJ / mm. The peak current in the GMAW waveform is 300A, the peak current drop rate is 50A / ms, the necking time is 3ms, and the arc length is 2.5mm.

[0051] Example 4

[0052] In this embodiment, the material to be welded is a 12-inch API 5L X65 riser, and a narrow gap U-shaped groove is used. The bottom welding process parameters are welding current 200A, welding voltage 15V, welding speed 700mm / min, and heat input 0.21kJ / mm. The peak current in the GMAW waveform is 370A, the peak current drop rate is 70A / ms, the necking time is 5ms, and the arc length is 1.8mm.

[0053] Example 5

[0054] In this embodiment, the material to be welded is a 12-inch API 5L X65 riser, and a narrow gap U-shaped groove is used. The bottom welding process parameters are welding current 190A, welding voltage 13V, welding speed 600mm / min, and heat input 0.20kJ / mm. The peak current in the GMAW waveform is 320A, the peak current drop rate is 55A / ms, the necking time is 7ms, and the arc length is 2.2mm.

[0055] Comparative Example 1

[0056] Comparative Example 1 is the same as Example 1, except that the arc length is 4 mm. During welding, the arc is attracted by the side wall and deflected. Fig. 9 As shown; obvious unfused defects were found in the macroscopic morphology of the joint, such as Fig.10 As shown in the figure, in terms of microstructure, the structure of the coarse-grained heat-affected zone at the 0-point position is mainly composed of granular bainite and coarse chain MA components; the structure of the coarse-grained zone at the 3-point position is mainly composed of martensite and chain MA components; the structure of the coarse-grained zone at the 6-point position is mainly composed of granular bainite, lath bainite and martensite, as shown in the figure. Fig.11 As shown; due to the formation of martensite, the maximum hardness of the joint reaches 260HV10, which appears in the heat affected zone, such as Fig.12 As shown;

[0057] After 720 hours of testing, the tensile surface of the SSC specimen was inspected under a low-power microscope with a magnification of ×10, and microcracks were found on the stress side of the weld root. After the specimen was cut and the root section was observed, the cracks in the weld joint at the 0 point position mainly initiated in the coarse-grained martensite and extended along the martensite and bainite. When the cracks extended to the needle-shaped body of the weld or the extension direction was perpendicular to the direction of the lath bainite, the cracks stopped extending. Fig.13 As shown in the figure, the cracks in the welded joint at the 3 and 6 o'clock positions mainly initiate in the coarse-grained martensite and extend along the martensite or bainite. The crack at the 3 o'clock position extends to the point perpendicular to the lath bainite and stops extending (as shown in the figure). Fig.14 As shown in Figure 1), the crack at the 6-point position propagates to the weld and then stops propagating due to the inhibition of acicular ferrite (as shown in Figure 1). Fig.15 shown).

[0058] Comparative Example 2

[0059] Comparative Example 2 is the same as Comparative Example 1, except that the peak current in the waveform is 260A, the peak current drop rate is 280A / ms, and the necking time is 2ms. Fig. 9 ), the maximum hardness of the joint is higher than that of comparative example 1, reaching 285HV10. After 720 hours of testing, the tensile surface of the SSC sample was inspected under a low-power microscope with a magnification of ×10, and obvious cracks were found on the stress side of the weld root (such as Fig.16 shown).

[0060] It will be easily understood by those skilled in the art that the above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present application shall be included in the scope of protection of the present application.

Claims

1. A high-efficiency and high-comprehensive-performance welding method for sea pipes under shaking of pipe-laying vessels, characterized in that: The welding method comprises: performing ultra-short arc GMAW full-position welding on the subsea pipe within a heat input range of 0.2 kJ / mm to 0.3 kJ / mm, wherein the arc length of the ultra-short arc is 1.5 mm to 2.5 mm, and the peak current in the GMAW waveform is set to 285A to 370A, the peak current drop rate is set to 50A / ms to 70A / ms, and the necking time is set to 3ms to 7ms. At the same time, a multi-layer single-pass welding process with a narrow gap U-shaped groove is adopted for welding, and during the welding process, the root excess height is ensured to be less than or equal to 0.5 mm, so as to form a welding effect of overall low heat input and local high heat input, thereby ensuring the stability of the subsea pipe full-position welding under shaking conditions.

2. The high-efficiency and high-comprehensive-performance welding method for sea pipes under shaking of a pipe-laying vessel as claimed in claim 1 is characterized in that: The parameters of the narrow gap U-shaped groove are: blunt edge thickness 1.0 mm to 1.6 mm, arc transition radius 2.4 mm to 3.2 mm, and single-side groove angle 2.5° to 3.5°.

3. The high-efficiency and high-comprehensive-performance welding method for sea pipes under shaking of a pipe-laying vessel as claimed in claim 1 is characterized in that: When using ultra-short arc GMAW technology to weld subsea pipes, the welding current is 160A~200A, the welding voltage is 12V~15V, and the welding speed is 450mm / min~700mm / min.

4. A sea pipe welded joint prepared by the welding method according to any one of claims 1 to 3.