A sulfide solid electrolyte and all-solid-state sodium ion battery
Through the liquid phase synthesis method and Mo-W dual element doping, the sodium ion conductivity and stability of the sulfide solid electrolyte are improved, solving the problems of poor stability and low conductivity of the existing sulfide electrolyte in the air, and achieving Higher electrochemical performance and applicability.
Patent Information
- Application Number
- CN202410804758.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-21
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2044-06-21
AI Technical Summary
Existing sulfide solid electrolytes have poor chemical stability and low conductivity in air, making it difficult to meet the practical application needs of sodium batteries.
The Na3-a-bWaMobSb1-a-bS4 sulfide solid electrolyte is prepared using a liquid phase synthesis method. The conductivity and stability are improved through Mo-W double element doping, combined with specific preparation conditions such as co-precipitation reaction, vacuum drying and heat treatment. , ensuring uniform distribution of doping elements.
It significantly improves the sodium ion conductivity and electrochemical stability of the sulfide solid electrolyte, enhances air stability, is suitable for industrial production, and meets the application needs of sodium batteries.
Smart Images

Figure CN118380643B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of sodium ion batteries, and in particular to a sulfide solid electrolyte and an all-solid-state sodium ion battery. Background Art
[0002] Due to the wide availability and low cost of sodium resources, various studies on sodium batteries are being accelerated. Among them, in order to overcome the safety and application limitations of NaS batteries, the use of solid composition materials and lower temperatures are necessary. For example, β-alumina and sodium ion superionic conductors (NASICON) are classic sodium ion conductive solid electrolytes with the advantages of high ionic conductivity, high sodium ion transmission rate, and high chemical stability, especially the high ionic conductivity at room temperature, which can reach more than 0.1 mS / cm, but it must be sintered at a temperature above 1000°C to reduce grain boundary resistance and improve conductivity, which is a necessary process for realizing all-solid-state batteries.
[0003] Similarly, sulfide-based solid electrolytes are a viable electrolyte. Unlike oxide-based electrolytes, sulfide-based materials can be easily densified by cold pressing at room temperature (the so-called "room temperature pressure sintering"). The continuous development of practical all-solid-state sodium batteries requires new sulfide-based solid electrolytes with high sodium ion conductivity. Based on the above characteristics, common Na3PS4, Na4SiS4, Na3PSe4 and Na3P 0.62 As 0.38 Highly conductive sulfide sodium ion solid electrolytes such as S4 have been widely studied. However, this type of sulfide-based solid electrolyte still has the following problems: 1) Conventional phosphorus-containing sulfide Na3PS4 materials have poor chemical stability in the air. They not only react with water in the environment, but also produce toxic H2S gas, which is mixed with oxygen in dry air, causing serious practical application obstacles; 2) Sulfide-based solid electrolytes are usually prepared by high-energy dry ball milling. The electrolyte materials prepared by this method have poor particle uniformity and serious particle aggregation, and often have low conductivity problems in practical applications.
[0004] In view of this, it is indeed necessary to provide a technical solution to the above problems. Summary of the invention
[0005] One of the purposes of the present invention is to provide a sulfide solid electrolyte to address the problems of poor chemical stability in air and low conductivity of the sulfide solid electrolyte currently used in sodium batteries in practical applications in view of the deficiencies in the prior art.
[0006] In order to achieve the above object, the present invention adopts the following technical solutions:
[0007] A sulfide solid electrolyte, made by liquid phase synthesis, with the chemical formula of Na 3-a-b W a Mo b Sb 1-a-b S4, 0<a<0.5, 0<b<0.5.
[0008] Preferably, 0.01≤a≤0.25, 0.01≤b≤0.25.
[0009] Preferably, 0.01<a≤0.2, 0.01<b≤0.2, and a≤b.
[0010] Preferably, 0.1≤a+b≤0.3, and 0≤ba≤0.1.
[0011] Preferably, the sodium ion conductivity is greater than or equal to 3.0 mS / cm at room temperature of 25°C.
[0012] Preferably, the preparation method of the liquid phase synthesis method is: mixing Na3SbS4 powder and sodium thiotungstate molybdate powder, preparing an aqueous solution and stirring to perform a coprecipitation reaction; then drying under vacuum conditions, and heat treating at 200-450°C in an inert atmosphere to obtain Na 3-a-b W a Mo b Sb 1-a-b S4 sulfide solid electrolyte.
[0013] Preferably, the coprecipitation reaction conditions are heating and stirring in a water bath at 60-80°C for 4-8 hours; vacuum drying temperature is 120-200°C, and the drying time is 8-15 hours; and the heat treatment time is 2-12 hours.
[0014] Preferably, the preparation method of Na3SbS4 powder is: add Na2S, Sb2S3 and sulfur powder to deionized water, heat and stir in a water bath at 60~80°C, filter to obtain a homogeneous precursor aqueous solution of Na3SbS4, then add alcohol for precipitation reaction to obtain Na3SbS4 hydrate, vacuum dry, and then heat treat at 200~350°C in an inert atmosphere to obtain Na3SbS4 powder.
[0015] Preferably, the preparation method of sodium thiotungstate molybdate powder is as follows: sodium alkali, thiotungstate salt, and thiomolybdate salt are mixed and added to deionized water, heated and stirred in a water bath at 60-80°C to obtain a precursor solution, vacuum dried, and then heat treated at 200-350°C in an inert atmosphere to obtain sodium thiotungstate molybdate powder, the chemical formula of which is Na2W x Mo yS4, 0<x≤1.0, 0<y≤1.0, and x+y=1.
[0016] The second object of the present invention is to provide a solid-state sodium battery, comprising a positive electrode sheet, a negative electrode sheet and a solid electrolyte membrane spaced between the positive electrode sheet and the negative electrode sheet, wherein the solid electrolyte membrane is a solid electrolyte membrane made of the above-mentioned sulfide solid electrolyte; the positive electrode sheet contains or does not contain the above-mentioned sulfide solid electrolyte; the negative electrode sheet contains or does not contain the above-mentioned sulfide solid electrolyte.
[0017] The beneficial effects of the present invention are as follows: the sulfide solid electrolyte provided by the present invention selects specific Mo and W elements, and dual-dopes Na3SbS4 through the Mo-W dual element. The inventors found that compared with doping with other elements, on the one hand, the Mo and W elements can effectively increase the number of vacancies of Na ions, which can effectively improve the ionic conductivity of Na3SbS4; on the other hand, through Mo-W dual element doping, the electrochemical stability of the electrolyte can be further improved, and at the same time, the air stability of the solid electrolyte is further improved, and the probability of its reaction with moisture in the air is reduced, which lays the foundation for the solid electrolyte to be widely used in industrial production. In addition, the inventors found through experiments that compared with the conventional solid-phase synthesis method, the Mo-W dual element needs to be prepared in conjunction with the liquid-phase synthesis method, which can ensure the uniformity of the distribution of the two doping elements, and prepare a solid electrolyte with uniform particle size and small agglomeration, which can effectively improve Na in practical applications. 3-a-b W a Mo b Sb 1-a-b Ionic conductivity of S4 sulfide solid electrolyte. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 This is a SEM image of the solid electrolyte of Example 3 of the present invention.
[0019] Figure 2 This is a SEM image of the solid electrolyte of Comparative Example 4 of the present invention.
[0020] Figure 3 1 and 2 are XRD diagrams of the solid electrolytes of Example 3 of the present invention and Comparative Examples 1 and 4.
[0021] Figure 4 1 and 2 are Raman graphs of the solid electrolytes of Example 3 and Comparative Example 1 of the present invention.
[0022] Figure 5 XRD pattern of the solid electrolyte of Comparative Example 1 of the present invention after being exposed to air for 6 hours.
[0023] Figure 6XRD pattern of the solid electrolyte of Example 3 of the present invention after being exposed to air for 6 hours. DETAILED DESCRIPTION
[0024] To make the technical solutions and advantages of the present invention more clear, the present invention and its beneficial effects will be described in further detail below in conjunction with specific implementation methods and accompanying drawings, but the implementation methods of the present invention are not limited thereto.
[0025] Generally speaking, the ionic conductivity of conventional sulfide solid electrolytes doped with some transition metal elements can be increased to 0.1 mS / cm or higher. However, even if the composition of each element is changed, the ionic conductivity of the experiments under the current optimal state can only be increased to 0.8mS / cm, or at most 3mS / cm. Although it has increased several times compared to 0.1 mS / cm, in the context of the current pursuit of applications such as fast charging, the ionic conductivity of 1mS / cm is still not enough to meet user needs.
[0026] Based on this, the inventors have conducted in-depth research and provided a sulfide solid electrolyte, which is prepared by liquid phase synthesis method and has the chemical formula of Na 3-a-b W a Mo b Sb 1-a-b S4, 0<a<0.5, 0<b<0.5.
[0027] After in-depth research, it was found that by using tungsten and molybdenum as dual doping elements and controlling the preparation method and the proportion of each other element, compared with sulfide solid electrolytes single-doped with molybdenum or single-doped with tungsten or doped with other elements, the sulfide solid electrolyte obtained by the present invention has a uniform distribution of doping elements, which can effectively increase the number of vacancies of Na ions and improve the ionic conductivity of the original Na3SbS4; at the same time, the electrochemical stability and air stability of the solid electrolyte are improved. In addition, the electrolyte synthesis method provided by the present invention is low-cost and more suitable for large-scale production, laying a foundation for the wide use of solid electrolytes in industrial production.
[0028] Among them, for the tungsten content, the value of a can be 0<a<0.01, 0.01≤a<0.05, 0.05≤a<0.1, 0.1≤a<0.15, 0.15≤a<0.2, 0.2≤a<0.25, 0.25≤a<0.35 or 0.35≤a<0.5.
[0029] For the molybdenum content, the value of b may be 0<b<0.01, 0.01≤b<0.05, 0.05≤b<0.1, 0.1≤b<0.15, 0.15≤b<0.2, 0.2≤b<0.25, 0.25≤b<0.35 or 0.35≤b<0.5.
[0030] Accordingly, according to the specific values of a and b, the content range of Na and Sb is adjusted so that the sulfide solid electrolyte of the present invention is Na 3-a-b W a Mo b Sb 1-a-b S4.
[0031] By controlling the values of a and b within the above range, excessive doping of a and b is avoided, which affects the content of Sb and Na, thereby affecting the structural stability of the sulfide solid electrolyte.
[0032] Preferably, for the tungsten content, a is preferably 0.01≤a≤0.25; for the molybdenum content, b is 0.01≤b≤0.25.
[0033] More preferably, for the tungsten content, a is 0.01<a≤0.2; for the molybdenum content, b is 0.01<b≤0.2, and a≤b. After multiple experiments, it was verified that when the tungsten doping amount was reduced to less than the molybdenum doping amount, the doping effect of the two elements on the improvement of ionic conductivity was more excellent. It is speculated that it may be affected by the two atomic structures. When the molybdenum content is relatively higher, the synergistic doping with tungsten can provide more vacancies for Na ions, thereby further improving the ionic conductivity of the solid electrolyte.
[0034] In addition, it was found that synchronously controlling the values of a and b to satisfy 0.1≤a+b≤0.3 and 0≤ba≤0.1 can further improve the ionic conductivity of the solid electrolyte, while also improving the oxidation resistance of the solid electrolyte, broadening the potential window, and achieving even better performance.
[0035] However, it should be noted that the inventors have found through research that the optimized elemental components of the present invention can be prepared in combination with the liquid phase synthesis method to ensure the uniformity of the distribution of each doping element, so as to prepare a solid electrolyte with uniform particle size and small agglomeration. Although the solid phase synthesis method is simpler to prepare powder mixing methods, the prepared particles often show poor particle size uniformity, and the distribution of doping elements in the particles is not uniform enough. Even if the solid phase synthesis method uses a small particle size and increases the mixing time, the obtained sulfide solid electrolyte is still limited in improving the ionic conductivity.
[0036] The sulfide solid electrolyte obtained by the present invention has a sodium ion conductivity greater than or equal to 3.0 mS / cm at room temperature of 25°C, and can particularly exhibit a sodium ion conductivity greater than 12 mS / cm after adjusting the composition of tungsten and molybdenum. Compared with existing sulfide solid electrolytes, the sodium ion conductivity is greatly improved, providing more application directions for the practical application of sodium batteries.
[0037] Specifically, the chemical formula of the sulfide solid electrolyte of the present invention includes but is not limited to Na 2.95 W 0.025 Mo 0.025 Sb 0.95 S4、Na 2.9 W 0.06 Mo 0.04 Sb 0.9 S4、Na 2.9 W 0.08 Mo 0.02 Sb 0.9 S4、Na 2.85 W 0.09 Mo 0.06 Sb 0.85 S4、Na 2.85 W 0.012 Mo 0.03 Sb 0.85 S4、Na 2.7 W 0.2 Mo 0.1 Sb 0.7 S4、Na 2.5 W 0.4 Mo 0.1 Sb 0.5 S4、Na 2.5 W 0.1 Mo 0.5 Sb 0.5 S4.
[0038] Specifically, the preparation method of the liquid phase synthesis method is: Na3SbS4 powder is mixed with sodium thiotungstate molybdate powder, and the mixture is prepared into an aqueous solution and stirred for coprecipitation reaction; then, after drying under vacuum conditions, the mixture is heat treated at 200-450°C in an inert atmosphere to obtain Na 3-a-b W a Mo b Sb 1-a-b S4 sulfide solid electrolyte.
[0039] The liquid phase synthesis method provided by the present invention adopts a multi-step liquid phase synthesis method for synthesis, wherein Na3SbS4 powder and sodium thiotungstate molybdate powder are used as precursors to first be made into an aqueous solution and then mixed and stirred for a coprecipitation reaction, thereby achieving uniform mixing of the doping elements at the atomic level, thereby ensuring the uniformity of subsequent doping; and then through heat treatment at a suitable temperature, the crystal water therein can be well removed, the crystal strength of the material is improved, the stability of the structure is ensured, and more vacancies are provided for Na ions.
[0040] Wherein, the temperature of heat treatment may be 200-250°C, 250-300°C, 300-350°C, 350-400°C or 400-450°C. The temperature of heat treatment is controlled within the above range. On the one hand, the temperature can meet the requirement of removing crystal water, and on the other hand, the overall structure of the solid electrolyte will not be destroyed, ensuring its air stability in practical applications. Preferably, the temperature of heat treatment may be 200-350°C. Because the preparation method of the present invention in the early stage is to mix in the liquid phase, the uniformity of the distribution of doping elements is ensured, so at the same heat treatment temperature, the solid electrolyte structure of the present invention is more stable after the crystal water is removed.
[0041] In some embodiments, the coprecipitation reaction conditions are heating and stirring in a water bath at 60-80° C. for 4-8 hours; vacuum drying temperature is 120-200° C., and the drying time is 8-15 hours; and the heat treatment time is 2-12 hours.
[0042] The water bath temperature of the coprecipitation is controlled at 60-80°C and the reaction is carried out for 4-8 hours, which can ensure that the elements can be fully mixed and doped, and the particle agglomeration is greatly avoided during the doping process, fully ensuring the uniformity of the components.
[0043] Since the present invention adopts a multi-step liquid phase synthesis method for preparation and contains a large amount of water as a solvent, vacuum drying is first performed to remove the moisture before heat treatment, which can ensure the effect of removing crystal water in subsequent heat treatment and ensure the uniformity of the components.
[0044] In some embodiments, the preparation method of Na3SbS4 powder is: add Na2S, Sb2S3 and sulfur powder to deionized water, heat and stir in a water bath at 60~80°C, filter to obtain a homogeneous precursor aqueous solution of Na3SbS4, then add alcohol for precipitation reaction, the alcohol may preferably be isopropanol, to obtain Na3SbS4 hydrate, vacuum dry, and then heat treat at 200~350°C in an inert atmosphere to obtain Na3SbS4 powder.
[0045] In some embodiments, the preparation method of sodium thiotungstate molybdate powder is as follows: sodium alkali, thiotungstate salt, and thiomolybdate salt are mixed and added to deionized water, heated and stirred in a water bath at 60-80°C to obtain a precursor solution, vacuum dried, and then heat treated at 200-350°C in an inert atmosphere to obtain sodium thiotungstate molybdate powder, the chemical formula of which is Na2W x Mo y S4, 0<x≤1.0, 0<y≤1.0, and x+y=1. Among them, the thiotungsten salt is preferably (NH4)2WS4, and the thiomolybdenum salt is preferably (NH4)2MoS4.
[0046] In addition, the precursor raw materials Na3SbS4 powder and sodium thiotungstate molybdate powder used in the present invention are both prepared by liquid phase synthesis method, which can better control the components and regulate the particle morphology and size of the two precursors, so that when the two are subsequently prepared into sulfide solid electrolyte in liquid phase, co-precipitation can achieve uniform mixing of metal elements at the atomic level, thereby better ensuring the uniformity of material components.
[0047] In addition, the precursor raw materials used in the present invention are Na3SbS4 powder and Na2W x Mo y S4 powder, W, Mo will not be mixed with Sb element first, which will affect the overall crystal structure of the solid electrolyte. And compared with the method of mixing molybdenum sulfide, tungsten sulfide, antimony sulfide and sodium sulfide as raw materials respectively, the present invention can better dope tungsten and molybdenum into the crystal structure on the basis of Na3SbS4, and the obtained solid electrolyte is more stable and has better air stability.
[0048] In addition, the present invention also provides a solid-state sodium battery, comprising a positive electrode sheet, a negative electrode sheet and a solid electrolyte membrane spaced between the positive electrode sheet and the negative electrode sheet, wherein the solid electrolyte membrane is a solid electrolyte membrane made of the above-mentioned sulfide solid electrolyte, the positive electrode sheet may or may not contain the above-mentioned sulfide solid electrolyte; the negative electrode sheet may or may not contain the above-mentioned sulfide solid electrolyte. The preparation method of the solid electrolyte membrane can refer to the existing solid electrolyte membrane preparation method, such as wet preparation or dry preparation, which will not be repeated here.
[0049] Preferably, the thickness of the solid electrolyte membrane is 10 μm to 2000 μm, and more preferably 50 μm to 200 μm. If the solid electrolyte membrane is too thin, the mechanical strength will be reduced and it will be easily damaged. In addition, internal short circuits are more likely to occur.
[0050] The positive electrode sheet specifically includes a positive electrode current collector and a positive electrode active material layer coated on at least one surface of the positive electrode current collector. The positive electrode active material in the positive electrode active material layer can be a conventional positive electrode active material for sodium ion batteries, such as layered transition metal sodium oxide, polyanion positive electrode material and Prussian positive electrode material. The layered transition metal sodium oxide can be a layered transition metal sodium oxide doped with elements such as Li, Mg, Zn, Ca, Al, V, Cr, Mn, Fe, Ti, Zr, Sn, Ru, Nb, Co, Ni, etc., which will not be described in detail here. The positive electrode current collector can be various materials suitable for use as a positive electrode current collector for sodium ion batteries in the art. For example, the positive electrode current collector can be, but is not limited to, metal foil, etc., and more specifically, can be, but is not limited to, aluminum foil, etc.
[0051] The positive electrode active material layer also includes currently commonly used binders, conductive agents, etc. The binders include but are not limited to at least one of SBR, PAA, PI, PAN, and PVDF, and the conductive agents include but are not limited to at least one of carbon black (such as Super-P, KS-6), VGCF, multi-walled CNT, and single-walled CNT. No further details will be given here.
[0052] Specifically, the preparation method of the positive electrode sheet can be prepared according to the conventional preparation of the positive electrode sheet, such as preparing according to the following method: the positive electrode active material, the conductive agent, and the binder are prepared into a slurry in proportion, and then coated, rolled, and die-cut at a certain surface density to obtain a positive electrode sheet. In the slurry, the positive electrode active material can account for 70wt%-90wt%, the conductive agent can account for 0.05wt%-5wt%; the binder can account for 0.5wt%-5wt%. In addition, in order to further increase the ionic conductivity of the all-solid-state sodium ion battery, the sulfide solid electrolyte of the present invention can also be added to the positive electrode active material layer, and the content can account for 5wt%-25wt%.
[0053] The negative electrode sheet includes a negative electrode current collector and a negative electrode active material layer coated on at least one surface of the negative electrode current collector. The negative electrode active material in the negative electrode active material layer may be one or more of soft carbon, hard carbon, carbon fiber, mesophase carbon microspheres, tin-based materials, oxide-type negative electrode materials, or other metals that can form alloys with sodium. Among them, the carbon-based negative electrode material can be selected from one or more of soft carbon, hard carbon, carbon fiber, and mesophase carbon microspheres; the tin-based material can be selected from one or more of elemental tin, tin oxide compounds, and tin alloys. The negative electrode current collector is usually a structure or part for collecting current. The negative electrode current collector can be various materials in the art that are suitable for use as a negative electrode current collector for sodium ion batteries. For example, the negative electrode current collector can be metal foil, etc., and more specifically can be aluminum foil and copper foil, etc., but are not limited to.
[0054] At present, the commonly used negative electrode active material is a hard carbon material, which has a large interlayer spacing and is easy for sodium ions to be embedded and extracted; in addition, in order to facilitate experimental detection, a sodium sheet can also be directly used as the negative electrode, and then assembled to obtain an all-solid-state sodium ion battery. For other selection settings in the negative electrode sheet, please refer to the conventional negative electrode sheet for sodium ion batteries. For example, the negative electrode active material layer also includes currently commonly used binders, conductive agents, etc., and the proportion of each substance can be 65wt%-95wt% for the negative electrode active material, 0.05wt%-5wt% for the conductive agent, and 0.5wt%-5wt% for the binder. In addition, in order to further increase the ionic conductivity of the present all-solid-state sodium ion battery, the sulfide solid electrolyte of the present invention can also be added to the negative electrode active material layer, and the content can account for 5wt%-25wt%.
[0055] When the sulfide solid electrolyte of the present invention is added to both the positive electrode sheet and the negative electrode sheet, and then a solid electrolyte membrane made of the sulfide solid electrolyte of the present invention is formed to form an all-solid-state sodium ion battery, the electrochemical performance and air stability of the battery are higher.
[0056] To make the technical solutions and advantages of the present invention more clear, the present invention and its beneficial effects will be described in further detail below in conjunction with specific implementation methods and accompanying drawings, but the implementation methods of the present invention are not limited thereto.
[0057] Example 1
[0058] A sulfide solid electrolyte, made by liquid phase synthesis, with the chemical formula of Na 2.95 W 0.025 Mo 0.025 Sb 0.95 S4.
[0059] The specific preparation steps of the liquid phase synthesis method are:
[0060] 1) The preparation method of Na3SbS4 powder is as follows: Na2S, Sb2S3 and sulfur powder are added to deionized water according to a stoichiometric ratio (molar ratio of 3:1:2), heated and stirred in a water bath at 70°C for 6 hours, filtered to remove residual substances such as antimony sulfide, and obtained a homogeneous precursor aqueous solution of Na3SbS4, and then isopropanol is added for precipitation reaction to obtain Na3SbS4·9H2O, dried at 160°C under vacuum for 12 hours, and then heat treated at 270°C in an Ar atmosphere for 6 hours to obtain Na3SbS4 powder;
[0061] 2) The preparation method of sodium thiotungstate molybdate powder is as follows: NaOH, (NH4)2WS4, (NH4)2MoS4 are mixed in a stoichiometric ratio (molar ratio of 4:1:1), added into deionized water, heated and stirred in a water bath at 70°C for 6 hours to obtain a precursor solution, dried at 160°C for 12 hours under vacuum, and then heat treated at 270°C in an Ar atmosphere for 6 hours to obtain Na2W 0.5 Mo 0.5 S4 powder;
[0062] 3) Mix Na3SbS4 powder with Na2W 0.5 Mo 0.5 S4 powder was weighed and mixed according to the stoichiometric ratio (molar ratio of 19:1), and deionized water was added to prepare an aqueous solution, which was heated and stirred in a water bath at 70°C for 6 hours for coprecipitation reaction; then dried under vacuum at 160°C for 12 hours, and heat treated at 270°C in an Ar atmosphere for 6 hours to obtain a solution with the chemical formula Na 2.95 W 0.025 Mo 0.025Sb 0.95 S4 sulfide solid electrolyte.
[0063] Example 2
[0064] Different from Example 1, the chemical formula of the sulfide solid electrolyte in this example is Na 2.95 W 0.01 Mo 0.04 Sb 0.95 S4, the preparation can be carried out by adjusting the added content according to the different molar ratios of the elements, as shown in Example 1, which will not be described here.
[0065] Example 3
[0066] Different from Example 1, the chemical formula of the sulfide solid electrolyte in this example is Na 2.9 W 0.04 Mo 0.06 Sb 0.9 S4, the preparation can be carried out by adjusting the added content according to the different molar ratios of the elements, as shown in Example 1, which will not be described here.
[0067] Example 4
[0068] Different from Example 1, the chemical formula of the sulfide solid electrolyte in this example is Na 2.9 W 0.02 Mo 0.08 Sb 0.9 S4, the preparation can be carried out by adjusting the added content according to the different molar ratios of the elements, as shown in Example 1, which will not be described here.
[0069] Example 5
[0070] Different from Example 1, the chemical formula of the sulfide solid electrolyte in this example is Na 2.9 W 0.06 Mo 0.04 Sb 0.9 S4, the preparation can be carried out by adjusting the added content according to the different molar ratios of the elements, as shown in Example 1, which will not be described here.
[0071] Example 6
[0072] Different from Example 1, the chemical formula of the sulfide solid electrolyte in this example is Na 2.85 W 0.06 Mo 0.09 Sb 0.85 S4, the preparation can be carried out by adjusting the added content according to the different molar ratios of the elements, as shown in Example 1, which will not be described here.
[0073] Example 7
[0074] Different from Example 1, the chemical formula of the sulfide solid electrolyte in this example is Na 2.85 W 0.03 Mo 0.12 Sb 0.85 S4, the preparation can be carried out by adjusting the added content according to the different molar ratios of the elements, as shown in Example 1, which will not be described here.
[0075] Example 8
[0076] Different from Example 1, the chemical formula of the sulfide solid electrolyte in this example is Na 2.85 W 0.005 Mo 0.145 Sb 0.85 S4, the preparation can be carried out by adjusting the added content according to the different molar ratios of the elements, as shown in Example 1, which will not be described here.
[0077] Example 9
[0078] Different from Example 1, the chemical formula of the sulfide solid electrolyte in this example is Na 2.85 W 0.09 Mo 0.06 Sb 0.85 S4, the preparation can be carried out by adjusting the added content according to the different molar ratios of the elements, as shown in Example 1, which will not be described here.
[0079] Example 10
[0080] Different from Example 1, the chemical formula of the sulfide solid electrolyte in this example is Na 2.7 W 0.15 Mo 0.15 Sb 0.7 S4, the preparation can be carried out by adjusting the added content according to the different molar ratios of the elements, as shown in Example 1, which will not be described here.
[0081] Embodiment 11
[0082] Different from Example 1, the chemical formula of the sulfide solid electrolyte in this example is Na 2.7 W 0.1 Mo 0.2 Sb 0.7 S4, the preparation can be carried out by adjusting the added content according to the different molar ratios of the elements, as shown in Example 1, which will not be described here.
[0083] Example 12
[0084] Different from Example 1, the chemical formula of the sulfide solid electrolyte in this example is Na 2.7 W 0.2 Mo0.1 Sb 0.7 S4, the preparation can be carried out by adjusting the added content according to the different molar ratios of the elements, as shown in Example 1, which will not be described here.
[0085] Embodiment 13
[0086] Different from Example 1, the chemical formula of the sulfide solid electrolyte in this example is Na 2.6 W 0.05 Mo 0.35 Sb 0.6 S4, the preparation can be carried out by adjusting the added content according to the different molar ratios of the elements, as shown in Example 1, which will not be described here.
[0087] Embodiment 14
[0088] Different from Example 1, the chemical formula of the sulfide solid electrolyte in this example is Na 2.5 W 0.05 Mo 0.45 Sb 0.5 S4, the preparation can be carried out by adjusting the added content according to the different molar ratios of the elements, as shown in Example 1, which will not be described here.
[0089] Embodiment 15
[0090] Different from Example 1, the chemical formula of the sulfide solid electrolyte in this example is Na 2.5 W 0.45 Mo 0.05 Sb 0.5 S4, the preparation can be carried out by adjusting the added content according to the different molar ratios of the elements, as shown in Example 1, which will not be described here.
[0091] Comparative Example 1
[0092] Different from Example 1, the chemical formula of the sulfide solid electrolyte in this example is Na3SbS4, that is, there is no tungsten and molybdenum doping elements, and Na3SbS4 can be directly synthesized by liquid phase. Please refer to Example 1 and no further details will be given here.
[0093] Comparative Example 2
[0094] Different from Example 1, the chemical formula of the sulfide solid electrolyte in this example is Na 2.9 W 0.1 Sb 0.9 S4, the preparation can be carried out by adjusting the added content according to the different molar ratios of the elements, as shown in Example 1, which will not be described here.
[0095] Comparative Example 3
[0096] Different from Example 1, the chemical formula of the sulfide solid electrolyte in this example is Na 2.9 Mo 0.1 Sb 0.9 S4, the preparation can be carried out by adjusting the added content according to the different molar ratios of the elements, as shown in Example 1, which will not be described here.
[0097] Comparative Example 4
[0098] The difference from Example 3 is the preparation method. The sulfide solid electrolyte Na 2.9 W 0.04 Mo 0.06 Sb 0.9 The preparation method of S4 is specifically as follows:
[0099] In an inert gas atmosphere, Na2S, Sb2S3, MoS2, WS2 and sulfur powder raw materials were weighed and mixed according to the required components, fully ground in an agate mortar, put into a zirconia ball mill, and ball-milled at a speed of 500 rpm for 12 h. After ball milling, the powder was recovered and heat-treated at 270 °C for 6 h in an Ar gas atmosphere to obtain Na 2.9 W 0.04 Mo 0.06 Sb 0.9 S4 solid electrolyte.
[0100] Comparative Example 5
[0101] Different from Example 1, the chemical formula of the sulfide solid electrolyte in this example is Na 2.9 Mn 0.04 Mo 0.06 Sb 0.9 S4, the preparation can be carried out by adjusting the added content according to the different molar ratios of the elements, as shown in Example 1, which will not be described here.
[0102] Comparative Example 6
[0103] Different from Example 1, the chemical formula of the sulfide solid electrolyte in this example is Na 2.9 W 0.04 Mg 0.06 Sb 0.9 S4, the preparation can be carried out by adjusting the added content according to the different molar ratios of the elements, as shown in Example 1, which will not be described here.
[0104] The chemical formulas of the sulfide solid electrolytes obtained in Examples 1 to 15 and Comparative Examples 1 to 6 were sorted out, and the sodium ion conductivity was tested at room temperature of about 25 degrees.
[0105] The test method for sodium ion conductivity is as follows: Sodium ion conductivity is measured using impedance method in a symmetrical battery blocking Sus (stainless steel) / solid electrolyte / Sus in a mold (diameter = 10 mm) AC; Ti rods are used as current collectors, electrolyte sheets are prepared under a pressure of 3 tons, and the ionic conductivity of the solid electrolyte is measured using electrochemical impedance spectroscopy (EIS) measurements. The data collected ranges from 3 MHz to 10 Hz, using an impedance analyzer (EC-Lab) and an applied AC voltage of 10–25 mV. Various temperatures of 25 degrees were selected for measurement. Sodium ion conductivity (σ) is calculated by the following formula:
[0106] σ(mS / cm)=T / (R×A)
[0107] In the above formula, T is the thickness of the electrolyte sheet (cm), A is the area of the electrolyte sheet (cm 2 ), R is the resistance obtained by electrochemical impedance spectroscopy (mS -1 ).
[0108] The test results are shown in Table 1 below.
[0109] Table 1
[0110]
[0111] It can be seen from the above test results that the solid electrolyte prepared by the present invention can obtain a solid electrolyte with uniform doping and high particle uniformity by dual doping with Mo and W and coordinating with liquid phase synthesis, which provides more vacancies for sodium ions and improves the sodium ion conductivity of the solid electrolyte.
[0112] In addition, it can be seen from the comparison of Examples 1 to 15 that the proportion of tungsten and molybdenum is controlled within the range of 0.01 to 0.2, which avoids the problem of reducing the proportion of Sb due to excessive doping of the two, affecting the structure of the solid electrolyte, thereby ensuring the subsequent sodium ion conductivity. Preferably, the sum of the doping amounts of tungsten and molybdenum is controlled between 0.1 and 0.3, and the solid electrolyte exhibits higher ionic conductivity; at the same time, the doping amount of molybdenum is controlled to be more than the doping amount of tungsten, which can further improve the ionic conductivity of the solid electrolyte. This may be because the differences in atomic mass, atomic structure, etc. of tungsten and molybdenum make the two show different support for the crystal structure of the solid electrolyte when doped, thereby improving the ionic conductivity of the solid electrolyte.
[0113] In addition, the solid electrolytes in Example 3, Comparative Example 1 and Comparative Example 4 were characterized by SEM electron microscopy, XRD and Raman. Figures 1 to 4 shown.
[0114] Among them, Figure 4It can be seen from the Raman spectrum that at a wavelength of about 470 cm -1 and 450 cm -1 WS4 2- and MoS4 2- It can be seen from the characteristic peaks of the solid electrolyte of the present invention that tungsten and molybdenum elements are doped.
[0115] Depend on Figure 1 and Figure 2 It can be seen from the SEM image that the solid electrolyte particles prepared by the liquid phase synthesis method of the present invention are uniform and less agglomerated, which also verifies the reason why it exhibits excellent sodium ion conductivity. The solid electrolyte prepared by the conventional solid phase synthesis method has relatively large particles and more agglomerates.
[0116] Depend on Figure 3 It can be seen from the XRD graph that the intensity of the characteristic peak of the solid electrolyte of the present invention is higher than that of the results of Comparative Examples 1 and 4. It can be concluded that the solid electrolyte obtained by the liquid phase method has higher crystallinity, no unreacted raw materials and other non-products, and higher raw material purity.
[0117] In order to further verify the advantages of W-Mo dual doping in the present invention, the stabilities of solid electrolytes with different components in air were compared. Figure 5 The XRD pattern of the solid electrolyte of the components of comparative example 1 of the present invention after being exposed to air for 6 hours is shown. It can be seen from the figure that after the W-doped electrolyte is exposed to air, it easily absorbs moisture in the air, the crystallinity of the material decreases, and some by-products appear.
[0118] Figure 6 This is the XRD diagram of the solid electrolyte of Example 3 of the present invention after being exposed to air for 6 hours. Compared with the W-doped electrolyte, the W-Mo dual-doped electrolyte material still maintains good crystallinity even after being exposed for 6 hours, without obvious crystal changes and the generation of by-products. Through the above comparison, it can be further explained that W-Mo dual-doping can improve the air stability of the electrolyte material.
[0119] To further verify the advantages of the present invention, the Na 2.9 W 0.04 Mo 0.06 Sb 0.9 Taking S4 solid electrolyte as an example, the advantages of the liquid phase synthesis method are further explored by changing its preparation conditions, as shown in the following comparison of Examples 16 to 29.
[0120] Example 16
[0121] The difference from Example 3 is that in preparation step 3), the heat treatment conditions are heat treatment at 200°C in Ar atmosphere for 6 hours. The rest refers to Example 3 and will not be repeated here.
[0122] Embodiment 17
[0123] The difference from Example 3 is that in preparation step 3), the heat treatment conditions are heat treatment at 330°C in Ar atmosphere for 6 hours. The rest refers to Example 3 and will not be repeated here.
[0124] Embodiment 18
[0125] The difference from Example 3 is the preparation step 3), the heat treatment condition is heat treatment at 450°C in Ar atmosphere for 6h, and the rest is referred to Example 3 and will not be repeated here.
[0126] Embodiment 19
[0127] The difference from Example 3 is the preparation step 3), the heat treatment condition is heat treatment at 330°C in Ar atmosphere for 2h, and the rest is referred to Example 3 and will not be repeated here.
[0128] Embodiment 20
[0129] The difference from Example 3 is preparation step 3), the heat treatment condition is heat treatment at 270°C in Ar atmosphere for 12 hours, and the rest is referred to Example 3 and will not be repeated here.
[0130] Embodiment 21
[0131] The difference from Example 3 is that in preparation step 3), after the coprecipitation reaction, the mixture is dried under vacuum at 80°C for 12 hours and then heat treated. The rest is as in Example 3 and will not be described again here.
[0132] Embodiment 22
[0133] The difference from Example 3 is that in preparation step 3), the temperature of water bath heating is 40°C. The rest is as in Example 3 and will not be repeated here.
[0134] Embodiment 23
[0135] The difference from Example 3 is that in preparation step 2), the temperature of water bath heating in the preparation process of sodium thiotungstate molybdate powder is 40° C. The rest is referred to Example 3 and will not be repeated here.
[0136] Embodiment 24
[0137] The difference from Example 3 is that in preparation step 2), the heat treatment conditions in the preparation process of sodium thiotungstate molybdate powder are heat treatment at 200° C. for 6 h in an Ar atmosphere. The rest is referred to Example 3 and will not be repeated here.
[0138] Embodiment 25
[0139] The difference from Example 3 is preparation step 2), the heat treatment conditions in the preparation process of sodium thiotungstate molybdate powder are heat treatment at 330°C in Ar atmosphere for 6h, and the rest is referred to Example 3, which will not be repeated here.
[0140] Embodiment 26
[0141] The difference from Example 3 is that in preparation step 2), the sodium thiotungstate molybdate powder is prepared by solid phase synthesis method, which can be referred to the solid phase synthesis method in Comparative Example 4. The rest is referred to Example 3, which will not be repeated here.
[0142] Embodiment 27
[0143] The difference from Example 3 is that in preparation step 1), Na3SbS4 powder is prepared by solid phase synthesis method, which can be referred to the solid phase synthesis method in Comparative Example 4. The rest can be referred to Example 3, which will not be repeated here.
[0144] Embodiment 28
[0145] The difference from Example 3 is that the preparation steps 1) and 2) are both prepared by solid phase synthesis method for Na3SbS4 powder and sodium thiotungstate molybdate powder. Please refer to the solid phase synthesis method in Comparative Example 4. The rest is referred to Example 3 and will not be repeated here.
[0146] Embodiment 29
[0147] The difference from Example 3 is that in preparation step 3), after the coprecipitation reaction, heat treatment is directly performed without the vacuum drying step. The rest is as in Example 3 and will not be repeated here.
[0148] The sodium ion conductivity of the sulfide solid electrolytes obtained in Examples 16 to 29 was tested at room temperature of about 25 degrees. The test results are shown in Table 2 below.
[0149] Table 2
[0150]
[0151] It can be seen from the test results in Table 2 that the simultaneous control of the precursor raw materials Na3SbS4 powder and sodium thiotungstate molybdate powder by liquid phase synthesis is more conducive to improving the sodium ion conductivity of the subsequent solid electrolyte. This is mainly because the precursor is also made by liquid phase synthesis, which can control the composition and regulate the morphology and size of the particles, making it easier to evenly mix tungsten and molybdenum at the atomic level during subsequent doping.
[0152] In summary, the sulfide solid electrolyte provided by the present invention effectively improves the problems of poor air stability and ion conductivity that cannot meet the requirements of wide application of conventional sulfide solid electrolytes, and can achieve higher sodium ion conductivity under optimal control.
[0153] According to the disclosure and teaching of the above description, those skilled in the art to which the present invention belongs can also change and modify the above embodiment. Therefore, the present invention is not limited to the above specific embodiment, and any obvious improvement, replacement or modification made by those skilled in the art on the basis of the present invention belongs to the protection scope of the present invention. In addition, although some specific terms are used in this specification, these terms are only for the convenience of description and do not constitute any limitation to the present invention.
Claims
1. A sulfide solid electrolyte, characterized in that: It is made by liquid phase synthesis method and its chemical formula is Na 3-a- b W a Mo b Sb 1-a-b S4, 0<a<0.5, 0<b<0.5; the preparation method of the liquid phase synthesis method is: Na3SbS4 powder is mixed with sodium thiotungstate molybdate powder, and the mixture is prepared into an aqueous solution and stirred for coprecipitation reaction; then, after drying under vacuum conditions, heat treatment is performed at 200~450°C in an inert atmosphere to obtain Na 3-a-b W a Mo b Sb 1-a-b S4 sulfide solid electrolyte.
2. The sulfide solid electrolyte according to claim 1, characterized in that 0.01≤a≤0.25, 0.01≤b≤0.
25.
3. The sulfide solid electrolyte according to claim 2, characterized in that: 0.01<a≤0.2, 0.01<b≤0.2, and a≤b.
4. The sulfide solid electrolyte according to claim 3, characterized in that 0.1≤a+b≤0.3, and 0≤ba≤0.
1.
5. The sulfide solid electrolyte according to any one of claims 1 to 4, characterized in that The sodium ion conductivity is greater than or equal to 3.0 mS / cm at room temperature of 25°C.
6. The sulfide solid electrolyte according to claim 1, characterized in that The coprecipitation reaction conditions are heating and stirring in a water bath at 60-80°C for 4-8 hours; vacuum drying temperature is 120-200°C, and the drying time is 8-15 hours; and the heat treatment time is 2-12 hours.
7. The sulfide solid electrolyte according to claim 1, characterized in that: The preparation method of Na3SbS4 powder is as follows: Na2S, Sb2S3 and sulfur powder are added to deionized water, heated and stirred in a water bath at 60-80°C, filtered to obtain a homogeneous precursor aqueous solution of Na3SbS4, then alcohol is added for precipitation reaction to obtain Na3SbS4 hydrate, vacuum dried, and then heat treated at 200-350°C in an inert atmosphere to obtain Na3SbS4 powder.
8. The sulfide solid electrolyte according to claim 1, characterized in that The preparation method of sodium thiotungstate molybdate powder is as follows: sodium alkali, thiotungstate salt and thiomolybdate salt are mixed and added into deionized water, heated and stirred in a water bath at 60-80°C to obtain a precursor solution, vacuum dried, and then heat treated at 200-350°C in an inert atmosphere to obtain sodium thiotungstate molybdate powder, the chemical formula of which is Na2W x Mo y S4, 0<x≤1.0, 0<y≤1.0, and x+y=1.
9. An all-solid-state sodium ion battery, comprising a positive electrode sheet, a negative electrode sheet and a solid electrolyte membrane spaced between the positive electrode sheet and the negative electrode sheet, characterized in that: The solid electrolyte membrane is a solid electrolyte membrane made of the sulfide solid electrolyte described in any one of claims 1 to 8; the positive electrode sheet contains or does not contain the sulfide solid electrolyte described in any one of claims 1 to 8; the negative electrode sheet contains or does not contain the sulfide solid electrolyte described in any one of claims 1 to 8.