A medium-strength, easy-to-form, high-temperature, corrosion-resistant, weldable titanium alloy for crane exhaust system and preparation method thereof

By developing medium-strength, easy-to-form, high-temperature, corrosion-resistant and weldable titanium alloy materials containing specific elemental components, the problem of insufficient cold-bending forming and welding performance of titanium alloys in the crane exhaust system in the existing technology has been solved, and the high-temperature stability of the material has been achieved. flexibility and complex pipeline processing capabilities, extending service life and reducing maintenance costs.

CN118389903BActive Publication Date: 2024-10-18CHONGQING QIRUI INTELLECTUAL PROPERTY SERVICE CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410852221.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-28
Publication Date
2024-10-18
Estimated Expiration
2044-06-28

AI Technical Summary

Technical Problem

Existing high-temperature titanium alloy materials cannot meet the cold bending performance and plastic deformation requirements of complex pipelines in crane exhaust systems. At the same time, their welding performance is also insufficient, resulting in shortened service life and increased maintenance costs in marine atmospheric environments.

Method used

Develop a medium-strength, easy-to-form, high-temperature corrosion-resistant and weldable titanium alloy material, containing Sn: 6.0% ~ 8.0%, Zr: 3.0% ~ 5.0%, Nb: 0.5% ~ 2.0%, Si: 0.1% ~ 0.4%, Er : 0.05% ~ 0.1%, O ≤ 0.06%, through specific hot processing and pickling processes, titanium alloy materials with excellent plasticity, cold bending performance and welding performance are prepared.

Benefits of technology

The prepared titanium alloy material shows good tensile strength, yield strength and elongation at both room temperature and high temperature. The cold bending performance is significantly improved, and the welding coefficient reaches 0.9-0.95. It is suitable for the processing and welding of complex pipelines and extends the Extended service life and reduced maintenance costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118389903B_ABST
    Figure CN118389903B_ABST
Patent Text Reader

Abstract

The present invention discloses a medium-strength, easy-to-form, high-temperature, corrosion-resistant and weldable titanium alloy for crane exhaust systems and a preparation method. The titanium alloy material of the present invention has good high-temperature strength, excellent plasticity, cold bending performance and welding performance. The material composition is Sn: 6.0% to 8.0%, Zr: 3.0% to 5.0%, Nb: 0.5% to 2.0%, Si: 0.1% to 0.4%, Er: 0.05% to 0.1%, O≤0.06%; the remainder is Ti and impurity elements. The tensile strength Rm at room temperature is ≥780MPa, the yield strength R p0.2 ≥710MPa, elongation A≥15%, cold bending performance α=180°, d=8t, qualified; tensile strength Rm≥520MPa at high temperature of 600℃, yield strength R p0.2 ≥450MPa, elongation A≥20%; corrosion rate<0.001 mm / a; welding coefficient≥0.9.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of titanium alloy materials for cranes, and in particular to a medium-strength, easy-to-form, high-temperature, corrosion-resistant and weldable titanium alloy for crane exhaust systems and a preparation method thereof. Background Art

[0002] Titanium and titanium alloys have excellent properties such as high specific strength, good plasticity and toughness, high temperature resistance, corrosion resistance and weldability, and are widely used in aerospace, marine engineering and other fields. The exhaust system of Haikou port cranes is severely corroded by the marine atmospheric environment, which greatly shortens its service life. If the crane exhaust pipe is made of titanium alloy, it can achieve full life cycle service. Considering the full use cycle, the use of titanium alloy materials for exhaust pipes can achieve the purpose of reducing the use cost and saving the time of replacing exhaust pipes.

[0003] For exhaust pipes, the requirements for the direction of the pipe are very high, which can be described as "nine bends and eighteen turns". However, the exhaust pipes made of conventional titanium alloys are not easy to bend due to the physical properties of titanium alloys themselves. If the pipes cannot be placed in the pipe bending machine for precise positioning and bending, interference will occur and become waste. In addition, the local operating temperature of the exhaust system can reach above 600℃. The titanium alloy used for exhaust pipes is not only required to have good high temperature resistance, but also excellent cold / hot forming performance, which puts higher requirements on its plasticity and cold bending forming performance.

[0004] At present, typical high-temperature titanium alloys at home and abroad mainly include Ti-1100 developed in the United States, IMI834 in the United Kingdom, BT36 developed in Russia, and Ti60, Ti600, TG6, Ti65 developed in my country. Their service temperature, alloy composition and basic mechanical properties are shown in Table 1. These high-temperature titanium alloys have excellent thermal stability and thermal strength, and have been widely used in the manufacture of high-temperature resistant parts of aircraft engines, such as blades, disks, etc. These application parts are mainly forgings or castings, and their high-temperature strength and high-temperature creep resistance are required to be high, but no subsequent cold forming processing is required, and their cold bending forming performance and plastic deformation ability are not required to be high. However, the pipeline structure of the crane exhaust system is complex, and the pipe bending machine needs to be precisely positioned and bent. The existing high-temperature alloys cannot meet the requirements of complex pipeline cold bending forming performance and plastic deformation ability. In addition, the intake and exhaust system uses titanium alloy materials, which requires a large number of welding connections, requiring titanium alloy materials to have good welding performance.

[0005] Existing high-temperature titanium alloys at home and abroad have good high-temperature resistance, but their plasticity, cold bending forming performance and welding performance cannot meet the needs of titanium alloy pipes for exhaust systems. Therefore, it is urgent to develop a titanium alloy material that is easy to form, high-temperature resistant, corrosion-resistant and weldable.

[0006] Table 1 Typical high temperature titanium alloys at home and abroad

[0007] Summary of the invention

[0008] Based on the fact that the high-temperature titanium alloy in the prior art does not have the cold-bending forming performance and plastic deformation ability of the complex pipelines of the exhaust system, the present invention provides a medium-strength, easy-to-form, high-temperature, corrosion-resistant and weldable titanium alloy for the crane exhaust system and a preparation method. The prepared titanium alloy material has good high-temperature strength and excellent plasticity, cold-bending performance and welding performance. The titanium alloy material prepared by the present invention can be made into seamless pipes or welded pipes, and the room temperature performance: tensile strength Rm≥780MPa, yield strength R p0.2 ≥710MPa, elongation A≥15%, cold bending performance α=180°, d=8t, qualified; 600℃ high temperature performance: tensile strength Rm≥520MPa, yield strength R p0.2 ≥450MPa, elongation A≥20%; welding performance: welding coefficient ≥0.9, with good welding process adaptability. The prepared titanium alloy material has good technical application and market prospects in the fields of marine atmospheric environment crane exhaust system and so on.

[0009] To achieve the purpose of the invention, the present invention adopts the following technical solutions:

[0010] A medium-strength, easy-to-form, high-temperature, corrosion-resistant, weldable titanium alloy material for a crane exhaust system. Expressed in mass percentage, the titanium alloy material comprises Sn: 6.0% to 8.0%, Zr: 3.0% to 5.0%, Nb: 0.5% to 2.0%, Si: 0.1% to 0.4%, Er: 0.05% to 0.1%, O≤0.06%; the remainder is Ti and unavoidable impurity elements, and the total content of impurity elements is less than 0.2%.

[0011] Furthermore, expressed in terms of mass percentage, the impurity elements C≤0.10%, N≤0.05%, and H≤0.01%.

[0012] Furthermore, after hot working, the titanium alloy material is a primary equiaxed α phase and an elongated α phase, the α volume fraction is more than 90%, and the average grain diameter is about 20μm-40μm.

[0013] Furthermore, the room temperature tensile strength of the titanium alloy material is 780-880MPa, the yield strength is 710-800MPa, the elongation is 15%-20%, and the cold bending performance is α=180°, d=8t continuous; the high temperature tensile strength at 600°C is 520-600MPa, the yield strength is 450-520MPa, and the elongation is 20%-28%; the corrosion rate is 0.00008-0.00021mm / a, and the welding coefficient is 0.9-0.95.

[0014] The present invention also provides a method for preparing the titanium alloy material, comprising the following steps:

[0015] Step 1: Consumable electrode production: Use a medium-strength, easy-to-form, high-temperature, corrosion-resistant, weldable titanium alloy material for a crane exhaust system as described in any one of claims 1-4, with Sn: 6.0% to 8.0%, Zr: 3.0% to 5.0%, Nb: 0.5 to 2.0%, Si: 0.1% to 0.4%, Er: 0.05% to 0.1%, O≤0.06%, and the remainder is special-grade sponge titanium, mix them evenly, press them into electrodes, and then weld them with consumable electrodes;

[0016] Step 2, ingot preparation: the consumable electrode obtained in step 1 is melted into an ingot by vacuum consumable arc melting technology, the pre-melting vacuum is ≤0.5Pa, the melting times are ≥2 times, the ingot surface is polished, and then non-destructive testing is performed and the riser is removed for blanking;

[0017] Step 3, blanking forging and machining: the bare ingot obtained in step 2 is heated to 1150°C and 1050°C for two rounds of blanking, and then forged at 980±30°C for 3-5 rounds, with a final forging temperature of ≥820°C. After processing, a titanium alloy cylindrical forging blank is obtained, and the outer skin is milled off to ensure that the surface is smooth and crack-free for perforation;

[0018] Step 4: Punching: Punch the titanium alloy forging billet in step 3 at the phase transition point T β Punch at a temperature of 5 to 100°C, then machine to keep the surface smooth and crack-free in preparation for hot rolling;

[0019] Step 5, hot rolling of pipe: the tube blank obtained in step 4 is subjected to the processes of tube rolling → titanium alloy tube reheating → sizing / reducing → heat treatment to obtain the tube blank of required specifications; the rolling temperature is 820℃~960℃, and the strain rate is controlled at ;

[0020] Step 6: Cold rolling of the tube: The tube obtained in step 5 is subjected to cold rolling / drawing → heat treatment → straightening → finishing → inspection, and finally a titanium alloy tube with a specification of DN (30~80)*(0.5~5) is obtained;

[0021] Step 7: Annealing of the pipe: annealing temperature is 550℃~700℃, annealing time is 30~60min;

[0022] Step 8: Pickling of pipes: The process is pickling → hot water washing → cold water washing → drying. The pickling process is 30%~40% HNO 3 +5%~7%HF+residue H 2 O, pickling temperature 50 ℃ ~ 80 ℃, time 5 ~ 10min, finally obtain the medium-strength, easy-to-form, high-temperature, corrosion-resistant and weldable titanium alloy material for the crane exhaust system. Beneficial Effects

[0023] Compared with the prior art, the most notable feature of the present invention is its excellent plasticity and cold bending properties, as well as good high temperature strength, especially its cold bending performance and plastic deformation capacity are higher than those of the existing high temperature titanium alloys. The specific positive and beneficial effects achieved are:

[0024] (1) The easily formed, high temperature, corrosion resistant and weldable titanium alloy material provided by the present invention is added with 0.05% to 0.1% Er element. The addition of Er element refines the original structure of the alloy, reduces the size of the grain boundary α phase, and reduces the thickness of the primary α phase layer, thereby inhibiting the brittle phase α 2 The precipitation and growth of Ti greatly improve the plasticity of the material (elongation A≥15% at room temperature, elongation A≥20% at 600℃) and cold bending performance (α=180°, d=8t, qualified). 5 Si 3 The particles are evenly distributed in the matrix, improving the comprehensive properties of the alloy.

[0025] (2) The easy-to-form, high-temperature, corrosion-resistant and weldable titanium alloy material provided by the present invention strictly controls the content of O. The lower O content in the titanium alloy can greatly improve the plasticity and cold bending properties. The O content of the special-grade sponge titanium is controlled at ≤0.06%. At the same time, Nd is added to the alloy to form rare earth oxides with O through internal oxidation, thereby reducing the oxygen content in the alloy and purifying the matrix. At the same time, Nd has a great influence on the performance of Ti 3 Sn inhibits the precipitation of brittle phase and improves the plasticity and thermal stability of the alloy.

[0026] (3) The easily formed, high temperature, corrosion resistant and weldable titanium alloy material provided by the present invention is added with Sn, Zr and Si elements. Sn and Zr are neutral elements and can be infinitely dissolved in the titanium alloy matrix, playing a role of solid solution strengthening and improving the thermal strength of the alloy. At the same time, the addition of Zr element has good welding performance, and can realize welding methods such as electron beam, laser, and manual TIG, with a welding coefficient ≥ 0.9. Si is an interstitial stabilizing element. Adding a small amount of Si can greatly improve the high temperature creep performance and oxidation resistance of titanium alloy. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 This is a metallographic structure photograph of Example 5 (Ti-7Sn-4Zr-0.5Nb-0.3Si-0.1Er-0.04O);

[0028] Figure 2 This is a scanning electron microscope photograph of the room temperature tensile fracture of Example 5 (Ti-7Sn-4Zr-0.5Nb-0.3Si-0.1Er-0.04O) alloy. DETAILED DESCRIPTION

[0029] The invention is further described below in conjunction with specific embodiments so that those skilled in the art can better understand the invention and implement it, but the embodiments are not intended to limit the invention.

[0030] A medium-strength, easy-to-form, high-temperature, corrosion-resistant, weldable titanium alloy material for a crane exhaust system. Expressed in percentage by mass, the titanium alloy pipe consists of the following components: Sn: 6.0% to 8.0%, Zr: 3.0% to 5.0%, Nb: 0.5% to 2.0%, Si: 0.1% to 0.4%, Er: 0.05% to 0.1%, O≤0.06%, the remainder being Ti and unavoidable impurity elements, such as C, H, N and the like, and the total content of impurity elements is less than 0.2%. After hot working, the titanium alloy material is a primary equiaxed α phase and an elongated α phase, with an α volume fraction of more than 90% and an average grain diameter of about 20μm-40μm; the room temperature tensile strength is 780-880MPa, the yield strength is 710-800MPa, the elongation is 15%-20%, and the cold bending performance is α=180°, d=8t continuous; the high temperature tensile strength at 600°C is 520-600MPa, the yield strength is 450-520MPa, and the elongation is 20%-28%; the corrosion rate is 0.00008-0.00021mm / a, and the welding coefficient is 0.90-0.95.

[0031] A medium-strength, easy-to-form, high-temperature, corrosion-resistant, weldable titanium alloy material for a crane exhaust system comprises the following steps:

[0032] Step 1: Consumable electrode production: Use a medium-strength, easy-to-form, high-temperature, corrosion-resistant, weldable titanium alloy material for a crane exhaust system as described in claim 1 or 2, according to the mass percentage of Sn: 6.0% to 8.0%, Zr: 3.0% to 5.0%, Nb: 0.5 to 2.0%, Si: 0.1% to 0.4%, Er: 0.05% to 0.1%, O≤0.06%, and the remainder is special-grade sponge titanium, mix them evenly, press them into electrodes, and then weld them with consumable electrodes;

[0033] Step 2, ingot preparation: the consumable electrode obtained in step 1 is melted into an ingot by vacuum consumable arc melting technology, the pre-melting vacuum is ≤0.5Pa, the melting times are ≥2 times, the ingot surface is turned, and then non-destructive testing is performed and the riser is removed for blanking;

[0034] Step 3, blanking forging and machining: the bare ingot obtained in step 2 is heated to 1150°C and 1050°C for two rounds of blanking, and then forged at 980±30°C for 3-5 rounds, with a final forging temperature of ≥820°C. After processing, a titanium alloy cylindrical forging blank is obtained, and the outer skin is milled off to ensure that the surface is smooth and crack-free for perforation;

[0035] Step 4: Punching: Punch the titanium alloy forging billet in step 3 at the phase transition point T β Punch at a temperature of 5 to 100°C, then machine to keep the surface smooth and crack-free in preparation for hot rolling;

[0036] Step 5, hot rolling of pipe: the tube blank obtained in step 4 is subjected to the processes of tube rolling → titanium alloy tube reheating → sizing / reducing → heat treatment to obtain the tube blank of required specifications; the rolling temperature is 820℃~960℃, and the strain rate is controlled at ;

[0037] Step 6: Cold rolling of the tube: The tube obtained in step 5 is subjected to cold rolling / drawing → heat treatment → straightening → finishing → inspection, and finally a titanium alloy tube with a specification of DN (30~80)*(0.5~5) is obtained;

[0038] Step 7: Annealing of the pipe: annealing temperature is 550℃~700℃, annealing time is 30~60min;

[0039] Step 8: Pickling of pipes: The process is pickling → hot water washing → cold water washing → drying. The pickling process is 30%~40% HNO 3 +5%~7%HF+residue H 2 O, pickling temperature 50℃~80℃, time 5~10min.

[0040] Example 1: Ti-8Sn-5Zr-2Nb-0.4Si-0.1Er-0.06O alloy

[0041] The raw materials were weighed according to the ingredients listed in Example 1, and the titanium alloy ingot was prepared by vacuum melting according to the composition ratio of 8.0 wt.% tin, 5.0 wt.% zirconium, 2.0 wt.% niobium, 0.4 wt.% silicon and 0.1 wt.% erbium and industrial special sponge titanium, and then the ingot was forged, pierced, rolled, annealed and pickled, wherein the annealing temperature was 550°C and the annealing time was 60 minutes; the pickling temperature was 50°C and the time was 5 minutes. The properties of the titanium alloy material are shown in Table 2.

[0042] Example 2: Ti-6Sn-3Zr-0.5Nb-0.1Si-0.05Er-0.05O alloy

[0043] The raw materials were weighed according to the ingredients listed in Example 2, and the titanium alloy ingot was prepared by vacuum melting according to the composition ratio of 6.0 wt.% tin, 3.0 wt.% zirconium, 0.5 wt.% niobium, 0.1 wt.% silicon and 0.05 wt.% erbium and industrial special sponge titanium, and then the ingot was forged, perforated, rolled, annealed and pickled, wherein the annealing temperature was 700°C and the annealing time was 60 min; the pickling temperature was 80°C and the time was 10 min. The properties of the titanium alloy material are shown in Table 2.

[0044] Example 3: Ti-8Sn-4Zr-2Nb-0.4Si-0.05Er-0.05O alloy

[0045] The raw materials were weighed according to the ingredients listed in Example 3, and the titanium alloy ingot was prepared by vacuum melting according to the composition ratio of 8.0 wt.% tin, 4.0 wt.% zirconium, 2.0 wt.% niobium, 0.4 wt.% silicon and 0.05 wt.% erbium and industrial special sponge titanium, and then the ingot was forged, pierced, rolled, annealed and pickled, wherein the annealing temperature was 550°C and the annealing time was 30 minutes; the pickling temperature was 70°C and the time was 7 minutes. The properties of the titanium alloy material are shown in Table 2.

[0046] Example 4: Ti-8Sn-4Zr-1Nb-0.2Si-0.1Er-0.06O alloy

[0047] The raw materials were weighed according to the ingredients listed in Example 4, and the titanium alloy ingot was prepared by vacuum melting according to the composition ratio of 8.0 wt.% tin, 4.0 wt.% zirconium, 1.0 wt.% niobium, 0.2 wt.% silicon and 0.1 wt.% erbium and industrial special sponge titanium, and then the ingot was forged, pierced, rolled, annealed and pickled, wherein the annealing temperature was 650°C and the annealing time was 45 minutes; the pickling temperature was 60°C and the time was 8 minutes. The properties of the titanium alloy material are shown in Table 2.

[0048] Example 5: Ti-7Sn-4Zr-1Nb-0.3Si-0.1Er-0.04O alloy

[0049] The raw materials were weighed according to the ingredients listed in Example 5, and the titanium alloy ingot was prepared by vacuum melting according to the composition ratio of 7.0 wt.% tin, 4.0 wt.% zirconium, 1.0 wt.% niobium, 0.3 wt.% silicon and 0.1 wt.% erbium and industrial special sponge titanium, and then the ingot was forged, pierced, rolled, annealed and pickled, wherein the annealing temperature was 600°C and the annealing time was 40min; the pickling temperature was 60°C and the time was 6min. The properties of the titanium alloy material are shown in Table 2.

[0050] Example 6: Ti-8Sn-3Zr-1Nb-0.1Si-0.1Er-0.05O alloy

[0051] The raw materials were weighed according to the ingredients listed in Example 6, and the titanium alloy ingot was prepared by vacuum melting according to the composition ratio of 8.0 wt.% tin, 3.0 wt.% zirconium, 1.0 wt.% niobium, 0.1 wt.% silicon and 0.1 wt.% erbium and industrial special sponge titanium, and then the ingot was forged, pierced, rolled, annealed and pickled, wherein the annealing temperature was 650°C and the annealing time was 30 minutes; the pickling temperature was 70°C and the time was 10 minutes. The properties of the titanium alloy material are shown in Table 2.

[0052] Example 7: Ti-7Sn-3Zr-0.5Nb-0.1Si-0.1Er-0.06O alloy

[0053] The raw materials were weighed according to the ingredients listed in Example 7, and the titanium alloy ingot was prepared by vacuum melting according to the composition ratio of 7.0 wt.% tin, 3.0 wt.% zirconium, 0.5 wt.% niobium, 0.1 wt.% silicon and 0.1 wt.% erbium and industrial special sponge titanium, and then the ingot was forged, pierced, rolled, annealed and pickled, wherein the annealing temperature was 550°C and the annealing time was 60 minutes; the pickling temperature was 80°C and the time was 5 minutes. The properties of the titanium alloy material are shown in Table 2.

[0054] Example 8: Ti-7Sn-3.5Zr-2Nb-0.2Si-0.08Er-0.05O alloy

[0055] The raw materials were weighed according to the ingredients listed in Example 8, and the titanium alloy ingot was prepared by vacuum melting according to the composition ratio of 7.0 wt.% tin, 3.5 wt.% zirconium, 2.0 wt.% niobium, 0.2 wt.% silicon and 0.08 wt.% erbium and industrial special sponge titanium, and then the ingot was forged, pierced, rolled, annealed and pickled, wherein the annealing temperature was 650°C and the annealing time was 50min; the pickling temperature was 60°C and the time was 8min. The properties of the titanium alloy material are shown in Table 2.

[0056] Table 2 Chemical composition and mechanical properties of medium-strength and easy-to-form high-temperature titanium alloy for exhaust system

[0057]

[0058] The chemical composition of the alloys in Table 2 was tested and analyzed using the national standard GB / T 4698 "Chemical Analysis Methods for Sponge Titanium, Titanium and Titanium Alloys"; room temperature and high temperature tensile tests were carried out in accordance with GB / T228 "Room Temperature Tensile Test Methods for Metallic Materials", and all test results are the average values ​​of three specimens; the cold bending performance of the cold bending specimens was tested using GB / T232 "Bending Test Methods for Metallic Materials"; the corrosion performance test used a natural seawater environment exposure corrosion test, the test environment was 60°C natural seawater, the test period was 60 days, and the corrosion rate of the alloy was obtained by weight loss measurement and corrosion rate calculation; the welding performance was performed using manual TIG welding, and its welding coefficient was calculated.

[0059] As shown in Table 2, Example 1 (Ti-8Sn-5Zr-5Nb-0.4Si-0.1Er-0.06O) has the highest tensile strength (864MPa) and yield strength (782MPa), but the lowest elongation (room temperature elongation 16.5%, 600℃ high temperature elongation 21.5%); while Example 2 (Ti-6Sn-3Zr-0.5Nb-0.1Si-0.05Er-0.05O) has the lowest tensile strength (791MPa) and yield strength (732MPa), but the highest elongation (room temperature elongation 19.5%, 600℃ high temperature elongation 26.0%). This is because the addition amounts of Sn, Zr, Nb, Si and Er elements in Example 1 are all at the upper limit of the composition range, the content of alloy elements added is high, and the solid solution strengthening effect is strong, resulting in high strength and poor plasticity. In Example 2, on the contrary, the addition amounts of Sn, Zr, Nb, Si and Er elements are at the lower limit of the alloy composition, and the strength is low but the plasticity is high.

[0060] In Example 5 (Ti-7Sn-4Zr-1Nb-0.3Si-0.1Er-0.04O), the alloy composition elements are optimized, the strength and plasticity are well matched, and the comprehensive performance is the best. Figure 1 This is a metallographic structure photograph of Example 5 (Ti-7Sn-4Zr-1Nb-0.3Si-0.1Er-0.03O). The microstructures are primary equiaxed α phase and elongated α phase. The elongated α is distributed along the pressure processing direction. The proportion of primary α phase is very high. Software analysis shows that the volume fraction of the α phase is 92%, and the average grain diameter is about 28μm.

[0061] Figure 2This is a scanning electron microscope photo of the room temperature tensile fracture of Example 5 (Ti-7Sn-4Zr-1Nb-0.3Si-0.1Er-0.04O) alloy. The tensile fracture characteristics of the sample are mainly ductile fracture, with a large fiber area, small dimples distributed in the large dimples, darker regional color, and larger surface undulations, such as ridges, indicating that the crack extension in this area is accompanied by large plastic deformation, and has excellent plasticity. This is because the alloy adds 0.1 wt.% of Er element, which refines the original structure of the alloy, inhibits the precipitation and growth of the brittle phase α, and reduces the size of the grain boundary α phase. The average grain diameter is about 28μm; special sponge titanium is used, the content of O element is strictly controlled, and 1.0 wt.% of Nd element is added to the alloy, which forms rare earth oxides with O element through internal oxidation, reduces the oxygen content in the alloy, purifies the matrix, and the O element content in the alloy is only 0.04 wt.%. In addition, Nd element has a great influence on Ti 3 Sn brittle phase precipitation inhibits the Ti 5 Si 3 The particles are evenly distributed in the matrix, greatly improving the plasticity and cold bending properties. The room temperature elongation A of the alloy is 18.5%, and the cold bending performance α=180°, d=8t, is continuous; the elongation at a high temperature of 600°C is 23.5%. The plasticity and cold bending properties of the alloy are much higher than those of the existing typical high-temperature titanium alloy materials at home and abroad in Table 1.

[0062] In addition, the alloy of Example 5 (Ti-7Sn-4Zr-1Nb-0.3Si-0.1Er-0.04O) adds 7 wt.% Sn, 4 wt.% Zr and 0.3 wt.% Si. Sn and Zr are neutral elements and can be infinitely dissolved in the titanium alloy matrix, playing a role of solid solution strengthening and improving the thermal strength of the alloy. At the same time, Si is an interstitial stabilizing element. Adding a small amount of Si can greatly improve the high-temperature creep performance and oxidation resistance of the titanium alloy. The alloy has a high-temperature tensile strength of 583MPa at 600°C and a yield strength of 492MPa. The addition of Zr element has good welding performance and can realize welding methods such as electron beam, laser, and manual TIG. The welding coefficient of the alloy is calculated to be about 0.93.

Claims

1. A medium-strength, easy-to-form, high-temperature, corrosion-resistant, weldable titanium alloy material for crane exhaust systems, characterized in that: The method for preparing the titanium alloy material comprises the following steps: Step 1: Consumable electrode production: according to the mass percentage of Sn: 6.0% ~ 8.0%, Zr: 3.0% ~ 5.0%, Nb: 0.5 ~ 2.0%, Si: 0.1% ~ 0.4%, Er: 0.05% ~ 0.1%, O ≤ 0.06% and the balance is special sponge titanium, mix them evenly, press them into electrodes, and then weld the consumable electrodes; Step 2, ingot preparation: the consumable electrode obtained in step 1 is melted into an ingot by vacuum consumable arc melting technology, the pre-melting vacuum is ≤0.5Pa, the melting times are ≥2 times, the ingot surface is polished, and then non-destructive testing is performed and the riser is removed for blanking; Step 3, blanking forging and machining: the bare ingot obtained in step 2 is heated to 1150°C and 1050°C for two rounds of blanking, and then forged at 980±30°C for 3-5 rounds, with a final forging temperature of ≥820°C. After processing, a titanium alloy cylindrical forging blank is obtained, and the outer skin is milled off to ensure that the surface is smooth and crack-free for perforation; Step 4: Punching: Punch the titanium alloy forging billet in step 3 at the phase transition point T β Punch at a temperature of 5 to 100°C, then machine to keep the surface smooth and crack-free in preparation for hot rolling; Step 5: Hot rolling of pipes: The peeled and pierced pipe blanks obtained in step 4 are subjected to pipe rolling → titanium alloy pipe reheating → sizing / reducing → heat treatment to obtain pipe blanks of required specifications; the rolling temperature is 820℃~960℃, and the strain rate is controlled at 0.01~0.1s -1 ; Step 6: Cold rolling of the tube: The tube obtained in step 5 is subjected to cold rolling / drawing → heat treatment → straightening → finishing → inspection, and finally a titanium alloy tube with a specification of DN (30~80)*(0.5~5) is obtained; Step 7: Annealing of the pipe: annealing temperature is 550℃~700℃, annealing time is 30~60min; Step 8, pipe pickling: the process is pickling → hot water washing → cold water washing → drying, the pickling process system is 30%~40% HNO3+5%~7% HF+ residual H2O, the pickling temperature is 50℃~80℃, the time is 5~10min, and finally the medium-strength, easy-to-form, high-temperature, corrosion-resistant and weldable titanium alloy material for the crane exhaust system is obtained; expressed in mass percentage, the composition of the titanium alloy material is Sn: 6.0%~8.0%, Zr: 3.0%~5.0%, Nb: 0.5%~2.0%, Si: 0.1%~0.4%, Er: 0.05%~0.1%, O≤0.06%; the balance is Ti and unavoidable impurity elements, and the total content of impurity elements is less than 0.2%.

2. A medium-strength, easy-to-form, high-temperature, corrosion-resistant, weldable titanium alloy material for a crane exhaust system as claimed in claim 1, characterized in that: Expressed as mass percentage, the impurity elements C≤0.10%, N≤0.05%, and H≤0.01%.

3. The medium-strength, easy-to-form, high-temperature, corrosion-resistant, weldable titanium alloy material for a crane exhaust system as claimed in claim 1, characterized in that: The titanium alloy material is a primary equiaxed α phase and an elongated α phase after hot working, the α volume fraction is more than 90%, and the average grain diameter is 20 μm-40 μm.

4. The medium-strength, easy-to-form, high-temperature, corrosion-resistant, weldable titanium alloy material for a crane exhaust system as claimed in claim 1, characterized in that: The room temperature tensile strength of the titanium alloy material is 780-880MPa, the yield strength is 710-800MPa, the elongation is 15%-20%, and the cold bending performance is α=180°, d=8t continuous; the high temperature tensile strength at 600°C is 520-600MPa, the yield strength is 450-520MPa, and the elongation is 20%-28%; the corrosion rate is 0.00008-0.00021mm / a, and the welding coefficient is 0.9-0.95.

Citation Information

Patent Citations

  • Titanium alloy with thin sheet layer microstructure and manufacturing method thereof

    CN101967581A

  • High-temperature titanium alloy and preparation method thereof

    CN113355560A

  • Heat-resistant titanium alloy