Two-dimensional polymer film material and preparation method thereof
The two-dimensional polymer film is formed on the substrate through sputtering deposition and evaporation deposition, which solves the problem of low preparation efficiency of two-dimensional polymer film materials in the existing technology, and achieves efficient large-area preparation and high reaction rate.
Patent Information
- Application Number
- CN202410833441.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-26
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-06-26
AI Technical Summary
It is difficult to efficiently prepare two-dimensional polymer film materials with a thickness of nanometers using existing technology, especially in terms of large-area preparation and reaction efficiency.
Sputtering deposition and evaporation deposition methods are used to deposit organic monomer materials on the substrate. The high-kinetic energy sputtering material is fully mixed and contacted with the gaseous evaporation material to promote the polymerization reaction and form a two-dimensional polymer film.
It significantly improves the reaction efficiency of organic monomer materials, realizes efficient large-area preparation of two-dimensional polymer films, and is suitable for industrial production.
Smart Images

Figure CN118389997B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of film coating technology, and in particular to a two-dimensional polymer film material and a preparation method thereof. Background Art
[0002] The molecules of traditional polymer materials are linear, and they can be prepared into specific three-dimensional structures through processing techniques such as injection molding, but it is difficult to form single-layer or few-layer two-dimensional materials with a thickness of nanometers. Two-dimensional polymers refer to lamellar polymers with covalent bonds connected in two dimensions and a thickness of nanometers. Compared with traditional linear polymer materials, two-dimensional polymers have significantly larger specific surface areas and have broad application prospects in many fields.
[0003] At present, the preparation methods of two-dimensional polymers can be mainly divided into stripping method, interfacial polymerization method and solution polymerization method. Among them, the stripping method is to use micromechanical force or other methods to destroy the van der Waals force between layers in the bulk material to obtain a few-layer structure, but the stripping method is not only inefficient, but also easy to destroy the molecular structure of the polymer material itself. Interfacial polymerization method refers to limiting the polymerization reaction area of the polymer by the interface, so that the polymerization reaction occurs only at the interface, thereby forming a layered two-dimensional polymer. Solution polymerization method refers to making a specific monomer material directly react in a solvent to form a layered two-dimensional polymer. Although the process of solution polymerization method is relatively simple, it is necessary to place the monomer material in an organic solvent and perform long-term violent vibration to promote the full progress of the reaction, and it has a problem of low reaction efficiency and is not suitable for large-scale preparation. Summary of the invention
[0004] Based on this, it is necessary to provide a method for preparing a two-dimensional polymer thin film material that is suitable for large-area preparation and can improve preparation efficiency in response to the problems in the above-mentioned background technology.
[0005] In a first aspect, some embodiments of the present disclosure provide a method for preparing a two-dimensional polymer thin film material, which comprises the following steps: sputtering depositing a first organic monomer material on a substrate, and evaporating depositing a second organic monomer material on the substrate, and polymerizing the first organic monomer material and the second organic monomer material on the substrate to form a two-dimensional polymer.
[0006] In some embodiments of the present disclosure, before depositing the first organic monomer material and the second organic monomer material, a step of preparing a two-dimensional material layer on the substrate is also included; the first organic monomer material and the second organic monomer material are both deposited on the two-dimensional material layer.
[0007] In some embodiments of the present disclosure, the material of the two-dimensional material layer includes graphene oxide, and the material of the substrate includes a metal capable of catalyzing the growth of the two-dimensional material layer.
[0008] In some embodiments of the present disclosure, after forming the two-dimensional polymer, the following steps are further included:
[0009] A fixing material is coated on a side of the two-dimensional polymer film away from the substrate and cured to form a fixing layer, wherein the fixing material comprises silicone oil.
[0010] In some embodiments of the present disclosure, the silicone oil in the fixing material is selected from one or more of vinyl silicone oil and hydrogen-containing silicone oil.
[0011] In some embodiments of the present disclosure, the thickness of the fixed layer formed is 0.5 mm to 5 mm.
[0012] In some embodiments of the present disclosure, the first organic monomer material is selected from one of melamine and trimesoyl chloride, and the second organic monomer material is selected from the other of melamine and trimesoyl chloride.
[0013] In some embodiments of the present disclosure, in the step of sputtering and depositing the first organic monomer material, the sputtering power is controlled to be 100W to 500W;
[0014] In the step of evaporating and depositing the second organic monomer material, an organic evaporation source is used to evaporate and deposit the second organic monomer material, and the evaporation temperature of the organic evaporation source is controlled to be 50° C. to 200° C.
[0015] In some embodiments of the present disclosure, the thickness of the formed two-dimensional polymer is 1 nm to 100 nm.
[0016] Furthermore, the present disclosure also provides a two-dimensional polymer thin film material, which is prepared by the preparation method of the two-dimensional polymer thin film material described in any of the above embodiments.
[0017] In the preparation method of the two-dimensional polymer thin film material, a first organic monomer material is deposited on a substrate by sputtering deposition, and a second organic monomer material is deposited on a substrate by evaporation deposition. The sputtered first organic monomer material has a high kinetic energy, and the evaporated second organic monomer material is in a gaseous state and can diffuse and be evenly distributed on the substrate, which enables the first organic monomer material to be fully mixed with the second organic monomer material and violently collide and contact to promote the reaction. Compared with the traditional solution polymerization method, the preparation method can significantly improve the reaction efficiency of the first organic monomer material and the second organic monomer material, and the preparation method adopts the processes of sputtering deposition and evaporation deposition, which can realize the large-area preparation of the two-dimensional polymer thin film material.
[0018] The above description is only an overview of the technical solution of the present invention. In order to more clearly understand the technical means of the present invention and implement it according to the contents of the specification, the following is a detailed description of the preferred embodiments of the present invention in conjunction with the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] In order to more clearly illustrate the technical solutions of the embodiments of the present disclosure, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present disclosure. For ordinary technicians in this field, drawings of other embodiments can be obtained based on these drawings without creative work.
[0020] Figure 1 A schematic diagram of the steps of a method for preparing a two-dimensional polymer film material;
[0021] Figure 2 A schematic diagram of the structure for preparing a two-dimensional material layer on a substrate;
[0022] Figure 3 For Figure 2 Schematic diagram of the structure of a two-dimensional polymer film formed on the basis of the structure shown;
[0023] Figure 4 For Figure 3 Schematic diagram of the structure of forming a fixed layer based on the structure shown.
[0024] The reference numerals and their meanings are as follows:
[0025] 110, substrate; 120, two-dimensional material layer; 130, two-dimensional polymer; 140, fixed layer. DETAILED DESCRIPTION
[0026] To facilitate understanding of the present invention, a more comprehensive description of the present invention is provided below. The preferred embodiments of the present invention are given herein. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the content of the present invention more thorough and comprehensive.
[0027] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this document pertains. The terms used herein in the specification of this document are only for describing specific embodiments and are not intended to limit this document.
[0028] It should be understood that when an element or layer is referred to as being "on, "adjacent to, "connected to, or "coupled to" another element or layer, it may be directly on, adjacent to, connected to, or coupled to the other element or layer, or there may be intervening elements or layers. In contrast, when an element is referred to as being "directly on, "directly adjacent to, "directly connected to, or "directly coupled to" another element or layer, there may be no intervening elements or layers. It should be understood that although the terms first, second, third, etc. may be used to describe various elements, components, regions, layers, and / or portions, these elements, components, regions, layers, and / or portions should not be limited by these terms. These terms are merely used to distinguish one element, component, region, layer, or portion from another element, component, region, layer, or portion.
[0029] Spatially relative terms such as "under," "beneath," "below," "under," "above," "above," and the like may be used herein for ease of description to describe the relationship of one element or feature to other elements or features. It should be understood that the spatially relative terms are intended to also include different orientations of the device in use and operation. For example, if the device in the accompanying drawings is flipped, then the elements or features described as "under other elements" or "under" or "under" will be oriented as "over" the other elements or features. Thus, the exemplary terms "under" and "under" may include both upper and lower orientations. The device may be otherwise oriented (e.g., rotated 90 degrees or other orientations) and the spatial descriptors used may be interpreted accordingly.
[0030] The purpose of the terms used herein is only to describe specific embodiments and is not intended to be a limitation of the present disclosure. When used herein, the singular forms "a", "an" and "the" are also intended to include plural forms, unless the context clearly indicates otherwise. It should also be understood that the terms "consisting of" and / or "comprising", when used in this specification, determine the presence of features, integers, steps, operations, elements and / or parts, but do not exclude the presence or addition of one or more other features, integers, steps, operations, elements, parts and / or groups. When used herein, the term "and / or" includes any and all combinations of the relevant listed items.
[0031] The present disclosure provides a method for preparing a two-dimensional polymer thin film material, which includes the following steps: sputtering and depositing a first organic monomer material on a substrate, and evaporating and depositing a second organic monomer material on the substrate, and polymerizing the first organic monomer material and the second organic monomer material to form a two-dimensional polymer thin film.
[0032] In the preparation method of the two-dimensional polymer thin film material, a first organic monomer material is deposited on a substrate by sputtering deposition, and a second organic monomer material is deposited on a substrate by evaporation deposition. The sputtered first organic monomer material has a high kinetic energy, and the evaporated second organic monomer material is in a gaseous state and can diffuse and be evenly distributed on the substrate, which enables the first organic monomer material to be fully mixed with the second organic monomer material and violently collide and contact to promote the reaction. Compared with the traditional solution polymerization method, the preparation method can significantly improve the reaction efficiency of the first organic monomer material and the second organic monomer material, and the preparation method adopts the processes of sputtering deposition and evaporation deposition, which can realize the large-area preparation of the two-dimensional polymer thin film material.
[0033] An embodiment of the present disclosure provides a more specific method for preparing a two-dimensional polymer film material. Figure 1 Schematic diagram of the steps of the preparation method. Figure 1 As shown, the method for preparing the two-dimensional polymer film material includes steps S1 to S3, which are specifically as follows.
[0034] Step S1 , providing a substrate 110 , and preparing a two-dimensional material layer 120 on the substrate 110 .
[0035] It can be understood that the substrate 110 is used to carry the two-dimensional polymer to be prepared, and the two-dimensional polymer can be directly prepared on the material or device that needs to be composited with the two-dimensional polymer. The material of the substrate 110 can be selected according to actual needs. For example, the material of the substrate 110 can include one or more of metal, glass, ceramic and quartz.
[0036] Figure 2 Schematic diagram of the structure of preparing a two-dimensional material layer 120 on a substrate 110. The two-dimensional material layer 120 has a similar planar structure, which has a certain guiding effect on the polymerization and growth direction of the first organic monomer material and the second organic monomer material, and can improve the flatness of the formed two-dimensional polymer, and obtain a two-dimensional planar two-dimensional polymer 130 with good quality.
[0037] Reference Figure 2 As shown, as some examples of this embodiment, the two-dimensional material layer 120 can be prepared on one side surface of the substrate 110. However, in other examples, the two-dimensional material layer 120 can also be prepared on two opposite sides of the substrate 110.
[0038] As some examples of this embodiment, the material of the two-dimensional material layer 120 can be selected from one or more of graphene and hexagonal boron nitride. Graphene has good compatibility with the molecular structure of the two-dimensional polymer film material. In this example, the material of the two-dimensional material layer 120 can include graphene, such as graphene oxide. There are oxygen-containing functional groups such as hydroxyl and carboxyl groups on the surface of carbon atoms in graphene oxide, which will be beneficial to further reinforce the formed two-dimensional polymer 130 in the subsequent preparation process.
[0039] As some examples of this embodiment, the two-dimensional material layer 120 is grown based on the substrate 110, and the substrate 110 may include a catalytic material that can be used to catalytically prepare the two-dimensional material layer 120. It can be understood that the two-dimensional material layer 120 can be directly grown on the substrate to form an integrated structure with the substrate, which can enhance the stable adhesion between the two-dimensional material layer 120 and the substrate, and ensure the stable connection between the two-dimensional material layer 120 and the substrate, which is conducive to further improving the bonding strength between the subsequently prepared two-dimensional polymer 130 and the substrate 110.
[0040] In this example, the material of the two-dimensional material layer 120 includes graphene oxide, and the substrate 110 may include one or more of iron, nickel and copper. The graphene material can be deposited on the substrate by, for example, physical vapor deposition or chemical vapor deposition. Furthermore, by oxidizing the deposited graphene material, graphene oxide having oxygen-containing functional groups on the surface can be obtained. Accordingly, the substrate 110 can be selected from a metal material including one or more of iron, nickel and copper, such as stainless steel. Alternatively, the substrate 110 may also include a substrate and a metal catalyst layer located on the substrate, wherein the metal catalyst layer may contain one or more of iron, nickel and copper, and the substrate may be other materials to be plated.
[0041] In step S2 , a first organic monomer material is sputter-deposited on the substrate 110 , and a second organic monomer material is evaporated and deposited on the substrate 110 , so that the first organic monomer material and the second organic monomer material are polymerized to form a two-dimensional polymer 130 .
[0042] Figure 3 For Figure 2 The schematic diagram of the structure of the two-dimensional polymer 130 is shown. Figure 3 As shown, the two-dimensional polymer 130 can be grown based on the two-dimensional material layer 120 and stacked on a side of the two-dimensional material layer 120 away from the substrate 110 .
[0043] In this embodiment, the first organic monomer material and the second organic monomer material are both deposited on the two-dimensional material layer 120 ; further, the first organic monomer material and the second organic monomer material may be in direct contact with the two-dimensional material layer 120 .
[0044] It can be understood that in this embodiment, the first organic monomer material and the second organic monomer material should be selected from two monomer materials that can undergo polymerization reaction along a planar direction, so that they can form a two-dimensional two-dimensional polymer 130 after polymerization reaction. The first organic monomer material and the second organic monomer material can be a known monomer combination that can form a two-dimensional polymer 130 material. The first organic monomer material and the second organic monomer material can be the same substance or different substances.
[0045] The traditional solution polymerization method requires the use of an organic solvent and also requires the use of a violent oscillation method to ensure the contact polymerization reaction between the monomer materials, but it still requires a long reaction time. In this embodiment, the gas environment of the second organic monomer material can be created on the surface of the substrate 110 by evaporation, thereby ensuring that it is fully mixed and contacted with the first organic monomer material without the need for an organic solvent. At the same time, the sputtering method can enable the molecules of the first organic monomer material to move to the substrate 110 with greater kinetic energy, and the sputtered first organic monomer material can provide energy for the polymerization reaction, thereby promoting the continuous reaction between the two. Therefore, this process can greatly increase the reaction speed of the first organic monomer material and the second organic monomer material while ensuring that the reaction of the two proceeds by fully mixing and contacting the first organic monomer and the second organic monomer and providing a greater reaction driving energy.
[0046] The preparation process is completed in a sputtering chamber, and the two-dimensional polymer 130 can be prepared directly on the substrate 110, and the step of transferring the two-dimensional polymer 130 can be saved. In addition, the traditional solution polymerization method can only produce a single area-prioritized two-dimensional polymer 130, while the two-dimensional polymer 130 prepared on the substrate 110 also has the advantages of a larger area and suitable for continuous preparation, and is therefore more suitable for industrial production.
[0047] As some examples of this embodiment, the first organic monomer material may be one of melamine and trimesoyl chloride, and the second organic monomer material may be the other of melamine and trimesoyl chloride. Melamine has three amine groups in its molecular structure, and trimesoyl chloride has three acyl chloride groups in its molecular structure. Melamine and trimesoyl chloride can be polymerized along a planar direction to form a polymer. In other examples, isophthaloyl chloride may be used instead of trimesoyl chloride as a reactant. However, compared to isophthaloyl chloride, the two-dimensional polymer 130 formed when trimesoyl chloride is used as a reactant is denser and has better performance.
[0048] Furthermore, in this embodiment, the first organic monomer material is selected from melamine, and the second organic monomer material is selected from trimesoyl chloride. The melting point of melamine is about 250°C, and the melting point of trimesoyl chloride is about 36.3°C. The trimesoyl chloride is deposited by organic evaporation.
[0049] As some examples of this embodiment, in the step of sputtering and depositing the first organic monomer material, the sputtering power can be controlled to be 100W-500W. For example, the sputtering power can be controlled to be 100W, 150W, 200W, 250W, 300W, 350W, 400W, 450W, 500W, or the sputtering power can also be in the range between any two of the above powers. Controlling the sputtering power to be 100W-500W allows the first organic monomer material to have a more appropriate sputtering rate, which can improve the quality of the two-dimensional polymer 130.
[0050] As some examples of this embodiment, in the step of evaporating and depositing the second organic monomer material, an organic evaporation source is used to evaporate and deposit the second organic monomer material. The organic evaporation source is a device that can evaporate an organic material in a coating chamber. The organic evaporation source and the sputtering target are arranged in the same coating chamber, that is, sputtering deposition and evaporation deposition can be achieved simultaneously.
[0051] As some examples of this embodiment, in the step of evaporating and depositing the second organic monomer material, the evaporation temperature of the organic evaporation source can be controlled to be 50°C to 200°C. For example, the evaporation temperature can be controlled to be 50°C, 75°C, 100°C, 125°C, 150°C, 175°C, 200°C, or the evaporation temperature can also be in the range between any two of the above temperatures. Controlling the evaporation temperature to be 50°C to 200°C can increase the reaction environment temperature between the second organic monomer material and the first organic monomer material, and can also minimize the morphological change of the two-dimensional polymer 130 caused by excessive temperature.
[0052] As some examples of this embodiment, the second organic monomer material has a boiling point below 200° C. corresponding to the evaporation temperature.
[0053] It is understandable that some combinations of the first organic monomer material and the second organic monomer material require an initiator to enable the polymerization reaction to proceed. In this case, the initiator can be pre-set on the substrate 110 or deposited on the substrate 110 by evaporation to ensure the polymerization reaction.
[0054] As some examples of this embodiment, in the step of depositing the first organic monomer material and the second organic monomer material, the deposition time may be controlled according to the thickness of the two-dimensional polymer 130 to be prepared.
[0055] As some examples of this embodiment, the thickness of the two-dimensional polymer 130 may be 1 nm to 100 nm. For example, the thickness of the two-dimensional polymer 130 may be 1 nm, 2 nm, 5 nm, 10 nm, 20 nm, 30 nm, 50 nm, 70 nm, 80 nm, 100 nm, or the thickness of the two-dimensional polymer 130 may also be in the range between any two of the above thicknesses.
[0056] In this embodiment, since the first organic monomer material and the second organic monomer material can react at a higher rate, the required deposition time is also shorter. As some examples of this embodiment, the deposition time can be controlled to be 1 min to 10 min. For example, the deposition time can be controlled to be 1 min, 2 min, 3 min, 4 min, 5 min, 6 min, 7 min, 8 min, 9 min, 10 min, or the deposition time can also be in the range between any two of the above times.
[0057] Step S3 , coating a fixing material on the side of the two-dimensional polymer 130 away from the substrate 110 and curing the fixing material to form a fixing layer 140 .
[0058] Figure 4 For Figure 3 A schematic diagram of a structure in which a fixed layer 140 is formed on the basis of the structure shown in FIG. Figure 4 As shown, the fixed layer 140 is disposed on a surface of the two-dimensional polymer 130 that is away from the substrate 110 .
[0059] In this embodiment, the fixing material includes silicone oil. It is understood that the silicone oil is liquid before curing, and the liquid silicone oil can be cross-linked and cured under the action of a catalyst to form a solid structure. As some examples of this embodiment, the catalyst for curing the fixing material can be a platinum-containing catalyst.
[0060] As some examples of this embodiment, the method of coating the fixing material on the side of the two-dimensional polymer 130 away from the substrate 110 may be spray coating, blade coating or spin coating.
[0061] As some examples of this embodiment, in the step of solidifying the fixing material, the solidification temperature may be controlled to be below 100° C., thereby avoiding the negative influence of excessively high temperature on the two-dimensional polymer 130 .
[0062] As some examples of this embodiment, the silicone oil in the fixing material is selected from one or more of vinyl silicone oil and hydrogen-containing silicone oil.
[0063] As some examples of this embodiment, the thickness of the fixed layer 140 may be 0.5 mm to 5 mm. For example, the thickness of the fixed layer 140 may be 0.5 mm, 1 mm, 1.5 mm, 2 mm, 2.5 mm, 3 mm, 3.5 mm, 4 mm, 4.5 mm, 5 mm, or the thickness of the fixed layer 140 may be between any two of the above thicknesses.
[0064] In this embodiment, there may be certain gaps or vacancies in the two-dimensional polymer 130. Silicone oil has certain adhesion, and the oxygen atoms in the silicone oil can form hydrogen bonds with the surface of the graphene oxide below the two-dimensional polymer 130, so that the formed fixed layer 140 has a strong binding force with the previously formed graphene oxide material, and the two have a strong fixing effect on the two-dimensional polymer 130 located in the middle, thereby ensuring the structural stability of the two-dimensional polymer 130. In addition, the silicone oil in the fixed layer 140 is also resistant to water, oxygen and corrosion, and can also be used as a packaging material for the two-dimensional polymer 130 to increase its service life.
[0065] It can be understood that, through the above steps S1 to S3, the method for preparing the two-dimensional polymer film material can prepare a composite material containing the two-dimensional polymer 130.
[0066] In a second aspect, the present disclosure further provides a two-dimensional polymer thin film material, which is prepared by the preparation method of the two-dimensional polymer thin film material of the present disclosure.
[0067] In some embodiments of the present disclosure, the two-dimensional polymer film material may include a substrate 110, a two-dimensional material layer 120, a two-dimensional polymer 130, and a fixed layer 140. The two-dimensional material layer 120 is stacked on the substrate 110, the two-dimensional polymer 130 is stacked on a side of the two-dimensional material layer 120 away from the substrate 110, and the fixed layer 140 is stacked on a side of the two-dimensional polymer 130 away from the two-dimensional material layer 120.
[0068] Further, as some examples of this embodiment, the material of the two-dimensional material layer 120 may include graphene oxide, and the material of the fixed layer 140 may include cured silicone oil.
[0069] Please note that the above embodiments are for illustrative purposes only and are not meant to be limiting of this document.
[0070] It should be understood that, unless otherwise specified herein, there is no strict order restriction for the execution of the steps, and the steps may be executed in other orders. Moreover, at least a portion of the steps in the preparation process may include multiple sub-steps or multiple stages, and these sub-steps or stages are not necessarily executed at the same time, but may be executed at different times, and the execution order of these sub-steps or stages is not necessarily sequential, but may be executed in turn or alternately with other steps or at least a portion of the sub-steps or stages of other steps.
[0071] The various embodiments in this specification are described in a progressive manner, and each embodiment focuses on the differences from other embodiments. The same or similar parts between the various embodiments can be referenced to each other.
[0072] The technical features of the above embodiments may be combined arbitrarily. To make the description concise, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
Claims
1. A method for preparing a two-dimensional polymer film material, characterized in that: The method comprises the following steps: sputtering and depositing a first organic monomer material on a substrate, and evaporating and depositing a second organic monomer material on the substrate, wherein the evaporated second organic monomer material is in a gaseous state and diffuses and is distributed on the substrate, the sputtered first organic monomer material is mixed with the second organic monomer material and contacts by collision, and the first organic monomer material and the second organic monomer material are polymerized on the substrate to form a two-dimensional polymer; Before depositing the first organic monomer material and the second organic monomer material, the method further includes the step of preparing a two-dimensional material layer on the substrate; the first organic monomer material and the second organic monomer material are both deposited on the two-dimensional material layer, and the material of the two-dimensional material layer includes graphene oxide; The first organic monomer material is selected from one of melamine and trimesoyl chloride, and the second organic monomer material is selected from the other of melamine and trimesoyl chloride.
2. The method for preparing a two-dimensional polymer film material according to claim 1, characterized in that: The material of the substrate includes a metal capable of catalyzing the growth of graphene.
3. The method for preparing a two-dimensional polymer film material according to claim 2, characterized in that: The material of the substrate includes one or more of iron, nickel and copper.
4. The method for preparing a two-dimensional polymer film material according to claim 3, characterized in that: After forming the two-dimensional polymer, the method further comprises the following steps: A fixing material is coated on a side of the two-dimensional polymer film away from the substrate and cured to form a fixing layer, wherein the fixing material comprises silicone oil.
5. The method for preparing a two-dimensional polymer film material according to claim 4, characterized in that: The silicone oil in the fixing material is selected from one or more of vinyl silicone oil and hydrogen-containing silicone oil.
6. The method for preparing a two-dimensional polymer film material according to claim 4, characterized in that: The thickness of the fixed layer formed is 0.5 mm to 5 mm.
7. The method for preparing a two-dimensional polymer film material according to any one of claims 1 to 6, characterized in that: The first organic monomer material is selected from melamine, and the second organic monomer material is selected from trimesoyl chloride.
8. The method for preparing a two-dimensional polymer film material according to claim 7, characterized in that: In the step of sputtering and depositing the first organic monomer material, the sputtering power is controlled to be 100W-500W; In the step of evaporating and depositing the second organic monomer material, an organic evaporation source is used to evaporate and deposit the second organic monomer material, and the evaporation temperature of the organic evaporation source is controlled to be 50° C. to 200° C.
9. The method for preparing a two-dimensional polymer film material according to any one of claims 1 to 6 and 8, characterized in that: The thickness of the formed two-dimensional polymer is 1 nm to 100 nm.
10. A two-dimensional polymer film material, characterized in that: The two-dimensional polymer film material is prepared by the method for preparing the two-dimensional polymer film material according to any one of claims 1 to 9.
Citation Information
Patent Citations
Preparation method for vapor grown two-dimensional material
CN104818526A