A refractory metal surface chemical modification catalyst and surface chemical modification method thereof
By using a penetrating agent composed of rare earth phosphate, rare earth fluoride and carrier particles on the surface of the refractory metal, combined with the vacuum carburizing process, the problems of uneven thickness and unstable performance of the surface modification layer are solved, and the surface hardness and performance are significantly improved. Corrosion resistance, suitable for high temperature environments.
Patent Information
- Application Number
- CN202410898358.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-05
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2044-07-05
AI Technical Summary
The existing refractory metal surface carburizing modification technology suffers from low efficiency, uneven thickness of the modified layer, cracking and unstable structural properties. In addition, the existing percolation agent has low activity and poor fluidity, and cannot fully utilize the properties of rare earth elements. Resulting in performance degradation in high temperature environments.
Using a penetrating agent composed of rare earth phosphate, rare earth fluoride, carrier particles and methyl silicone oil, through uniform mixing and vacuum carburizing process, a modified layer with uniform depth is formed to improve surface hardness and chemical corrosion resistance.
It significantly improves the depth and thickness uniformity of the refractory metal surface modification layer, enhances the material's high-temperature stability and chemical corrosion resistance, and is suitable for harsher extreme environments.
Smart Images

Figure CN118422111B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of metal material surface treatment, and in particular to a refractory metal surface chemical modification catalyst and a surface chemical modification method thereof. Background Art
[0002] Refractory metals and their alloys have been successfully applied in aerospace and aviation engineering and have become indispensable materials due to their high temperature strength, good resistance to liquid metal corrosion, and plastic processing. The development of the aerospace industry will inevitably put forward new demands for refractory metal materials, among which high temperature strength, high temperature oxidation and protection, and material lightweighting are new challenges that cannot be avoided. Usually, the failure behavior of refractory metal materials in the service process often starts from its surface. Therefore, the surface properties of the material directly affect whether the material can serve for a long time in the harsh environment of high-intensity thermal shock and wear and corrosion. Surface treatment technology is widely used by coating one or more layers of metal or non-metal on the surface of the substrate, which has the advantages of improving the wear resistance, heat resistance, corrosion resistance, and high temperature stability of the substrate. At present, the commonly used surface modification methods mainly include: alloying, coating, nitriding, carburizing, etc. Among them, carburizing modification forms a carbide modification layer on the surface of the metal substrate to resist oxidation and melt corrosion, and has the advantages of simple process and no effect on the performance of the substrate. However, refractory metals have strong hydrogen absorption properties, so they are prone to hydrogen embrittlement during surface treatment, which reduces the mechanical properties of the material. The current surface carburizing modification technology for refractory metals has disadvantages such as low surface treatment efficiency, uneven thickness of the surface modified layer, cracking of the modified layer, and unstable organizational properties of the modified layer.
[0003] Research and production practice in recent years have proved that the addition of rare earth elements has a significant activation and catalytic effect on the chemical heat treatment process, and also has the characteristics of changing the chemical composition and structure of the workpiece surface and improving the material properties. However, in reality, there are various problems with the use of rare earth catalysts. In particular, the existing catalysts are generally dissolved in a carburizing carrier gas solvent such as methanol, so they have low activity and poor fluidity, which makes it impossible for the rare earth elements to fully contact the workpiece surface, and thus cannot fully exert the characteristics of the rare earth elements, and easily lead to problems such as blockage.
[0004] CN109234666A discloses a rare earth catalyst for heat treating materials to achieve carburizing modification, which mainly includes an organic solvent and a rare earth compound; wherein the rare earth compound includes a rare earth nitrate and / or a rare earth alcohol amine salt; the rare earth compound exists in the form of being dispersed in the organic solvent; the obtained rare earth catalyst can achieve carburizing processing of the material with high efficiency, and significantly improves the physical and chemical indicators of the product, and also has a great improvement on the heat treatment deformation of the product; however, the rare earth catalyst used has a relatively low cracking temperature, and the treatment temperature is low when the material is heat treated, and is not suitable for carburizing modification of the surface of refractory metal matrix materials.
[0005] Therefore, there is still a need to find a surface chemical modification method suitable for refractory metal matrix materials. Summary of the invention
[0006] Based on the above problems, the present invention provides a refractory metal surface chemical modification catalyst and a surface chemical modification method thereof, which can effectively improve the carburizing efficiency of refractory metals and improve the high temperature stability and chemical corrosion resistance of the material.
[0007] A refractory metal surface chemical modification catalyst, the rare earth catalyst is composed of the following components by mass percentage: 5-15% rare earth phosphate, 1-10% rare earth fluoride, 50-80% carrier particles, 1-15% methyl silicone oil, and the balance is solvent; wherein the rare earth phosphate is at least one of lanthanum, cerium, and yttrium phosphate powders; the rare earth fluoride is at least one of lanthanum, cerium, and yttrium fluoride salt powders; the carrier particles are at least one of quartz sand, aluminum oxide, and silicon carbide; the solvent is any one of methanol, ethanol, and isopropanol; the refractory metal is one of tantalum, tantalum alloy, tungsten, tungsten alloy, rhenium, and rhenium alloy.
[0008] Preferably, the particle size of the carrier particles is 5-500 μm. Too small or too large particle size is not conducive to the carburizing effect. Too small particle size has a barrier effect on acetylene and is easy to react with the metal surface to form uncontrollable compounds; while too large particle size has limited adhesion, resulting in uneven coating.
[0009] Further, the preparation process of the penetration catalyst is as follows:
[0010] (1) adding rare earth phosphate and rare earth fluoride into a reactor according to the formula amount and mixing them thoroughly;
[0011] (2) gradually adding the carrier particles while stirring and mixing until a uniform powder mixture is formed;
[0012] (3) Add methyl silicone oil to the powder mixture and mix thoroughly to ensure that the powder is evenly coated;
[0013] (4) Add the solvent and stir to mix until a uniform penetration catalyst is formed.
[0014] Preferably, the penetration catalyst is in the form of a paste or ointment.
[0015] A surface chemical modification method using a refractory metal surface chemical modification catalyst comprises the following steps: surface treatment of a refractory metal substrate, preparation of a catalyst, coating, baking, carburizing and surface polishing, wherein the coating, baking, carburizing and surface polishing steps need to be repeated, with the number of repetitions being ≤5 times.
[0016] Preferably, the number of repetitions should not be too many, as the surface will become brittle if it exceeds 5 times.
[0017] Furthermore, the coating process adopts at least one of spraying, dipping or brushing.
[0018] Furthermore, in the coating process, the coating environment temperature is 15-40° C., and the coating thickness is 50-200 μm or 200-500 μm.
[0019] Furthermore, the errors generated in the coating process are different when the coating thickness is different, wherein the error is ±20 μm when the coating thickness is 50-200 μm, and the error is ±50 μm when the coating thickness is 201-500 μm.
[0020] Furthermore, the baking process is performed at a temperature of 200-300° C. and a time of 2-6 h.
[0021] Furthermore, the carburizing method in the carburizing process is vacuum carburizing.
[0022] Furthermore, the vacuum carburizing process includes four stages carried out in sequence, wherein the first stage is to raise the temperature to 1200-1800°C under the condition of vacuum better than 6.7×10-1Pa; the second stage is to introduce acetylene gas into the vacuum furnace with a furnace pressure of 100-1000Pa, and keep it at 1200-1800°C for 6-12 hours; the third stage is to evacuate to above 6.7×10-1Pa, and introduce nitrogen or argon with a furnace pressure of 1000-3000Pa, and keep it at 1400-1800°C for 6-12 hours; the fourth stage is to cool down to below 100°C with the furnace and take it out of the furnace.
[0023] The advantages of the present invention are:
[0024] The present invention can promote the breaking of hydrocarbon chains of hydrocarbon compounds and release more active carbon atoms through the catalytic effect of rare earth phosphate, rare earth fluoride and the like in the catalyst; it can also activate the surface of refractory metals, change the microstructure of the metal surface and the properties of grain defects, improve the surface activity, promote the adsorption and diffusion of carbon atoms on the metal surface, effectively increase the depth and thickness uniformity of the modified layer on the refractory metal surface, and improve the surface hardness and chemical corrosion resistance of the material. The process is simple, does not affect the performance of the matrix, and the obtained material has the advantage of being suitable for service in more severe and extreme environments. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 This is a process flow chart of carburizing modification using a refractory metal surface chemical modification catalyst created by the present invention;
[0026] Figure 2 This is a SEM test image of the tantalum metal surface modification layer of Example 1 of the present invention;
[0027] Figure 3 This is a SEM test image of the tantalum metal surface modification layer of comparative example 1 of the present invention. DETAILED DESCRIPTION
[0028] The present invention provides a refractory metal surface chemical modification catalyst and a surface chemical modification method thereof, which meet the requirements for service in more severe and extreme environments and can be applied in the fields of aerospace and nuclear industry.
[0029] The following will be combined with the drawings in the embodiments of the invention to clearly and completely describe the technical solutions in the embodiments of the invention. Obviously, the described embodiments are only part of the embodiments of the invention, not all of them. Based on the embodiments in the invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the invention.
[0030] Example 1. This example provides a catalyst for chemically modifying the surface of refractory metals, which is composed of the following components in percentage by mass: 5% rare earth phosphate, 1% rare earth fluoride, 80% carrier particles, 1% methyl silicone oil, and the balance is methanol; wherein the rare earth phosphate described in this example is a mixture powder of lanthanum, cerium, and yttrium phosphates; the rare earth fluoride described in this example is a mixture powder of lanthanum, cerium, and yttrium fluoride salts; the carrier particles described in this example are alumina with a particle size of 5 μm.
[0031] like Figure 1 As shown, this embodiment also provides a surface chemical modification method using a refractory metal surface chemical modification catalyst, including the steps of metal substrate surface treatment, catalyst preparation, coating, baking, carburizing and surface polishing performed in sequence, and the specific process is as follows:
[0032] (1) Surface treatment of substrate: cleaning and degreasing the surface of the refractory metal substrate to ensure that the surface is clean and free of impurities (the refractory metal substrate described in this embodiment is pure tantalum);
[0033] (2) Preparation of the catalyst: Add rare earth phosphate and rare earth fluoride according to the formula amount into a container and mix them thoroughly; gradually add alumina and stir to form a uniform powder mixture; add methyl silicone oil to the powder mixture and stir to ensure that the powder particles are evenly coated; finally, add methanol and stir to form a uniform paste catalyst;
[0034] (3) Coating process: Spray coating, working environment temperature is 15°C, coating thickness is 50 μm, error is ±20 μm);
[0035] (4) Baking process: Place the metal parts treated in step (3) in an electric hot air drying oven for baking at a temperature of 200°C for 2 hours;
[0036] (5) Vacuum carburizing: The metal parts treated in step (4) are placed in a vacuum heat treatment furnace for high temperature and low pressure carburizing. The four stages of the treatment are as follows:
[0037] The first stage: at a vacuum degree of 6.7×10 -1 Pa conditions to 1200 °C;
[0038] The second stage: acetylene gas is introduced into the vacuum furnace, the furnace pressure is 100-600 Pa, and the temperature is kept at 1200℃ for 6 hours;
[0039] The third stage: vacuum to 6.7×10 -1 Pa, then nitrogen is introduced, the furnace pressure is 1000-2000 Pa, and the temperature is kept at 1400℃ for 6 hours;
[0040] The fourth stage: the temperature is lowered to below 100℃ and then taken out of the furnace;
[0041] (6) Surface polishing: Polish and clean the surface of tantalum metal materials to ensure that there is no dirt and coating on the surface;
[0042] (7) Carburizing is completed.
[0043] Example 2. This example provides a catalyst for chemically modifying the surface of a refractory metal, which is composed of the following components by mass percentage: 5% rare earth phosphate, 1% rare earth fluoride, 80% carrier particles, 1% methyl silicone oil, and the remainder is ethanol; the rare earth phosphate described in this example is a lanthanum and cerium phosphate mixture powder; the rare earth fluoride described in this example is a lanthanum fluoride salt powder; the carrier particles described in this example are a mixture of quartz sand and alumina, and the particle size is 250 μm.
[0044] This embodiment provides a surface chemical modification method using a refractory metal surface chemical modification catalyst, and the specific process is as follows:
[0045] (1) Substrate surface treatment: Clean and degrease the surface of the refractory metal substrate to ensure that the surface is clean and free of impurities (the refractory metal substrate in this embodiment is 93WNiFe);
[0046] (2) Preparation of the catalyst: Add rare earth phosphate and rare earth fluoride according to the formula amount into a container and mix them thoroughly; gradually add the quartz sand and alumina mixture and stir and mix until a uniform powder mixture is formed; add methyl silicone oil to the powder mixture and mix thoroughly to ensure that the powder particles are evenly coated; finally, add ethanol and stir and mix until a uniform paste catalyst is formed;
[0047] (3) Coating process: Dipping method is used to ensure uniform coating; the ambient temperature is 25°C, the coating thickness is 150 μm, and the error is ±20 μm;
[0048] (4) Baking process: Place the metal parts treated with the catalytic coating in an electric blast drying oven or other equipment that can be used for baking and heating for baking at a temperature of 250°C for 4 h. If the surface is visually uneven, apply the coating again for 2 h.
[0049] (5) Vacuum carburizing: The metal parts treated with the catalytic coating are placed in a vacuum heat treatment furnace for high temperature and low pressure carburizing. The four stages of the treatment are as follows:
[0050] The first stage: at a vacuum degree of 6.7×10 -1 Pa conditions to 1500 °C;
[0051] The second stage: acetylene gas is introduced into the vacuum furnace, the furnace pressure is 500-1000 Pa, and the temperature is kept at 1600℃ for 9 hours;
[0052] The third stage: vacuum to 6.7×10 -1 Pa, then nitrogen is introduced, the furnace pressure is 1500-2500Pa, and the temperature is kept at 1600℃ for 9 hours;
[0053] The fourth stage: the temperature is lowered to below 100℃ and then taken out of the furnace;
[0054] (6) Surface polishing: Polish and clean the surface of the tungsten alloy material to ensure that there is no dirt and coating on the surface;
[0055] (7) Repeat the coating, baking, carburizing and grinding process of steps (3) to (6) three times;
[0056] (8) Carburizing is completed.
[0057] Example 3. This example provides a catalyst for chemically modifying the surface of a refractory metal, which is composed of the following components by mass percentage: 15% rare earth phosphate, 10% rare earth fluoride, 50% carrier particles, 15% methyl silicone oil, and the balance is isopropanol; the rare earth phosphate in this example is lanthanum salt powder; the rare earth fluoride in this example is cerium fluoride salt powder; the carrier particles in this example are a mixture of quartz sand, alumina and silicon carbide, with a particle size of 500 μm.
[0058] This embodiment provides a surface chemical modification method using a refractory metal surface chemical modification catalyst, and the specific process is as follows:
[0059] (1) Surface treatment of the substrate: cleaning and degreasing the surface of the refractory metal substrate to ensure that the surface is clean and free of impurities (in this embodiment, the refractory metal substrate is pure rhenium);
[0060] (2) Preparation of the catalyst: Add rare earth phosphate and rare earth fluoride according to the formula amount into a container and mix them thoroughly; gradually add the quartz sand, alumina and silicon carbide mixture and stir and mix them at the same time until a uniform powder mixture is formed; add methyl silicone oil to the powder mixture and mix them thoroughly to ensure that the powder particles are evenly coated; finally, add isopropyl alcohol and stir and mix them at the same time until a uniform paste catalyst is formed;
[0061] (3) Coating process: Dipping method is used to ensure uniform coating; the ambient temperature is 40 °C, the coating thickness is 500 μm, and the error is ±50 μm;
[0062] (4) Baking process: Place the rhenium metal parts treated with the catalytic coating in an electric blast drying oven or other equipment that can be used for baking and heating for baking at a temperature of 300°C for 6 h. If the surface is visually uneven, apply another coat of the coating for 2 h.
[0063] (5) Vacuum carburizing: The metal parts treated with the catalytic coating are placed in a vacuum heat treatment furnace for high temperature and low pressure carburizing. The four stages of the treatment are as follows:
[0064] The first stage: at a vacuum degree of 6.7×10 -1 Pa conditions to 1800 °C;
[0065] The second stage: acetylene gas is introduced into the vacuum furnace, the furnace pressure is 500-1000 Pa, and the temperature is kept at 1800℃ for 12 hours;
[0066] The third stage: vacuum to 6.7×10 -1 Pa, then argon gas is introduced, the furnace pressure is 2000-3000Pa, and the temperature is kept at 1600℃ for 9 hours;
[0067] The fourth stage: the temperature is lowered to below 100℃ and then taken out of the furnace;
[0068] (6) Surface polishing: Polish and clean the surface of the rhenium metal material to ensure that there is no dirt and coating on the surface;
[0069] (7) Repeat the coating, baking, carburizing and grinding process of steps (3) to (6) five times;
[0070] (8) Carburizing is completed.
[0071] Comparative Example 1
[0072] The surface chemical modification method of the refractory metal material provided in this comparative example is different from that in Example 1 in that no catalyst is added in this comparative example, and no process related to the catalyst is included. The specific process is as follows:
[0073] (1) Surface treatment of substrate: Clean and degrease the surface of the refractory metal substrate to ensure that the surface is clean and free of impurities (the refractory metal substrate in this comparative example is pure tantalum);
[0074] (2) Vacuum carburizing: The treated metal parts are placed in a vacuum heat treatment furnace for high temperature and low pressure carburizing. The four stages of the treatment are as follows:
[0075] The first stage: at a vacuum degree of 6.7×10 -1 Pa conditions to 1200 °C;
[0076] The second stage: acetylene gas is introduced into the vacuum furnace, the furnace pressure is 100-600Pa, and the temperature is kept at 1200℃ for 6 hours;
[0077] The third stage: vacuum to 6.7×10 -1 Pa, then nitrogen is introduced, the furnace pressure is 1000-2000Pa, and the temperature is kept at 1400℃ for 6 hours;
[0078] The fourth stage: the temperature is lowered to below 100℃ and then taken out of the furnace;
[0079] Carburizing is finished.
[0080] Comparative Example 2
[0081] The refractory metal substrate treated in this comparative example is the same as that in Example 1, that is, pure tantalum.
[0082] The method for chemical modification of the surface of refractory metals provided in this comparative example is the same as that in Example 1, except that the catalyst component used in this comparative example is different, and is composed of the following components, by mass percentage: 5% rare earth phosphate, 1% rare earth chloride, 80% carrier particles, 1% methyl silicone oil, and the balance is methanol; wherein the rare earth phosphate described in this example is a mixture powder of lanthanum, cerium, and yttrium phosphates; the rare earth chloride described in this example is a mixture powder of lanthanum, cerium, and yttrium chlorides; the carrier particles described in this example are alumina with a particle size of 5 μm.
[0083] Comparative Example 3
[0084] The refractory metal substrate treated in this comparative example is the same as that in Example 1, that is, pure tantalum.
[0085] The method for chemical modification of the surface of refractory metals provided in this comparative example is the same as that in Example 1, except that the catalyst component used in this comparative example is different, and is composed of the following components by mass percentage: 5% rare earth carbonate, 1% rare earth fluoride, 80% carrier particles, 1% methyl silicone oil, and the balance is methanol; wherein the rare earth carbonate described in this example is a mixture powder of lanthanum, cerium, and yttrium carbonates; the rare earth fluoride described in this example is a mixture powder of lanthanum, cerium, and yttrium fluoride salts; and the carrier particles described in this example are alumina with a particle size of 5 μm.
[0086] Test Example 1
[0087] According to the refractory metal surface modification layer samples obtained in the above embodiments and comparative examples, the samples were cut longitudinally, and the surface modification layers were observed and analyzed by scanning electron microscopy (SEM) and metallographic microscopy. The results are shown in Table 1.
[0088] Among them, the results of Example 1 and Comparative Example 1 are as follows Figure 2 and Figure 3 As shown, it can be seen from the figure that the average thickness of the surface modification layer of comparative example 1 is 6.0 μm, and the thickness of the modified layer is uneven, with a small amount of cracking. The average thickness of the surface modification layer of embodiment 1 is 56.0 μm, and the internal structure is dense, tightly combined with the metal matrix, the thickness of the modified layer is uniform, and there is no cracking. It can be seen that the surface modification effect of refractory metals using the surface chemical modification catalyst and the surface chemical modification method of the present invention is significant.
[0089] Test Example 2
[0090] The Vickers hardness test of the refractory metal surface modification layer samples obtained in the above embodiments and comparative examples was performed according to the Vickers hardness test method for metal materials in national standard GB / T 4340.1-2009. The test results are shown in Table 1.
[0091] It can be seen from Table 1 that the hardness of the surface modified layer of Example 1 is HV2240, while the hardness of the surface modified layer of Comparative Example 1 without using a catalyst is HV1860. It can be seen that the hardness of the surface modified layer using a catalyst is significantly improved, and the hardness of Comparative Example 2 in which rare earth chloride is used instead of rare earth fluoride to prepare a catalyst is HV2040, and the hardness of Comparative Example 3 in which rare earth carbonate is used instead of rare earth phosphate to prepare a catalyst is HV2120, which can further illustrate that the catalyst prepared by the formula of the present invention is more conducive to improving the hardness of the surface modified layer of the metal material.
[0092] From the results of Examples 1-3, it can be seen that the hardness of the surface modified layer of the metal material in Example 3, which repeated the coating, baking, carburizing and polishing steps for 5 times, is better than that in Example 2, which repeated the above steps for 3 times, and is even better than that in Example 1, which did not repeat the above steps. This shows that repeating the coating, baking, carburizing and polishing steps helps to improve the surface hardness, but the number of times should not be too many, as too many times will easily lead to brittleness of the material surface.
[0093] In summary, the refractory metal surface chemical modification catalyst and the surface chemical modification method of the present invention both have significant modification effects on the refractory metal surface and can improve the surface hardness and wear resistance of the material.
[0094] Test Example 3
[0095] The refractory metal surface modification layer samples obtained in the above examples and comparative examples were kept in a NaCl-KCl molten salt system at a temperature of 950°C for 12 hours and subjected to corrosion resistance tests. The results are shown in Table 1. It can be seen that the corrosion weight loss of Example 3 is 0.5 μg / mm 2 , the corrosion resistance is the best.
[0096] Compared with Comparative Examples 1, 2 and 3, Example 1, which also uses refractory metal pure tantalum as the matrix, has a corrosion weight loss of 22.4 μg / mm2 in Comparative Example 1 without using a catalyst. 2 The corrosion weight loss of comparative example 2 using rare earth chloride instead of rare earth fluoride as the catalyst was 18.4 μg / mm 2 The comparative example 3 using rare earth carbonate instead of rare earth phosphate as the catalyst has a corrosion weight loss of 16.2 μg / mm 2 The corrosion weight loss of Example 1 using the catalyst of the present invention is 8.5 μg / mm 2It can be seen that the rare earth fluoride in the catalyst of the present invention has a certain trace corrosion effect on refractory metals, promoting the penetration of carbon atoms, while the rare earth phosphate can slow down the corrosion caused by the rare earth fluoride, protect the surface, and thus play a balancing role. Therefore, the catalyst provided by the present invention and its surface chemical modification method have significant modification effect on the surface of refractory metal substrates, and the resulting material can significantly improve the corrosion resistance.
[0097]
[0098] It can be seen from the above test examples 1-3 that the present invention can activate the surface of refractory metals, improve the surface activity, promote the adsorption and diffusion of carbon atoms on the surface of refractory metals, and significantly increase the depth of the surface modification layer of refractory metals through the composite of rare earth phosphate and rare earth fluoride in the catalyst, and improve the surface hardness and chemical corrosion resistance of refractory metal materials through the surface chemical modification method of the present invention.
[0099] For those skilled in the art, the invention is not limited to the details of the above exemplary embodiments, and can be implemented in other specific forms without departing from the spirit or basic characteristics of the invention; therefore, no matter from which point of view, the embodiments should be regarded as exemplary and non-restrictive, and the scope of the invention is defined by the appended claims rather than the above description, so it is intended to include all changes within the meaning and scope of the equivalent elements of the claims. Any reference numerals in the claims should not be regarded as limiting the claims involved.
[0100] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any minor modifications, equivalent substitutions and improvements made to the above embodiments based on the technical essence of the present invention should be included in the protection scope of the technical solution of the present invention.
Claims
1. A catalyst for chemically modifying the surface of refractory metals, It is characterized in that The catalyst is composed of the following components by mass percentage: 5-15% rare earth phosphate, 1-10% rare earth fluoride, 50-80% carrier particles, 1-15% methyl silicone oil, and the balance is solvent; wherein the rare earth phosphate is at least one of lanthanum, cerium, and yttrium phosphate powders; the rare earth fluoride is at least one of lanthanum, cerium, and yttrium fluoride powders; the carrier particles are at least one of quartz sand, alumina, and silicon carbide, with a particle size of 5-500 μm; the solvent is any one of methanol, ethanol, and isopropanol; the refractory metal is one of tantalum, tantalum alloy, tungsten, tungsten alloy, rhenium, and rhenium alloy.
2. The refractory metal surface chemical modification catalyst according to claim 1, It is characterized in that The penetration catalyst is in the form of a paste or ointment.
3. The refractory metal surface chemical modification catalyst according to claim 1, It is characterized in that The preparation process of the penetration catalyst is as follows: (1) adding rare earth phosphate and rare earth fluoride into a reactor according to the formula amount and mixing them thoroughly; (2) gradually adding the carrier particles while stirring and mixing until a uniform powder mixture is formed; (3) Add methyl silicone oil to the powder mixture and mix thoroughly to ensure that the powder is evenly coated; (4) Add the solvent and stir to mix until a uniform penetration catalyst is formed.
4. A surface chemical modification method using the refractory metal surface chemical modification catalyst according to claim 1, comprising the following steps: surface treatment of refractory metal substrate → preparation of catalyst → coating → baking → carburizing → surface polishing process, It is characterized in that The carburizing process adopts vacuum carburizing as the carburizing method, and the coating, baking, carburizing and surface grinding processes need to be repeated, and the number of repetitions is ≤5 times.
5. The surface chemical modification method using a refractory metal surface chemical modification catalyst according to claim 4, It is characterized in that In the coating process, the coating method is at least one of spraying, dipping or brushing.
6. The surface chemical modification method using a refractory metal surface chemical modification catalyst according to claim 5, It is characterized in that The coating process environment temperature is 15-40° C., and the coating thickness is 50-500 μm, wherein the coating thickness has an error of ±20 μm when it is 50-200 μm, and the coating thickness has an error of ±50 μm when it is 201-500 μm.
7. The surface chemical modification method using a refractory metal surface chemical modification catalyst according to claim 4, It is characterized in that The baking process is performed at a temperature of 200-300° C. and for a time of 2-6 h.
8. The surface chemical modification method using a refractory metal surface chemical modification catalyst according to claim 4, It is characterized in that The vacuum carburizing process includes four stages, in which the first stage is to -1 Pa conditions to 1200-1800 ° C; the second stage is to introduce acetylene gas into the vacuum furnace, the furnace pressure is 100-1000Pa, and keep it at 1200-1800 ° C for 6-12 hours; the third stage is to evacuate to 6.7×10 -1 Pa, and introduce nitrogen or argon, the furnace pressure is 1000-3000Pa, and the insulation time is 6-12 hours at 1400-1800℃; the fourth stage is to cool down to below 100℃ and take it out of the furnace.