A thin film solar cell and its preparation method

By using materials such as ethylene-tetrafluoroethylene copolymer as a protective layer and two-dimensional graphene as an absorption layer, combined with a modified tin dioxide electron transport layer, the process of thin-film solar cells is simplified, and the process complexity and complexity in the existing technology are solved. Solve the problem of waste liquid pollution and realize high-efficiency and environmentally friendly thin-film solar cell production.

CN118382303BActive Publication Date: 2024-10-22GUANGDONG SUNRUI NEW MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410468531.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-18
Publication Date
2024-10-22
Estimated Expiration
2044-04-18

AI Technical Summary

Technical Problem

The manufacturing process of existing thin-film solar cells is complex and the production efficiency is low. Moreover, the wet film-forming process leads to waste liquid pollution and affects environmental protection.

Method used

It uses ethylene-tetrafluoroethylene copolymer, perfluoroethylene propylene copolymer, and polyimide film as the protective layer, combined with two-dimensional graphene transition metal carbide/carbonitride as the absorption layer, and modified tin dioxide as the electron transport layer, forming a buffer layer through ALD deposition, simplifying the process and improving material matching.

Benefits of technology

It improves the photoelectric conversion efficiency of thin-film solar cells, reduces manufacturing costs, has a simple process, is suitable for large-scale industrial production, reduces waste liquid pollution, and improves environmental performance.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present application relates to the technical field of solar cells, and more specifically, it relates to a thin-film solar cell and a method for preparing the same. The invention comprises a substrate, a light-transmitting layer and a protective layer stacked in sequence, a back electrode layer is formed on the substrate; an absorption layer is formed on the back electrode layer; a buffer layer is formed on the absorption layer; an electron transport layer is formed on the buffer layer, and a hole blocking layer is formed on the electron transport layer; the protective layer comprises one of an ethylene-tetrafluoroethylene copolymer film, a perfluoroethylene-propylene copolymer film, a chloroperfluoroethylene copolymer, a polyimide film, and a polyethylene terephthalate film; the light-transmitting layer is a transparent conductive oxide, and the transparent conductive oxide comprises indium-doped tin oxide, fluorine-doped tin oxide, and aluminum-doped zinc oxide; the absorption layer is Ti3C2T x MXene. Improve the photoelectric conversion efficiency of thin-film solar cells.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of solar cells, and more specifically, to a thin film solar cell and a preparation method thereof. Background Art

[0002] Thin-film solar cells have become the mainstream of solar cell development due to their advantages such as being free from resource and environmental restrictions, strong light transmittance, long power generation time, short industrial chain, low cost, short payback period, little impact from temperature changes, and wide application fields. Thin-film solar cells include back electrode layers, absorption layers, buffer layers, window layers and other film layers. At present, the manufacturing process of thin-film solar cells usually adopts a mixed dry and wet process. The buffer layer is formed by a wet film formation method (such as chemical water bath deposition), and other film layers are generally formed by a dry film formation process. However, since complex solution preparation is required during wet film formation, the process is complicated and the production efficiency is low; and after the preparation is completed, the remaining waste liquid is prone to pollution.

[0003] Solar cells are carriers for converting solar energy into electrical energy, and their performance directly affects the efficiency of solar energy utilization. At present, high efficiency and flexibility are the two main development directions of solar cells. High efficiency is an eternal topic in the development of solar cells. The continuous breakthroughs in basic research results have made the photoelectric conversion efficiency of solar cells approach the theoretical limit, and the technical barriers to large-scale industrial applications have been continuously overcome. Flexibility is a necessary way for solar cells to truly realize industrial applications. In a sense, solar cells can only be truly integrated into human daily production and life if they are flexible. Summary of the invention

[0004] The present invention provides a thin film solar cell and a preparation method thereof, which improve the photoelectric conversion efficiency of the thin film solar cell.

[0005] In a first aspect, the present disclosure provides a solar cell, comprising a substrate, a light-transmitting layer and a protective layer stacked in sequence, wherein a back electrode layer is formed on the substrate; an absorption layer is formed on the back electrode layer; a buffer layer is formed on the absorption layer; an electron transport layer is formed on the buffer layer, and a hole blocking layer is formed on the electron transport layer;

[0006] The protective layer comprises one of ethylene-tetrafluoroethylene copolymer film, perfluoroethylene-propylene copolymer film, chloroperfluoroethylene copolymer, polyimide film, and polyethylene terephthalate film;

[0007] The light-transmitting layer is a transparent conductive oxide, and the transparent conductive oxide includes indium-doped tin oxide, fluorine-doped tin oxide and aluminum-doped zinc oxide;

[0008] The absorption layer is a two-dimensional graphene-like transition metal carbide / carbonitride.

[0009] Preferably, the raw materials for preparing the protective layer include: zinc nitrate, gallium nitrate, antimony chloride, fluorine-containing diamine 2,2′-bis(trifluoromethyl)biphenyl diamine, embedded metal fullerene, sulfone-containing diamine monomer 3,3′-diaminodiphenyl sulfone, sodium dodecyl sulfonate, ethanol and ethylene glycol monoethyl ether.

[0010] Preferably, the two-dimensional graphene-like transition metal carbide / carbonitride is a new type of two-dimensional nanomaterial with a general structural formula of Mn+1Xn or Mn+1XnTx, which is usually obtained by selectively etching A atoms of the corresponding Mn+1AXn (n=1, 2, 3) phase precursor by chemical liquid phase or molten salt etching, wherein M represents one of the transition group metal elements of Ti, V, Cr, Sr, Zr, Nb, Mo, and Ta, A represents IIIA and IV group elements, X represents C and / or N elements, and T is a surface functionalized substitution group covering the outer metal layer.

[0011] Preferably, the absorption layer has a thickness of 300-1500 nm.

[0012] Preferably, the buffer layer is Zn(Ox, S1-x) deposited by ALD, wherein x=0-0.9.

[0013] Preferably, the thickness of the buffer layer is 1-30 nm.

[0014] Preferably, the electron transport layer is modified tin dioxide, and the method for preparing the electron transport layer comprises the following steps:

[0015] S1: Preparation of tin dioxide solution: SnO2 colloidal solution and ultrapure water were mixed in a volume ratio of 1:5, stirred on a stirring table for 30 min, and SnO2, water and 1,2-dibenzoyloxyphenyl chitosan dispersion were mixed in a volume ratio of 1:2.5-4.5:0.5-2.5;

[0016] S2: Preparation of electron transport layer: The prepared tin dioxide solution was filtered using a 0.22 μm polytetrafluoroethylene filter head, spin coated on a cleaned FTO glass substrate at a speed of 4000-6000 r / min for 30-60s, then annealed on a 150-200°C heating table for 30-40min, and naturally cooled to room temperature.

[0017] Preferably, the thickness of the electron transport layer is 1-200 nm.

[0018] Preferably, the back electrode layer is Au, Ag or Pt, and the thickness of the metal electrode is 30-500 nm.

[0019] In summary, this application has the following beneficial effects:

[0020] 1. The two-dimensional MXene materials in this application have become a promising class of materials in solar cell applications due to their excellent optical transparency, electrical properties and surface chemical compatibility. The construction of two-dimensional MXene materials for solar cells is mainly concentrated on Ti3C2Tx, which has excellent photoelectric properties due to its layered structure, high conductivity and rich surface active groups.

[0021] 2. The solar cell in this application has the characteristics of low manufacturing cost, simple process, high photoelectric conversion efficiency (PCE) and wide applicability. After improvement, the energy level matching between the SnO2 electron transport layer and the absorption layer is better, and the carrier extraction and transport performance is optimized;

[0022] 3. The present application changes the components of the protective layer in the cell to construct a new protective layer, thereby improving the overall working efficiency of the entire thin-film solar cell. The resulting thin-film solar cell is very suitable for large-scale industrial production applications.

[0023] It should be understood that the foregoing general description and the following detailed description are exemplary and explanatory only and are not intended to limit the scope of protection of the present disclosure. DETAILED DESCRIPTION

[0024] The present application is further described in detail below in conjunction with the examples. It is particularly noted that if no specific conditions are specified in the following examples, the experiments are carried out according to conventional conditions or the conditions recommended by the manufacturer. Unless otherwise specified, the raw materials used in the following examples can be obtained from common commercial sources.

[0025] Preparation examples of raw materials and / or intermediates

[0026] Preparation Example 1

[0027] The method for preparing an electron transport layer comprises the following steps:

[0028] S1: Preparation of tin dioxide solution: SnO2 colloidal solution and ultrapure water were mixed in a volume ratio of 1:5 and stirred on a stirring table for 30 min. SnO2, water and 1,2-dibenzoyloxyphenyl chitosan dispersion were mixed in a volume ratio of 1:2.5:0.5;

[0029] S2: Preparation of electron transport layer: The prepared tin dioxide solution was filtered using a 0.22 μm polytetrafluoroethylene filter head, spin coated on the cleaned FTO glass substrate at a speed of 4000 r / min for 30 seconds, then annealed on a heating table at 150°C for 30 minutes, and naturally cooled to room temperature.

[0030] Preparation Example 2

[0031] The method for preparing an electron transport layer comprises the following steps:

[0032] S1: Preparation of tin dioxide solution: SnO2 colloidal solution and ultrapure water were mixed in a volume ratio of 1:5 and stirred on a stirring table for 30 min. SnO2, water and 1,2-dibenzoyloxyphenyl chitosan dispersion were mixed in a volume ratio of 1:3:1;

[0033] S2: Preparation of electron transport layer: The prepared tin dioxide solution was filtered using a 0.22 μm polytetrafluoroethylene filter head, spin coated on the cleaned FTO glass substrate at a speed of 6000 r / min for 60 seconds, then annealed on a heating table at 200°C for 40 minutes, and naturally cooled to room temperature.

[0034] Preparation Example 3

[0035] The method for preparing an electron transport layer comprises the following steps:

[0036] S1: Preparation of tin dioxide solution: SnO2 colloidal solution and ultrapure water were mixed in a volume ratio of 1:5 and stirred on a stirring table for 30 min. SnO2, water and 1,2-dibenzoyloxyphenyl chitosan dispersion were mixed in a volume ratio of 1:4.5:2.5;

[0037] S2: Preparation of electron transport layer: The prepared tin dioxide solution was filtered using a 0.22 μm polytetrafluoroethylene filter head, spin coated on the cleaned FTO glass substrate at a speed of 4000 r / min for 30 seconds, then annealed on a heating table at 180°C for 30 minutes, and naturally cooled to room temperature. Example Example 1

[0038] A solar cell comprises a substrate, a light-transmitting layer and a protective layer stacked in sequence, wherein a back electrode layer is formed on the substrate; an absorption layer is formed on the back electrode layer; a buffer layer is formed on the absorption layer; an electron transport layer is formed on the buffer layer, and a hole blocking layer is formed on the electron transport layer;

[0039] The substrate is selected to contain a corresponding transparent conductive glass substrate; the light-transmitting layer is indium-doped tin oxide;

[0040] The raw materials for preparing the protective layer include: zinc nitrate, gallium nitrate, antimony chloride, fluorine-containing diamine 2,2′-bis(trifluoromethyl)diphenyl diamine, embedded metal fullerene, sulfone-containing diamine monomer 3,3′-diaminodiphenyl sulfone, sodium dodecyl sulfonate, ethanol and ethylene glycol monoethyl ether are mixed, and the mixture is coated on the surface of a substrate (the substrate is ultrasonically cleaned with ethanol for 30 minutes) at an amount of 45 mg / cm2, and then heated for the first time, the temperature of the first heating is 150°C, and the time of the first heating is 1 hour. Hydrogen is then introduced at a flow rate of 1.5 L / min, and heated for the second time, the temperature of the second heating is 800°C, and the time of the second heating is 1.5 hours to obtain a protective layer.

[0041] The absorber layer is Ti3C2Tx MXene; the buffer layer is an ALD-deposited Zn(O, S) layer;

[0042] The electron transport layer is prepared in Preparation Example 1; the back electrode layer is Au;

[0043] The thickness of the absorption layer is 300nm, the hole blocking layer is a silicon oxide layer with a thickness of 200nm formed by vacuum coating, the thickness of the buffer layer is 21nm, the thickness of the electron transport layer is 155nm, and the thickness of the back electrode is 45nm. Example 2

[0044] A solar cell comprises a substrate, a light-transmitting layer and a protective layer stacked in sequence, wherein a back electrode layer is formed on the substrate; an absorption layer is formed on the back electrode layer; a buffer layer is formed on the absorption layer; an electron transport layer is formed on the buffer layer, and a hole blocking layer is formed on the electron transport layer;

[0045] The substrate is selected to contain a corresponding transparent conductive glass substrate; the light-transmitting layer is indium-doped tin oxide;

[0046] The raw materials for preparing the protective layer include: zinc nitrate, gallium nitrate, antimony chloride, fluorine-containing diamine 2,2′-bis(trifluoromethyl)diphenyl diamine, embedded metal fullerene, sulfone-containing diamine monomer 3,3′-diaminodiphenyl sulfone, sodium dodecyl sulfonate, ethanol and ethylene glycol monoethyl ether are mixed, and the mixture is coated on the surface of a substrate (the substrate is ultrasonically cleaned with ethanol for 30 minutes) at an amount of 45 mg / cm2, and then heated for the first time, the temperature of the first heating is 150°C, and the time of the first heating is 1 hour. Hydrogen is then introduced at a flow rate of 1.5 L / min, and heated for the second time, the temperature of the second heating is 800°C, and the time of the second heating is 1.5 hours to obtain a protective layer.

[0047] The absorber layer is Ti3C2Tx MXene; the buffer layer is an ALD-deposited Zn(O, S) layer;

[0048] The electron transport layer is prepared in Preparation Example 2; the back electrode layer is Au;

[0049] The thickness of the absorption layer is 300nm, the hole blocking layer is a silicon oxide layer with a thickness of 300nm formed by vacuum coating, the thickness of the buffer layer is 30nm, the thickness of the electron transport layer is 185nm, and the thickness of the back electrode is 451nm. Example 3

[0050] A solar cell comprises a substrate, a light-transmitting layer and a protective layer stacked in sequence, wherein a back electrode layer is formed on the substrate; an absorption layer is formed on the back electrode layer; a buffer layer is formed on the absorption layer; an electron transport layer is formed on the buffer layer, and a hole blocking layer is formed on the electron transport layer;

[0051] The substrate is selected to contain a corresponding transparent conductive glass substrate; the light-transmitting layer is indium-doped tin oxide;

[0052] The raw materials for preparing the protective layer include: zinc nitrate, gallium nitrate, antimony chloride, fluorine-containing diamine 2,2′-bis(trifluoromethyl)diphenyl diamine, embedded metal fullerene, sulfone-containing diamine monomer 3,3′-diaminodiphenyl sulfone, sodium dodecyl sulfonate, ethanol and ethylene glycol monoethyl ether are mixed, and the mixture is coated on the surface of a substrate (the substrate is ultrasonically cleaned with ethanol for 30 minutes) at an amount of 45 mg / cm2, and then heated for the first time, the temperature of the first heating is 150°C, and the time of the first heating is 1 hour. Hydrogen is then introduced at a flow rate of 1.5 L / min, and heated for the second time, the temperature of the second heating is 800°C, and the time of the second heating is 1.5 hours to obtain a protective layer.

[0053] The absorber layer is Ti3C2Tx MXene; the buffer layer is an ALD-deposited Zn(O, S) layer;

[0054] The electron transport layer is prepared in Preparation Example 3; the back electrode layer is Au;

[0055] The thickness of the absorption layer is 552nm, the hole blocking layer is a silicon oxide layer with a thickness of 210nm formed by vacuum coating, the thickness of the buffer layer is 21nm, the thickness of the electron transport layer is 166nm, and the thickness of the back electrode is 384nm.

[0056] Comparative Example

[0057] Comparative Example 1

[0058] The thin film solar cell was prepared according to the method of Example 2, except that the electron transport layer was replaced by a SnO2 electron transport layer prepared from a common commercial colloidal solution.

[0059] Comparative Example 2

[0060] The thin-film solar cell is prepared according to the method of Example 2, except that the absorption layer is replaced by graphene.

[0061] For the thin-film solar cells prepared in Examples 1-3 and Comparative Examples 1-2, an effective spectral region of the protective layer was detected using an ultraviolet-visible / near-infrared spectrophotometer; the photoelectric conversion efficiency was tested with reference to GBT34160-2017 Test Method for Photoelectric Conversion Efficiency of Terrestrial Photovoltaic Modules; the results are shown in Table 1.

[0062] Table 1

[0063] Effective spectral range (nm) Photoelectric conversion efficiency (%) Example 1 250-1850 38.9 Example 2 221-1910 39.2 Example 3 245-2010 40.1 Comparative Example 1 459-1200 20.3 Comparative Example 2 421-1430 25.6

[0064] It can be seen from Table 1 that the photoelectric conversion efficiency of the thin-film solar cell prepared in Example 2 is the best, indicating that the working efficiency of the electron transport layer and the light absorption layer is the best.

[0065] The above is only an exemplary embodiment of the present disclosure, but the protection scope of the present disclosure is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed in the present disclosure should be included in the protection scope of the present disclosure. Therefore, the protection scope of the present disclosure should be based on the protection scope of the claims.

Claims

1. A solar cell, It is characterized in that The invention comprises a substrate, a light-transmitting layer and a protective layer stacked in sequence, wherein a back electrode layer is formed on the substrate; an absorption layer is formed on the back electrode layer; a buffer layer is formed on the absorption layer; an electron transport layer is formed on the buffer layer, and a hole blocking layer is formed on the electron transport layer; The protective layer comprises one of ethylene-tetrafluoroethylene copolymer film, perfluoroethylene-propylene copolymer film, chlorinated perfluoroethylene copolymer, polyimide film, and polyethylene terephthalate film; The light-transmitting layer is a transparent conductive oxide, and the transparent conductive oxide includes indium-doped tin oxide, fluorine-doped tin oxide and aluminum-doped zinc oxide; The absorption layer is Ti 3 C 2 T x MXene.

2. The solar cell according to claim 1, It is characterized in that The raw materials for preparing the protective layer include: zinc nitrate, gallium nitrate, antimony chloride, fluorine-containing diamine 2,2'-bis(trifluoromethyl)biphenyl diamine, embedded metal fullerene, sulfone-containing diamine monomer 3,3'-diaminodiphenyl sulfone, sodium dodecyl sulfonate, ethanol and ethylene glycol monoethyl ether.

3. The solar cell according to claim 1, It is characterized in that The thickness of the absorption layer is 300-1500 nm.

4. The solar cell according to claim 1, It is characterized in that The buffer layer is Zn(O x , S 1-x ), where x=0-0.

9.

5. The solar cell according to claim 1, It is characterized in that The thickness of the buffer layer is 1-30 nm.

6. The solar cell according to claim 1, It is characterized in that The hole blocking layer is a silicon oxide layer with a thickness of 1-300 nm formed by vacuum coating.

7. The solar cell according to claim 1, It is characterized in that The electron transport layer is modified tin dioxide, and the preparation method of the electron transport layer comprises the following steps: S1: Preparation of tin dioxide solution: SnO 2 The colloidal solution and ultrapure water were mixed in a volume ratio of 1:5 and stirred on a stirring table for 30 min. 2 , water and 1,2-dibenzoyloxyphenyl chitosan dispersion are mixed in a volume ratio of 1:2.5-4.5:0.5-2.5; S2: Preparation of electron transport layer: The prepared tin dioxide solution was filtered using a 0.22 μm polytetrafluoroethylene filter head, spin coated on a cleaned FTO glass substrate at a speed of 4000-6000 r / min for 30-60s, then annealed on a 150-200°C heating table for 30-40min, and naturally cooled to room temperature.

8. The solar cell according to claim 1, It is characterized in that The thickness of the electron transport layer is 1-200 nm.

9. The solar cell according to claim 1, It is characterized in that The back electrode layer is Au, Ag or Pt, and the thickness of the back electrode is 30-500 nm.