A low-temperature heat-sealed single polyethylene composite packaging film and preparation method thereof
Through the preparation of low-temperature heat-sealing single polyethylene material composite packaging film, the problem of difficulty in recycling multi-material composite packaging is solved, and a high-performance and sustainable packaging film is achieved, with excellent comprehensive performance and hygienic safety.
Patent Information
- Application Number
- CN202410772627.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-17
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-06-17
AI Technical Summary
Existing multi-material composite packaging has difficulties in recycling, which affects the sustainable development of plastic packaging.
Using a low-temperature heat-sealing single polyethylene material composite packaging film preparation method, through the combination of different levels of polyethylene materials and fillers, the antibacterial, antioxidant, and mechanical properties are improved, and the hydrophobic and antifouling properties are enhanced through modified calcium sulfate whiskers. , forming a three-layer structure packaging film.
It achieves low-temperature heat sealing, improves the overall performance of the packaging film, enhances the sustainability and hygienic safety of recycling, avoids the middle printing layer from contacting food, and improves the overall performance of the packaging film.
Smart Images

Figure CN118342829B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of packaging films, and in particular to a low-temperature heat-sealed single polyethylene composite packaging film and a preparation method thereof. Background Art
[0002] At present, most plastic flexible packaging is made of films of different materials that are tightly bonded (compounded) with glue. For example, one of the composite packaging structures of rice is BOPA film / adhesive / PE film. The demand and output of packaging materials are increasing, but it is not easy to classify and recycle multi-material composite packaging after it is discarded after the packaging life cycle. Therefore, single-material design that is conducive to recycling has become an important trend in the sustainable development of the plastic packaging field, which can better achieve the sustainable development of packaging materials. Summary of the invention
[0003] In order to solve the above technical problems, the present invention provides a method for preparing a low-temperature heat-sealable single polyethylene composite packaging film, comprising the following steps:
[0004] Step (1), mixing linear low density polyethylene, metallocene linear low density polyethylene, an anti-blocking agent, tea polyphenols, and nano zinc oxide, and extruding to obtain melt A; mixing medium density polyethylene, linear low density polyethylene, metallocene linear low density polyethylene, paraffin, and cellulose nanocrystals, and extruding to obtain melt B; taking metallocene linear low density polyethylene as a raw material, and extruding to obtain melt C; casting melt A, melt B, and melt C to prepare a second PE film having a three-layer structure of layer A, layer B, and layer C; in the above process, the second PE film is used as a low-temperature heat sealing layer, wherein the melting point of the linear low density polyethylene is The melting point of metallocene linear low-density polyethylene is 98°C, the melting point of low-density polyethylene is 110°C, the melting point of low-density polyethylene is 111°C, and the melting point of medium-density polyethylene is 126°C; among them, layer A is used as the innermost layer of the composite packaging film, and has the lowest heat-sealing temperature. The addition of tea polyphenols and nano zinc oxide contained in it improves the antibacterial property, UV barrier property, and mechanical property of layer A; the addition of cellulose nanocrystals in layer B enhances its mechanical property and barrier property, and the addition of paraffin can further reduce the heat-sealing temperature of layer B; layer C uses metallocene linear low-density polyethylene as raw material, which can reduce the heat-sealing temperature while improving the impact strength;
[0005] Step (2), mixing medium density polyethylene and metallocene linear low density polyethylene, extruding to obtain melt E; mixing low density polyethylene and low molecular weight polylimonene, extruding to obtain melt F; mixing modified high density polyethylene and shikonin, extruding to obtain melt G; casting melt E, melt F, and melt G to produce a first PE film having a three-layer structure of E layer, F layer, and G layer; in the above process, the E layer is made of medium density polyethylene and metallocene linear low density polyethylene as raw materials, and has better weldability (i.e., it is not easy to generate cracks, pores, etc. at the heat sealing part during the heat sealing process, and has higher mechanical properties), resistance to environmental stress cracking, high strength, and high toughness; the low molecular weight polylimonene in the F layer is non-volatile, and has higher thermal stability and antioxidant capacity than the monomer, so that the F layer has high antioxidant and UV barrier properties; the G layer is the outermost layer of the composite packaging film, and is made of modified high density polyethylene. Polyethylene is used as the main raw material, and nano-silica is grafted onto the side chain of high-density polyethylene in the form of chemical bonds to improve the dispersibility and compatibility of nano-silica, so that the G layer has better mechanical properties, barrier properties and good hydrophobic antifouling properties. Furthermore, the addition of shikonin containing many quinone groups not only has a significant impact on the improvement of the hydrophobic effect of the G layer, but also helps to improve the antibacterial performance; wherein, the preparation method of the modified high-density polyethylene comprises the following steps: step S1, modifying nano-silica by (3-mercaptopropyl) trimethoxysilane to obtain surface-modified nano-silica; step S2, grafting and modifying high-density polyethylene by glycidyl methacrylate to obtain surface-grafted high-density polyethylene; step S3, reacting the surface-modified nano-silica with the surface-grafted high-density polyethylene to obtain modified high-density polyethylene;
[0006] Step (3), mixing high-density polyethylene and modified calcium sulfate whiskers, extruding and then processing into a film, printing, and obtaining an intermediate printed layer; in the above process, the calcium sulfate whiskers are fibrous, can exert excellent barrier effect, and have the characteristics of high stiffness, high strength, excellent heat resistance and low cost, and the calcium sulfate whiskers are activated and modified to improve their compatibility in the high-density polyethylene matrix;
[0007] Step (4), placing the first PE film, the middle printing layer, and the second PE film in order from top to bottom, and connecting them by hot pressing and bonding to obtain a low-temperature heat-sealable single polyethylene material composite packaging film.
[0008] Preferably, in step (1), the contents of the components in the melt A are, by weight, 15-30 parts of linear low-density polyethylene, 35-68 parts of metallocene linear low-density polyethylene, 2-4 parts of anti-blocking agent, 0.7-2 parts of tea polyphenols, and 3-5 parts of nano zinc oxide; the contents of the components in the melt B are, by weight, 20-30 parts of medium-density polyethylene, 35-45 parts of linear low-density polyethylene, 50-65 parts of metallocene linear low-density polyethylene, 12-18 parts of paraffin, and 8-16 parts of cellulose nanocrystals; and the mass ratio of the metallocene linear low-density polyethylene in the melt C to the metallocene linear low-density polyethylene in the melt B is (100-150):(50-65).
[0009] Preferably, in step (1), the extrusion conditions of melt A and melt B are: temperature of 190-235°C and rotation speed of 40-60rpm; the extrusion conditions of melt C are: temperature of 190-235°C and rotation speed of 10-20rpm.
[0010] Preferably, in step (2), the contents of the components in the melt E are, by weight, 40-60 parts of medium-density polyethylene and 60-80 parts of metallocene linear low-density polyethylene; the contents of the components in the melt F are, by weight, 100-150 parts of low-density polyethylene and 0.5-3 parts of low-molecular-weight polylimonene; the contents of the components in the melt G are, by weight, 100-150 parts of modified high-density polyethylene and 2-8 parts of shikonin.
[0011] Preferably, in step (2), the extrusion conditions of melt E and melt G are: temperature of 190-235°C and rotation speed of 10-20 rpm; the extrusion conditions of melt F are: temperature of 130-150°C and rotation speed of 10-20 rpm.
[0012] Preferably, in step (3), the contents of the components in the intermediate printing layer are, by weight, 100-150 parts of high-density polyethylene and 6-10 parts of modified calcium sulfate whiskers; and the extrusion conditions are: temperature of 190-235° C. and rotation speed of 40-60 rpm.
[0013] Preferably, in step (3), the preparation method of the modified calcium sulfate whisker is as follows: mixing the calcium sulfate whisker with a 30wt% aqueous hydrogen peroxide solution, heating to 70-90°C for reaction for 5.5-6.5h, filtering, washing, and vacuum drying at 60-80°C to obtain activated calcium sulfate whisker; wherein the amount ratio of the calcium sulfate whisker to the aqueous hydrogen peroxide solution is (20-30) g: (100-200) mL; adding the activated calcium sulfate whisker and glycidyl methacrylate to N,N-dimethyl The method comprises the following steps: ultrasonically treating the mixture in formamide for 50-80 minutes, heating the mixture under stirring in a nitrogen atmosphere, adding acetic acid when the temperature rises to 90-110°C, and reacting the mixture for 9-11 hours. After the reaction is completed, the mixture is filtered, washed, and dried to obtain modified calcium sulfate whiskers. The ratio of activated calcium sulfate whiskers, 3.5-7 g of glycidyl methacrylate, N,N-dimethylformamide, and acetic acid is (10-15) g: (3.5-7) g: (60-150) mL: (2-4) mL.
[0014] Preferably, in step (2), the preparation method of the low molecular weight polylimonene is as follows: limonene, 2,2,2-tribromoethanol, thioxanthene-9-one, pentamethyldiethylenetriamine and N,N-dimethylacetamide are mixed in a molar ratio of 100: (1.5-2): (1.5-2): (8-9): (170-180), and the mixture is irradiated with ultraviolet light for 10-20 minutes in a nitrogen atmosphere, and then heated to 38-42°C under light for reaction for 5.5-6.5 hours. After the reaction is completed, the reaction mixture is evaporated at 42-48°C for 45-50 hours, and finally precipitated with ethanol and filtered to obtain the low molecular weight polylimonene.
[0015] Preferably, in step (2), the preparation method of the modified high-density polyethylene is:
[0016] Step S1, adding nano-silica to ethanol, and ultrasonically treating at 25-35°C for 40-80 minutes to obtain a nano-silica suspension; wherein the mass ratio of nano-silica to ethanol is (0.5-1.5): (70-300); (3-mercaptopropyl)trimethoxysilane, ethanol, acetic acid, and water are mixed in a volume ratio of (3.2-6.5): 0.05: 25: 0.1, and then dripped into the nano-silica suspension under stirring conditions within 20-40 minutes, continued stirring for 3.5-4.5 hours, centrifuged, and the centrifuged product was washed with acetone for 3-5 times, and dried to obtain surface-modified nano-silica; wherein the amount ratio between nano-silica and (3-mercaptopropyl)trimethoxysilane is 0.5g: (3-60)mL;
[0017] Step S2, adding high-density polyethylene particles to glycidyl methacrylate, and then adding dibenzoyl peroxide and toluene, reacting at 100-110° C. for 100-150 minutes, filtering, and ultrasonically cleaning the obtained filtered product with acetone for 20-40 minutes to obtain surface-grafted high-density polyethylene; wherein the mass ratio of high-density polyethylene particles, glycidyl methacrylate, dibenzoyl peroxide, and toluene is (2-4): (30-50): (0.1-0.15): (4-10);
[0018] Step S3, adding surface-modified nano-silica and surface-grafted high-density polyethylene to tetrahydrofuran, adding a sodium carbonate / sodium bicarbonate buffer solution with a concentration of 0.5 mol / L and a pH of 9.51 to adjust the pH of the mixed system to 8.4-8.6, heating to 35-45°C and stirring at a speed of 100-150 r / min for 7-9 hours, and removing the solvent by rotary evaporation to obtain modified high-density polyethylene; wherein the amount ratio of the surface-modified nano-silica, the surface-grafted high-density polyethylene, and tetrahydrofuran is (0.5-1.2) g: (10-15) g: (10-20) mL; in the above process, the nano-silica and (3 -mercaptopropyl)trimethoxysilane is reacted to introduce mercapto groups on the surface of nano-silica to obtain surface-modified nano-silica; high-density polyethylene is modified by glycidyl methacrylate, and the introduction of glycidyl methacrylate not only introduces epoxy groups into high-density polyethylene, but also improves the hydrophobicity of high-density polyethylene; surface-modified nano-silica and surface-grafted high-density polyethylene are connected to high-density polyethylene in the form of chemical bonds through the reaction between mercapto groups and epoxy groups, thereby improving the compatibility of silica and high-density polyethylene. The introduction of inorganic nano-silica improves the mechanical properties and barrier properties of high-density polyethylene.
[0019] The low-temperature heat-sealing single polyethylene composite packaging film is prepared by the method.
[0020] Compared with the prior art, the present invention has the following beneficial effects:
[0021] 1. The low-temperature heat-sealable single polyethylene composite packaging film of the present invention comprises a first PE film, an intermediate printing layer and a second PE film from top to bottom. The heat-seal temperature of the second PE film is lower than that of the first PE film. The intermediate printing layer is arranged between the first PE film and the second PE film to prevent the intermediate printing layer from contacting food, which is more hygienic and safe. In the present invention, polyethylene is used as the main material, which is recyclable and environmentally friendly.
[0022] 2. The first PE film and the second PE film in the low-temperature heat-sealable single polyethylene material composite packaging film of the present invention are both composed of three-layer co-extruded PE films, and each layer is endowed with more functions by adding or treating different fillers, and the printing layer of the present invention is also added with modified calcium sulfate whiskers to make it have better performance. Ultimately, the low-temperature heat-sealable single polyethylene material composite packaging film product of the present invention has excellent comprehensive performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 It is a schematic structural diagram of the low-temperature heat-sealable single polyethylene composite packaging film of the present invention; wherein, 1-A layer; 2-B layer; 3-C layer; 4-middle printing layer; 5-E layer; 6-F layer; 7-G layer. DETAILED DESCRIPTION
[0024] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0025] Example 1
[0026] The present embodiment discloses a method for preparing a modified calcium sulfate whisker, comprising the following steps: mixing 25 g of calcium sulfate whisker with 150 mL of a 30 wt% aqueous hydrogen peroxide solution, heating to 80° C. for reaction for 6 h, filtering, washing, and vacuum drying at 70° C. to obtain activated calcium sulfate whisker; adding 12.5 g of activated calcium sulfate whisker and 5.5 g of glycidyl methacrylate to 100 mL of N,N-dimethylformamide, ultrasonically treating for 60 min, heating under stirring in a nitrogen atmosphere, adding 3 mL of acetic acid when the temperature rises to 100° C., reacting for 10 h, filtering, washing, and drying after the reaction is completed to obtain modified calcium sulfate whisker.
[0027] Example 2
[0028] The present embodiment discloses a method for preparing low molecular weight polylimonene, comprising the following steps: mixing limonene, 2,2,2-tribromoethanol, thioxanthene-9-one, pentamethyldiethylenetriamine, and N,N-dimethylacetamide in a molar ratio of 100:1.8:1.8:8.5:175, irradiating with ultraviolet light for 15 minutes in a nitrogen atmosphere, and then heating to 40° C. under light for reaction for 6 hours. After the reaction is completed, evaporating the reaction mixture at 45° C. for 48 hours, and finally precipitating with ethanol and filtering to obtain low molecular weight polylimonene.
[0029] Example 3
[0030] This embodiment discloses a method for preparing a modified high-density polyethylene, comprising the following steps:
[0031] Step A1, adding 1g of nano-silica to 180g of ethanol, ultrasonically treating at 30°C for 60min to obtain a nano-silica suspension; mixing (3-mercaptopropyl)trimethoxysilane, ethanol, acetic acid, and water in a volume ratio of 4.8:0.05:25:0.1, and then dripping into the nano-silica suspension under stirring conditions within 30min, continuing stirring for 4h, centrifuging, washing the centrifuged product with acetone 4 times, and drying to obtain surface-modified nano-silica; wherein the amount ratio between nano-silica and (3-mercaptopropyl)trimethoxysilane is 0.5g:31mL;
[0032] Step A2, adding high-density polyethylene particles to glycidyl methacrylate, and then adding dibenzoyl peroxide and toluene, reacting at 105° C. for 120 minutes, filtering, and ultrasonically cleaning the obtained filtered product with acetone for 30 minutes to obtain surface-grafted high-density polyethylene; wherein the mass ratio of high-density polyethylene particles, glycidyl methacrylate, dibenzoyl peroxide, and toluene is 3:40:0.12:7;
[0033] Step A3, add 0.9g of surface modified nano-silica and 12.5g of surface grafted high-density polyethylene to 15mL of tetrahydrofuran, add 0.5mol / L sodium carbonate / sodium bicarbonate buffer solution with a pH of 9.51 to adjust the pH of the mixed system to 8.5, heat to 40°C and stir the reaction at a speed of 120r / min for 8h, and remove the solvent by rotary evaporation to obtain modified high-density polyethylene.
[0034] Example 4
[0035] This embodiment discloses a method for preparing a low-temperature heat-sealable single polyethylene composite packaging film, comprising the following steps:
[0036] Step (1), by weight, 15 parts of linear low density polyethylene, 35 parts of metallocene linear low density polyethylene, 2 parts of anti-blocking agent, 0.7 parts of tea polyphenols, and 3 parts of nano zinc oxide are mixed, and extruded at a temperature of 190° C. and a rotation speed of 60 rpm to obtain melt A; by weight, 20 parts of medium density polyethylene, 35 parts of linear low density polyethylene, 50 parts of metallocene linear low density polyethylene, 12 parts of paraffin, and 8 parts of cellulose nanocrystals are mixed, and extruded at a temperature of 190° C. and a rotation speed of 60 rpm to obtain melt B; by weight, 100 parts of metallocene linear low density polyethylene are taken as raw materials, and extruded at a temperature of 190° C. and a rotation speed of 20 rpm to obtain melt C; melt A, melt B, and melt C are pressurized and stabilized by a melt pump, and then cast by a distributor and a casting die to produce a second PE film having a three-layer structure of layer A, layer B, and layer C;
[0037] Step (2), by weight, 40 parts of medium-density polyethylene and 60 parts of metallocene linear low-density polyethylene are mixed, and the mixture is extruded at a temperature of 190° C. and a rotation speed of 20 rpm to obtain a melt E; by weight, 100 parts of low-density polyethylene and 0.5 parts of low-molecular-weight polylimonene are mixed, and the mixture is extruded at a temperature of 130° C. and a rotation speed of 20 rpm to obtain a melt F; by weight, 100 parts of modified high-density polyethylene and 2 parts of shikonin are mixed, and the mixture is extruded at a temperature of 190° C. and a rotation speed of 20 rpm to obtain a melt G; the melts E, F, and G are pressurized and stabilized by a melt pump, and then cast by a distributor and a casting die to produce a first PE film having a three-layer structure of an E layer, an F layer, and a G layer;
[0038] Step (3), taking 100 parts of high-density polyethylene and 6 parts of modified calcium sulfate whiskers by weight, extruding at a temperature of 190° C. and a rotation speed of 60 rpm, and then processing into a film, printing, to obtain an intermediate printing layer;
[0039] Step (4), placing the first PE film, the middle printing layer, and the second PE film in order from top to bottom, and connecting them by hot pressing and bonding to obtain a low-temperature heat-sealable single polyethylene material composite packaging film.
[0040] Example 5
[0041] This embodiment discloses a method for preparing a low-temperature heat-sealable single polyethylene composite packaging film, comprising the following steps:
[0042] Step (1), by weight, 30 parts of linear low density polyethylene, 68 parts of metallocene linear low density polyethylene, 4 parts of anti-blocking agent, 2 parts of tea polyphenols, and 5 parts of nano zinc oxide are mixed, and extruded at a temperature of 235° C. and a rotation speed of 40 rpm to obtain melt A; by weight, 30 parts of medium density polyethylene, 45 parts of linear low density polyethylene, 65 parts of metallocene linear low density polyethylene, 18 parts of paraffin wax, and 16 parts of cellulose nanocrystals are mixed, and extruded at a temperature of 235° C. and a rotation speed of 40 rpm to obtain melt B; by weight, 150 parts of metallocene linear low density polyethylene are taken as raw materials, and extruded at a temperature of 235° C. and a rotation speed of 10 rpm to obtain melt C; melt A, melt B, and melt C are pressurized and stabilized by a melt pump, and then cast by a distributor and a casting die to produce a second PE film having a three-layer structure of layer A, layer B, and layer C;
[0043] Step (2), by weight, 60 parts of medium-density polyethylene and 80 parts of metallocene linear low-density polyethylene are mixed, and the mixture is extruded at a temperature of 235° C. and a rotation speed of 10 rpm to obtain a melt E; by weight, 150 parts of low-density polyethylene and 3 parts of low-molecular-weight polylimonene are mixed, and the mixture is extruded at a temperature of 150° C. and a rotation speed of 10 rpm to obtain a melt F; by weight, 150 parts of modified high-density polyethylene and 8 parts of shikonin are mixed, and the mixture is extruded at a temperature of 235° C. and a rotation speed of 10 rpm to obtain a melt G; the melts E, F, and G are pressurized and stabilized by a melt pump, and then cast by a distributor and a casting die to produce a first PE film having a three-layer structure of an E layer, an F layer, and a G layer;
[0044] Step (3), taking 150 parts of high-density polyethylene and 10 parts of modified calcium sulfate whiskers by weight, extruding at a temperature of 235° C. and a rotation speed of 40 rpm, and then processing into a film, printing, to obtain an intermediate printing layer;
[0045] Step (4), placing the first PE film, the middle printing layer, and the second PE film in order from top to bottom, and connecting them by hot pressing and bonding to obtain a low-temperature heat-sealable single polyethylene material composite packaging film.
[0046] Example 6
[0047] This embodiment discloses a method for preparing a low-temperature heat-sealable single polyethylene composite packaging film, comprising the following steps:
[0048] Step (1), by weight, 22.5 parts of linear low-density polyethylene, 51.5 parts of metallocene linear low-density polyethylene, 3 parts of an anti-blocking agent, 1.4 parts of tea polyphenols, and 4 parts of nano zinc oxide are mixed, and extruded at a temperature of 212° C. and a rotation speed of 50 rpm to obtain melt A; by weight, 25 parts of medium-density polyethylene, 40 parts of linear low-density polyethylene, 52 parts of metallocene linear low-density polyethylene, 15 parts of paraffin, and 12 parts of cellulose nanocrystals are mixed, and extruded at a temperature of 212° C. and a rotation speed of 50 rpm to obtain melt B; by weight, 125 parts of metallocene linear low-density polyethylene are taken as raw materials, and extruded at a temperature of 212° C. and a rotation speed of 15 rpm to obtain melt C; melt A, melt B, and melt C are pressurized and stabilized by a melt pump, and then cast by a distributor and a casting die to produce a second PE film having a three-layer structure of layer A, layer B, and layer C;
[0049] Step (2), by weight, 50 parts of medium-density polyethylene and 70 parts of metallocene linear low-density polyethylene are mixed, and the mixture is extruded at a temperature of 212° C. and a rotation speed of 15 rpm to obtain a melt E; by weight, 125 parts of low-density polyethylene and 1.8 parts of low-molecular-weight polylimonene are mixed, and the mixture is extruded at a temperature of 140° C. and a rotation speed of 15 rpm to obtain a melt F; by weight, 125 parts of modified high-density polyethylene and 5 parts of shikonin are mixed, and the mixture is extruded at a temperature of 212° C. and a rotation speed of 15 rpm to obtain a melt G; the melts E, F, and G are pressurized and stabilized by a melt pump, and then cast by a distributor and a casting die to produce a first PE film having a three-layer structure of an E layer, an F layer, and a G layer;
[0050] Step (3), taking 125 parts of high-density polyethylene and 8 parts of modified calcium sulfate whiskers by weight, extruding at a temperature of 212° C. and a rotation speed of 50 rpm, and then processing into a film, printing, to obtain an intermediate printing layer;
[0051] Step (4), placing the first PE film, the middle printing layer, and the second PE film in order from top to bottom, and connecting them by hot pressing and bonding to obtain a low-temperature heat-sealable single polyethylene material composite packaging film.
[0052] The above Examples 4-6 use the modified calcium sulfate whiskers prepared in Example 1, the low molecular weight polylimonene prepared in Example 2, and the modified high density polyethylene prepared in Example 3.
[0053] Comparative Example 1
[0054] Comparative Example 1 Compared with Example 6, in the process of preparing the middle printing layer in Comparative Example 1, calcium sulfate whiskers were used instead of modified calcium sulfate whiskers, and other conditions remained unchanged.
[0055] Comparative Example 2
[0056] Comparative Example 2 Compared with Example 6, in the process of preparing the middle printing layer in Comparative Example 2, no modified calcium sulfate whisker was added, and other conditions remained unchanged.
[0057] Comparative Example 3
[0058] Compared with Example 6, in Comparative Example 3, tea polyphenols were not added during the preparation of melt A, and other conditions remained unchanged.
[0059] Comparative Example 4
[0060] Comparative Example 4 Compared with Example 6, in Comparative Example 4, no nano zinc oxide was added during the preparation of melt A, and other conditions remained unchanged.
[0061] Comparative Example 5
[0062] Comparative Example 5 Compared with Example 6, in Comparative Example 5, low molecular weight polylimonene was not added during the preparation of melt F, and other conditions remained unchanged.
[0063] Comparative Example 6
[0064] Comparative Example 6 Compared with Example 6, in Comparative Example 6, no shikonin was added during the preparation of melt G, and other conditions remained unchanged.
[0065] Comparative Example 7
[0066] Compared with Example 6, in Comparative Example 7, high-density polyethylene is used instead of modified high-density polyethylene during the preparation of melt G, and other conditions remain unchanged.
[0067] Experimental example
[0068] Performance tests were performed on the low-temperature heat-sealable single polyethylene composite packaging film samples of Examples 4-6 and Comparative Examples 1-7.
[0069] 1. Tensile strength test: refer to GB / T 1040.3-2006.
[0070] 2. Oxygen barrier performance test: refer to GB / T 1038-2000.
[0071] 3. Hydrophobic performance test: The water contact angle of the G layer was tested by the static contact angle method.
[0072] 4. Antibacterial performance test: The plate colony counting method was used to quantitatively determine the antibacterial properties against Staphylococcus aureus and Escherichia coli.
[0073] 5. UV blocking performance test: 2,2-diphenyl-1-trinitrohydrazine (DPPH) was used to evaluate the antioxidant activity of the samples by colorimetry, and the DPPH scavenging rate was calculated.
[0074] The test results are shown in Table 1:
[0075]
[0076] It can be seen from the test results in Table 1 that the low-temperature heat-sealable single polyethylene composite packaging films prepared in Examples 4-6 of the present invention have excellent comprehensive properties. From the comparison between comparative examples 1 and 2 and example 6, it can be seen that the addition of calcium sulfate whiskers helps to improve the barrier properties and mechanical properties of the packaging film, and the modification of the calcium sulfate whiskers makes it play a better role; from the comparison between comparative example 3 and example 6, it can be seen that the addition of tea polyphenols has a significant effect on the antibacterial properties and ultraviolet barrier properties of the packaging film; from the comparison between comparative example 4 and example 6, it can be seen that the addition of inorganic nano zinc oxide improves the antibacterial properties, ultraviolet barrier properties and mechanical properties of the packaging film; from the comparison between comparative example 5 and example 6, it can be seen that the addition of low molecular weight polylimonene has a significant effect on the ultraviolet barrier properties of the packaging film; from the comparison between comparative example 6 and example 6, it can be seen that the addition of shikonin has a positive effect on the antibacterial properties, hydrophobicity and mechanical properties of the packaging film; from the comparison between comparative example 7 and example 6, it can be seen that the modification of the high-density polyethylene in the G layer can improve the barrier properties, hydrophobicity and mechanical properties of the packaging film.
[0077] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for preparing a low-temperature heat-sealed single polyethylene composite packaging film, It is characterized in that The following steps are involved: Step (1), mixing linear low density polyethylene, metallocene linear low density polyethylene, an anti-blocking agent, tea polyphenols, and nano zinc oxide, and extruding to obtain melt A; mixing medium density polyethylene, linear low density polyethylene, metallocene linear low density polyethylene, paraffin, and cellulose nanocrystals, and extruding to obtain melt B; taking metallocene linear low density polyethylene as a raw material, and extruding to obtain melt C; and casting melt A, melt B, and melt C to produce a second PE film; Step (2), mixing medium-density polyethylene and metallocene linear low-density polyethylene, and extruding to obtain melt E; mixing low-density polyethylene and low-molecular-weight polylimonene, and extruding to obtain melt F; mixing modified high-density polyethylene and shikonin, and extruding to obtain melt G; and casting melt E, melt F, and melt G to produce a first PE film; wherein the preparation method of the modified high-density polyethylene comprises the following steps: step S1, modifying nano-silica by (3-mercaptopropyl)trimethoxysilane to obtain surface-modified nano-silica; step S2, grafting high-density polyethylene by glycidyl methacrylate to obtain surface-grafted high-density polyethylene; step S3, reacting surface-modified nano-silica with surface-grafted high-density polyethylene to obtain modified high-density polyethylene; Step (3), mixing high-density polyethylene and modified calcium sulfate whiskers, extruding and then processing into a film, printing, and obtaining an intermediate printed layer; Step (4), placing the first PE film, the middle printing layer, and the second PE film in order from top to bottom, and connecting them by hot pressing and bonding to obtain a low-temperature heat-sealed single polyethylene composite packaging film; In the step (1), the contents of the components in the melt A are, by weight, 15-30 parts of linear low-density polyethylene, 35-68 parts of metallocene linear low-density polyethylene, 2-4 parts of anti-blocking agent, 0.7-2 parts of tea polyphenols, and 3-5 parts of nano zinc oxide; the contents of the components in the melt B are, by weight, 20-30 parts of medium-density polyethylene, 35-45 parts of linear low-density polyethylene, 50-65 parts of metallocene linear low-density polyethylene, 12-18 parts of paraffin, and 8-16 parts of cellulose nanocrystals; the mass ratio of the metallocene linear low-density polyethylene in the melt C to the metallocene linear low-density polyethylene in the melt B is (100-150):(50-65); In the step (1), the extrusion conditions of the melt A and melt B are: temperature of 190-235°C, rotation speed of 40-60rpm; the extrusion conditions of the melt C are: temperature of 190-235°C, rotation speed of 10-20rpm; In the step (2), the contents of the components in the melt E are, by weight, 40-60 parts of medium-density polyethylene and 60-80 parts of metallocene linear low-density polyethylene; the contents of the components in the melt F are, by weight, 100-150 parts of low-density polyethylene and 0.5-3 parts of low-molecular-weight polylimonene; the contents of the components in the melt G are, by weight, 100-150 parts of modified high-density polyethylene and 2-8 parts of shikonin; In step (2), the extrusion conditions of melt E and melt G are: temperature of 190-235°C and rotation speed of 10-20rpm; the extrusion conditions of melt F are: temperature of 130-150°C and rotation speed of 10-20rpm; In the step (3), the contents of the components in the intermediate printing layer are as follows: 100-150 parts of high-density polyethylene and 6-10 parts of modified calcium sulfate whiskers; the extrusion conditions are as follows: the temperature is 190-235°C and the rotation speed is 40-60rpm; In the step (3), the preparation method of the modified calcium sulfate whisker is as follows: mixing the calcium sulfate whisker with a 30wt% aqueous hydrogen peroxide solution, heating to 70-90°C for reaction for 5.5-6.5h, filtering, washing, and vacuum drying at 60-80°C to obtain activated calcium sulfate whisker; wherein the amount ratio of the calcium sulfate whisker to the aqueous hydrogen peroxide solution is (20-30) g: (100-200) mL; adding the activated calcium sulfate whisker and glycidyl methacrylate to N,N-dimethylformamide The method comprises the following steps: ultrasonically treating the activated calcium sulfate whisker in dimethylformamide for 50-80 minutes, heating under stirring in a nitrogen atmosphere, adding acetic acid when the temperature rises to 90-110°C, reacting for 9-11 hours, filtering, washing and drying after the reaction to obtain modified calcium sulfate whiskers; wherein the amount ratio of activated calcium sulfate whiskers, glycidyl methacrylate, N,N-dimethylformamide and acetic acid is (10-15) g: (3.5-7) g: (60-150) mL: (2-4) mL; In the step (2), the preparation method of the low molecular weight polylimonene is as follows: limonene, 2,2,2-tribromoethanol, thioxanthene-9-one, pentamethyldiethylenetriamine, and N,N-dimethylacetamide are mixed in a molar ratio of 100: (1.5-2): (1.5-2): (8-9): (170-180), and the mixture is irradiated with ultraviolet light for 10-20 minutes in a nitrogen atmosphere, and then heated to 38-42° C. under light for reaction for 5.5-6.5 hours. After the reaction is completed, the reaction mixture is evaporated at 42-48° C. for 45-50 hours, and finally precipitated with ethanol and filtered to obtain the low molecular weight polylimonene; In the step (2), the preparation method of the modified high-density polyethylene is: Step S1, adding nano-silica to ethanol, and ultrasonically treating at 25-35°C for 40-80 minutes to obtain a nano-silica suspension; wherein the mass ratio of nano-silica to ethanol is (0.5-1.5): (70-300); (3-mercaptopropyl)trimethoxysilane, ethanol, acetic acid, and water are mixed in a volume ratio of (3.2-6.5): 0.05: 25: 0.1, and then dripped into the nano-silica suspension under stirring conditions within 20-40 minutes, continued stirring for 3.5-4.5 hours, centrifuged, and the centrifuged product was washed with acetone for 3-5 times, and dried to obtain surface-modified nano-silica; wherein the amount ratio between nano-silica and (3-mercaptopropyl)trimethoxysilane is 0.5g: (3-60)mL; Step S2, adding high-density polyethylene particles to glycidyl methacrylate, and then adding dibenzoyl peroxide and toluene, reacting at 100-110° C. for 100-150 minutes, filtering, and ultrasonically cleaning the obtained filtered product with acetone for 20-40 minutes to obtain surface-grafted high-density polyethylene; wherein the mass ratio of high-density polyethylene particles, glycidyl methacrylate, dibenzoyl peroxide, and toluene is (2-4): (30-50): (0.1-0.15): (4-10); Step S3, adding surface-modified nano-silica and surface-grafted high-density polyethylene to tetrahydrofuran, adding a sodium carbonate / sodium bicarbonate buffer solution with a concentration of 0.5 mol / L and a pH of 9.51 to adjust the pH of the mixed system to 8.4-8.6, heating to 35-45°C and stirring at a speed of 100-150 r / min for 7-9 hours, and removing the solvent by rotary evaporation to obtain modified high-density polyethylene; wherein the amount ratio of the surface-modified nano-silica, the surface-grafted high-density polyethylene, and the tetrahydrofuran is (0.5-1.2) g: (10-15) g: (10-20) mL.
2. A low-temperature heat-sealable single polyethylene composite packaging film prepared by the method according to claim 1.
Citation Information
Patent Citations
Method for surface modification of calcium sulfate whisker
CN109320771A
Casting polyethylene film, composite film thereof and preparation method of composite film
CN111267447A
All-polyethylene composite film and preparation method thereof
CN117584584A