A method for preparing biomass-based hard carbon negative electrode material
Through the gelatinization and fermentation of starch to form a uniform pore structure, combined with the uniform distribution of tetrabutyl titanate and titanium dioxide, high-temperature carbonization treatment solves the problem of inconsistent performance in the preparation of biomass hard carbon materials and achieves structural consistency and Hard carbon material with stable performance, suitable for sodium-ion battery negative electrode.
Patent Information
- Application Number
- CN202410577504.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-10
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2044-05-10
AI Technical Summary
During the preparation process of existing biomass hard carbon materials, product performance cannot be effectively guaranteed, resulting in inconsistent structures and large performance differences.
Starch is used as the carbon source, and an open and uniform pore structure is formed through gelatinization and fermentation. Combined with the uniform distribution of tetrabutyl titanate and titanium dioxide, high-temperature carbonization is carried out through the control of hydrogen and inert atmosphere to ensure the structure of the hard carbon material. Consistency and stable performance.
It achieves the structural consistency and performance stability of hard carbon materials, improves its cycle life and safety, and ensures the efficiency and safety of sodium-ion battery anode materials.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of secondary battery materials and more specifically relates to a method for preparing a biomass-based hard carbon negative electrode material. Background Art
[0002] The ideal negative electrode material for sodium-ion batteries should meet the following requirements as far as possible: low operating voltage, high specific capacity, high first-cycle Coulomb efficiency, high compaction density, high electronic and ionic conductivity, stable structure (small volume deformation) and air stability, low cost, and safety and non-toxicity.
[0003] At present, the main negative electrode materials for sodium batteries are carbon-based materials, alloy materials, transition metal oxides and organic compounds. Among carbon-based materials, traditional graphite is the most important negative electrode material for lithium battery systems. However, due to thermodynamic reasons, sodium ions cannot be embedded in the graphite interlayer to form a stable compound with carbon, so graphite is difficult to use as a negative electrode material for sodium batteries. Amorphous carbon (soft carbon, hard carbon) with a large interlayer spacing has a higher sodium storage capacity, lower sodium storage potential, excellent cycle stability, and good application prospects. Hard carbon is carbon that cannot be graphitized after high-temperature treatment above 2800°C. It has the advantages of high capacity, support for fast charging and over-discharging, and strong safety. The theoretical capacity can reach 530mAh / g. Under the demand for high energy density in terminal applications, hard carbon materials have become the mainstream negative electrode materials.
[0004] Ensuring the consistency of material structure is the basis for ensuring the cycle life and safety of the battery system. Biomass from different origins and batches is often inconsistent, and the structure of hard carbon materials depends on the state of the precursor and the carbonization process. Only by ensuring that the precursor is highly consistent and the heat is very uniform during the carbonization process can the consistency of the final hard carbon material product be guaranteed.
[0005] Hard carbon anodes using different biomass materials as precursors require different carbonization temperatures, and the resulting anode materials have significantly different first-cycle coulomb efficiencies. Temperature, humidity, atmosphere, raw material ratio and other factors have different effects on the product's mass density, pore structure and distribution, mechanical strength, and electrical conductivity. Summary of the invention
[0006] The technical problem to be solved by the present invention is to overcome the problem that the product performance cannot be effectively guaranteed during the preparation process of existing biomass hard carbon materials, and provide a method for preparing a biomass-based hard carbon negative electrode material.
[0007] The purpose of the present invention is to provide a method for preparing a biomass-based hard carbon negative electrode material.
[0008] The above-mentioned purpose of the present invention is achieved through the following technical solutions:
[0009] A method for preparing a biomass-based hard carbon negative electrode material, the specific preparation steps comprising:
[0010] Starch gelatinization:
[0011] After starch and water are mixed, gelatinization is performed to obtain gelatinized starch;
[0012] Starch fermentation:
[0013] The gelatinized starch and lactic acid bacteria are mixed and fermented to obtain fermented starch;
[0014] Carbonization of starch:
[0015] After drying the fermented starch to a moisture content of less than 3%, grinding it into powder and sieving it to obtain refined starch;
[0016] Dispersing the refined starch in N-methylpyrrolidone, adding 6-8% of tetrabutyl titanate by weight of the refined starch, heating under reflux for more than 6 hours, filtering, washing and drying to obtain a precursor;
[0017] The precursor is heated and reduced in a hydrogen atmosphere, and then heated to 1000-1200° C. in an inert atmosphere, and carbonized for 4-6 hours, and then cooled and discharged to obtain a biomass-based hard carbon negative electrode material.
[0018] First, by using gelatinized starch as a carbon source, after gelatinization, the starch, on the one hand, helps to form an open pore structure, which can provide more active sites and faster ion transfer paths; on the other hand, it helps to improve the thermal stability of starch, which is particularly important for maintaining its microstructure during high-temperature carbonization. Secondly, further fermentation after gelatinization can remove volatile substances existing in the starch itself or produced during the gelatinization process, thereby improving the yield of hard carbon. In addition, a more uniform pore structure can be formed on the basis of gelatinization during the fermentation process. The reason why lactic acid bacteria are chosen for fermentation is that its fermentation can produce a small amount of lactic acid. In the subsequent reaction process with tetrabutyl titanate, first, a small amount of water remaining in the fermented starch can evaporate and react with tetrabutyl titanate. As the reflux reaction continues, lactic acid and the active hydroxyl groups in the starch gelatinization or fermentation products undergo esterification reactions, and the water molecules produced by the esterification and dehydration continue to contact with tetrabutyl titanate to continuously form titanium dioxide. In particular, titanium dioxide can be evenly dispersed and deposited in the open and uniform pore structure produced in the previous gelatinization and fermentation processes, so that it can play a more uniform role inside the hard carbon pores, improve the crystallinity of hard carbon in different parts, and its effect becomes uniform due to the uniform distribution of titanium dioxide.
[0019] Furthermore, the gelatinization of the starch also includes:
[0020] Take starch and warm water at a temperature of 45-50°C in a mass ratio of 1:1, divide the warm water into 3 equal parts, stir and mix one part with starch, then add the second part of warm water, continue to stir and mix, then add the third part of warm water, continue to stir and mix, heat and gelatinize at a temperature of 100-105°C for 40-60 minutes, cool to room temperature, and discharge to obtain gelatinized starch.
[0021] Furthermore, the screening is through a 800-1250 mesh sieve.
[0022] Furthermore, the carbonization of the starch also includes:
[0023] Heat the precursor to 400-420°C at a rate of 1-3°C / min under a hydrogen atmosphere and reduce it for 2-3 hours;
[0024] The hydrogen atmosphere is a mixed gas composed of hydrogen and nitrogen in a volume ratio of 1:5-1:6.
[0025] Through hydrogen reduction, the oxygen content in the product is regulated, and by adjusting the process parameters such as the gas introduction rate, reduction temperature and time, it is ensured that the mixed gas can diffuse in the aforementioned open and uniform channel, so that the effect of hydrogen is also uniform and sufficient.
[0026] Furthermore, the carbonization of the starch also includes:
[0027] In an inert atmosphere, slowly heat to 1000-1200℃ at a rate of 0.8-1.5℃ / min, keep carbonized for 4-6h, cool to room temperature with the furnace, and discharge;
[0028] Wherein, the inert atmosphere is selected from any one of argon or nitrogen.
[0029] Furthermore, by using a slow heating rate, the pore structure of the carbon is prevented from changing too drastically, thereby causing the titanium dioxide adsorbed inside the pores to desorb during the carbonization process.
[0030] Furthermore, the fermentation of starch also includes:
[0031] Add gelatinized starch into a fermentation tank, and inoculate lactic acid bacteria at an inoculation rate of 3-5%. Under the conditions that the initial pH of the material in the fermentation tank is 7.2-7.4 and the fermentation temperature is 30-35°C, fermentation is continued for 8-12 hours, and then the material is discharged and sterilized to obtain fermented starch.
[0032] Furthermore, the specific preparation steps also include:
[0033] After the carbonization of the starch, an activation treatment is performed.
[0034] Furthermore, the specific preparation steps also include:
[0035] Carbonization of starch:
[0036] After drying the fermented starch to a moisture content of less than 3%, grinding it into powder and sieving it to obtain refined starch;
[0037] Dispersing the refined starch in N-methylpyrrolidone, adding 6-8% of tetrabutyl titanate by weight of the refined starch, heating under reflux for more than 6 hours, filtering, washing and drying to obtain a precursor;
[0038] The precursor is heated and reduced in a hydrogen atmosphere, and then heated to 1000-1200°C in an inert atmosphere, and carbonized for 4-6 hours, and then cooled and discharged to obtain carbonized starch;
[0039] Product activation:
[0040] The carbonized starch and a saturated sodium bicarbonate solution at a temperature of 50°C are mixed and dispersed evenly by ultrasonication, then cooled to 5-10°C and filtered. The filter cake is dried and transferred to a carbonization furnace. The temperature is raised to 250-270°C in a nitrogen atmosphere. After the reaction is kept warm for 2-3 hours, the product is cooled, discharged, washed and dried to complete the activation of the product. DETAILED DESCRIPTION
[0041] The present invention is further described below with reference to specific examples, but the examples do not limit the present invention in any form. Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art.
[0042] Unless otherwise specified, the reagents and materials used in the following examples are commercially available.
[0043] Example 1
[0044] Starch gelatinization:
[0045] Starch and warm water at a temperature of 45°C are taken at a mass ratio of 1:1, and the warm water is divided into 3 equal parts, one of which is mixed with starch, and stirred and mixed for 2 hours at a stirring speed of 200 r / min, and then the second part of warm water is added under stirring, and the stirring and mixing is continued for 1 hour, and then the third part of warm water is added under stirring, and the stirring and mixing is continued for 2 hours, and then heated and gelatinized for 40 minutes at a temperature of 100°C under stirring, and then cooled to room temperature and discharged to obtain gelatinized starch;
[0046] The starch is selected from corn starch;
[0047] Starch fermentation:
[0048] Add gelatinized starch into a fermentation tank, and inoculate lactic acid bacteria at an inoculation rate of 3%. Under the conditions that the initial pH of the material in the fermentation tank is 7.2 and the fermentation temperature is 30°C, the fermentation is continued for 8 hours, and then the material is discharged and sterilized to obtain fermented starch;
[0049] Carbonization of starch:
[0050] The fermented starch was dried to a moisture content of 3%, then ground into powder and passed through an 800-mesh sieve to obtain refined starch;
[0051] Dispersing the refined starch in N-methylpyrrolidone, adding 6% tetrabutyl titanate by weight of the refined starch, heating under reflux for 6 hours, filtering, washing and drying to obtain a precursor;
[0052] The precursor was heated to 400°C at a rate of 1°C / min in a hydrogen atmosphere and kept for reduction for 2h;
[0053] Wherein, the hydrogen atmosphere is a mixed gas formed by mixing hydrogen and nitrogen in a volume ratio of 1:5;
[0054] In an inert atmosphere, slowly heat to 1000°C at a rate of 0.8°C / min, carbonize for 4 hours, cool to room temperature with the furnace, and discharge to obtain carbonized starch;
[0055] Wherein, the inert atmosphere is selected from argon;
[0056] Product activation:
[0057] The carbonized starch and a saturated sodium bicarbonate solution at a temperature of 50°C were mixed and dispersed evenly by ultrasonication, then cooled to 5°C and filtered. The filter cake was dried and transferred to a carbonization furnace. The temperature was raised to 250°C in a nitrogen atmosphere. After the reaction was kept warm for 2 hours, the product was cooled, discharged, washed and dried to complete the activation of the product.
[0058] Example 2
[0059] Starch gelatinization:
[0060] Take starch and warm water at a temperature of 48°C in a mass ratio of 1:1, divide the warm water into 3 equal parts, mix one part with starch, stir and mix for 3 hours at a stirring speed of 250r / min, then add the second part of warm water under stirring, continue to stir and mix for 1.5 hours, then add the third part of warm water under stirring, continue to stir and mix for 2.5 hours, heat and gelatinize at 102°C under stirring for 50 minutes, cool to room temperature, and discharge to obtain gelatinized starch;
[0061] The starch is selected from corn starch;
[0062] Starch fermentation:
[0063] Add gelatinized starch into a fermentation tank, and inoculate lactic acid bacteria at an inoculation rate of 4%. Under the conditions that the initial pH of the material in the fermentation tank is 7.3 and the fermentation temperature is 32°C, the fermentation is continued for 10 hours, and then the material is discharged and sterilized to obtain fermented starch;
[0064] Carbonization of starch:
[0065] The fermented starch was dried to a moisture content of 2.8%, then ground into powder and passed through a 1000-mesh sieve to obtain refined starch;
[0066] The refined starch is dispersed in N-methylpyrrolidone, and then 7% of the weight of the refined starch is added with tetrabutyl titanate, heated under reflux for 6.2 hours, filtered, washed and dried to obtain a precursor;
[0067] The precursor was heated to 410°C at a rate of 2°C / min under a hydrogen atmosphere and reduced for 2.5 h;
[0068] Wherein, the hydrogen atmosphere is a mixed gas formed by mixing hydrogen and nitrogen in a volume ratio of 1:5;
[0069] In an inert atmosphere, slowly heat to 1100°C at a rate of 1.2°C / min, carbonize for 5 hours, cool to room temperature with the furnace, and discharge to obtain carbonized starch;
[0070] Wherein, the inert atmosphere is selected from argon;
[0071] Product activation:
[0072] The carbonized starch and a saturated sodium bicarbonate solution at a temperature of 50°C were mixed and dispersed evenly by ultrasonication, then cooled to 8°C and filtered. The filter cake was dried and transferred to a carbonization furnace. The temperature was raised to 260°C in a nitrogen atmosphere. After the reaction was kept warm for 2.5 hours, the product was cooled, discharged, washed and dried to complete the activation of the product.
[0073] Example 3
[0074] Starch gelatinization:
[0075] Take starch and warm water at a temperature of 50°C in a mass ratio of 1:1, divide the warm water into 3 equal parts, mix one part with starch, stir and mix for 4 hours at a stirring speed of 300r / min, then add the second part of warm water under stirring, continue to stir and mix for 2 hours, then add the third part of warm water under stirring, continue to stir and mix for 3 hours, heat and gelatinize at 105°C for 60 minutes under stirring, cool to room temperature, and discharge to obtain gelatinized starch;
[0076] The starch is selected from corn starch;
[0077] Starch fermentation:
[0078] Add gelatinized starch into a fermentation tank, and inoculate lactic acid bacteria at an inoculation rate of 5%. Under the conditions that the initial pH of the material in the fermentation tank is 7.4 and the fermentation temperature is 35°C, ferment for 12 hours, discharge the material, and sterilize to obtain fermented starch;
[0079] Carbonization of starch:
[0080] The fermented starch was dried to a moisture content of 2.5%, then ground into powder and passed through a 1250-mesh sieve to obtain refined starch;
[0081] Dispersing the refined starch in N-methylpyrrolidone, adding tetrabutyl titanate at 8% of the weight of the refined starch, heating under reflux for 6.8 hours, filtering, washing and drying to obtain a precursor;
[0082] The precursor was heated to 420°C at a rate of 3°C / min in a hydrogen atmosphere and reduced for 3 h;
[0083] Wherein, the hydrogen atmosphere is a mixed gas formed by mixing hydrogen and nitrogen in a volume ratio of 1:6;
[0084] In an inert atmosphere, slowly heat to 1200°C at a rate of 1.5°C / min, carbonize for 6 hours, cool to room temperature with the furnace, and discharge to obtain carbonized starch;
[0085] Wherein, the inert atmosphere is selected from nitrogen;
[0086] Product activation:
[0087] The carbonized starch and a saturated sodium bicarbonate solution at a temperature of 50°C were mixed and dispersed evenly by ultrasonication, then cooled to 10°C and filtered. The filter cake was dried and transferred to a carbonization furnace. The temperature was raised to 270°C in a nitrogen atmosphere. After the reaction was kept warm for 3 hours, the product was cooled, discharged, washed and dried to complete the activation of the product.
[0088] Example 4
[0089] Compared with Example 1, this embodiment is different in that:
[0090] Carbonization of starch:
[0091] The fermented starch was dried to a moisture content of 3%, then ground into powder and passed through an 800-mesh sieve to obtain refined starch;
[0092] Dispersing the refined starch in N-methylpyrrolidone, adding 6% tetrabutyl titanate by weight of the refined starch, heating under reflux for 6 hours, filtering, washing and drying to obtain a precursor;
[0093] The precursor was heated to 400°C at a rate of 5°C / min in a hydrogen atmosphere and kept for reduction for 2h;
[0094] Wherein, the hydrogen atmosphere is a mixed gas formed by mixing hydrogen and nitrogen in a volume ratio of 1:5;
[0095] In an inert atmosphere, slowly heat to 1000°C at a rate of 8°C / min, carbonize for 4 hours, cool to room temperature with the furnace, and discharge to obtain carbonized starch;
[0096] Wherein, the inert atmosphere is selected from argon.
[0097] The rest of the conditions remain unchanged.
[0098] Example 5
[0099] Compared with Example 1, this example is different in that the product activation is not performed, and the other conditions remain unchanged.
[0100] Since no further activation treatment is performed, the porosity of the product is relatively low, but thanks to the treatment in the previous steps, the product performance is basically guaranteed.
[0101] Comparative Example 1
[0102] The difference between this comparative example and Example 1 is that an equal amount of N-methylpyrrolidone is used to replace tetrabutyl titanate, and other conditions remain unchanged.
[0103] Comparative Example 2
[0104] The difference between this comparative example and Example 1 is that the starch is not gelatinized, and the other conditions remain unchanged.
[0105] Comparative Example 3
[0106] The difference between this comparative example and Example 1 is that the gelatinized starch is not fermented, and the other conditions remain unchanged.
[0107] The performance tests were performed on the products obtained in Examples 1-5 and Comparative Examples 1-3. The specific test methods and test results are as follows:
[0108] The hard carbon material, conductive carbon black and polyvinylidene fluoride prepared in the above-mentioned embodiments or comparative examples were dissolved in a solvent N-methylpyrrolidone at a mass ratio of 8:1:1. The slurry was evenly coated on a copper foil to prepare an electrode plate. The prepared electrode plate was vacuum dried at 80 °C for 12 hours and then cut into a circular plate with a diameter of 12 mm. With metal Na as the counter electrode and glass fiber membrane as the diaphragm, a CR2032 button battery was assembled in a glove box filled with argon (H2O <0.1ppm; O2 <0.1ppm).
[0109] The constant current charge and discharge test was carried out using the CT2001A battery test system, with a voltage of 0.01-2.50 V. The rate performance test was carried out at 0.2 C, 0.5 C, 1.0 C and 2.0 C rates. Specifically, the capacity retention rate of the battery was tested after 100 cycles of charge and discharge at the corresponding current density. The ambient temperature of the electrochemical performance test was 30 ℃; the specific test results are shown in Table 1;
[0110] Table 1: Product performance test results
[0111]
[0112] It can be seen from the test results in Table 1 that the product obtained by the present invention has a beneficial rate performance and has a relatively beneficial capacity retention rate after long-term cycling.
[0113] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.
Claims
1. A method for preparing a biomass-based hard carbon negative electrode material, characterized in that: The specific preparation steps include: Starch gelatinization: After starch and water are mixed, gelatinization is performed to obtain gelatinized starch; Starch fermentation: The gelatinized starch and lactic acid bacteria are mixed and fermented to obtain fermented starch; Carbonization of starch: After drying the fermented starch to a moisture content of less than 3%, grinding it into powder and sieving it to obtain refined starch; Dispersing the refined starch in N-methylpyrrolidone, adding 6-8% of tetrabutyl titanate by weight of the refined starch, heating under reflux for more than 6 hours, filtering, washing and drying to obtain a precursor; The precursor is heated and reduced in a hydrogen atmosphere, and then heated to 1000-1200° C. in an inert atmosphere, and carbonized for 4-6 hours, and then cooled and discharged to obtain a biomass-based hard carbon negative electrode material.
2. The method for preparing a biomass-based hard carbon negative electrode material according to claim 1, characterized in that: The gelatinization of the starch also includes: Take starch and warm water at a temperature of 45-50°C in a mass ratio of 1:1, divide the warm water into 3 equal parts, stir and mix one part with starch, then add the second part of warm water, continue to stir and mix, then add the third part of warm water, continue to stir and mix, heat and gelatinize at a temperature of 100-105°C for 40-60 minutes, cool to room temperature, and discharge to obtain gelatinized starch.
3. The method for preparing a biomass-based hard carbon negative electrode material according to claim 1, characterized in that: The sieving is through a 800-1250 mesh sieve.
4. The method for preparing a biomass-based hard carbon negative electrode material according to claim 1, characterized in that: The carbonization of the starch also includes: Heat the precursor to 400-420°C at a rate of 1-3°C / min under a hydrogen atmosphere and reduce it for 2-3 hours; The hydrogen atmosphere is a mixed gas composed of hydrogen and nitrogen in a volume ratio of 1:5-1:
6.
5. The method for preparing a biomass-based hard carbon negative electrode material according to claim 4, characterized in that: The carbonization of the starch also includes: In an inert atmosphere, slowly heat to 1000-1200℃ at a rate of 0.8-1.5℃ / min, keep carbonized for 4-6h, cool to room temperature with the furnace, and discharge; Wherein, the inert atmosphere is selected from any one of argon or nitrogen.
6. The method for preparing a biomass-based hard carbon negative electrode material according to claim 2, characterized in that: The fermentation of the starch also includes: Add gelatinized starch into a fermentation tank, and inoculate lactic acid bacteria at an inoculation rate of 3-5%. Under the conditions that the initial pH of the material in the fermentation tank is 7.2-7.4 and the fermentation temperature is 30-35°C, fermentation is continued for 8-12 hours, and then the material is discharged and sterilized to obtain fermented starch.
7. The method for preparing a biomass-based hard carbon negative electrode material according to claim 1, characterized in that: The specific preparation steps also include: After the carbonization of the starch, an activation treatment is performed.
8. The method for preparing a biomass-based hard carbon negative electrode material according to claim 7, characterized in that: The specific preparation steps also include: Carbonization of starch: After drying the fermented starch to a moisture content of less than 3%, grinding it into powder and sieving it to obtain refined starch; Dispersing the refined starch in N-methylpyrrolidone, adding 6-8% of tetrabutyl titanate by weight of the refined starch, heating under reflux for more than 6 hours, filtering, washing and drying to obtain a precursor; The precursor is heated and reduced in a hydrogen atmosphere, and then heated to 1000-1200°C in an inert atmosphere, and carbonized for 4-6 hours, and then cooled and discharged to obtain carbonized starch; Product activation: The carbonized starch and a saturated sodium bicarbonate solution at a temperature of 50°C are mixed and dispersed evenly by ultrasonication, then cooled to 5-10°C and filtered. The filter cake is dried and transferred to a carbonization furnace. The temperature is raised to 250-270°C in a nitrogen atmosphere. After the reaction is kept warm for 2-3 hours, the product is cooled, discharged, washed and dried to complete the activation of the product.