A positive electrode sheet and its preparation method and application
By setting a functional compound functional layer of amide group and -COO- group on the cathode material layer of the sodium-ion battery, the problem of electrochemical decomposition and irreversible capacity loss of Prussian blue cathode materials in sodium-ion batteries is solved, and the The electrochemical and safety properties of the battery extend its service life.
Patent Information
- Application Number
- CN202410882235.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-03
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-07-03
AI Technical Summary
Coordinated water in the crystal lattice of Prussian blue cathode materials in sodium-ion batteries may transfer into the electrolyte, leading to electrochemical decomposition, high irreversible capacity loss in the first cycle, and dissolution of transition metals, which affects electrochemical performance and safety performance.
A functional compound functional layer containing amide groups and -COO- groups is provided on the side of the positive electrode material layer away from the current collector to inhibit metal dissolution, absorb carbon dioxide, and improve battery electrochemistry and safety performance.
The first-cycle Coulomb efficiency, long cycle performance and safety performance of the battery are improved, and the service life of the battery is extended.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of batteries and relates to a positive electrode sheet and a preparation method and application thereof. Background Art
[0002] As market demand increases, the development of lithium-ion batteries may be constrained by lithium resources. Lithium is an element that accounts for only 0.0065% of the earth's crust. Lithium reserves are not abundant and their geographical distribution is relatively uneven. The application of lithium-ion batteries is severely limited by lithium resources.
[0003] Sodium-ion batteries are another type of energy storage battery with a similar working mechanism and battery structure to lithium-ion batteries. The abundance of sodium resources is much higher than that of lithium resources, and they are evenly distributed around the world. They are cheap and stable. Since sodium resources are easily accessible and cheap, and the negative electrode current collector of sodium-ion batteries can use aluminum foil instead of copper foil like lithium-ion batteries, sodium-ion batteries have great potential price advantages. With the continuous deepening of research, the potential advantages of sodium-ion batteries are constantly being explored, especially the excellent performance at high and low temperatures and high safety, which lays a good foundation for the application of sodium-ion batteries in the fields of energy storage and power.
[0004] Positive electrode materials are a key component for reducing the cost of sodium-ion batteries. Among them, positive electrode materials such as Prussian blue are characterized by low cost, easy scale-up, simple process, and high safety. However, sodium-ion batteries such as Prussian blue have the following problems:
[0005] First, the coordinated water in the lattice of positive electrode materials such as Prussian blue may be transferred into the electrolyte, causing electrochemical decomposition, leading to the destruction of the electrolyte, affecting the electrochemical performance of the battery, and even causing safety hazards;
[0006] Second, when a Prussian blue-based positive electrode material is used as the positive electrode and a sodium-free carbon material is used as the negative electrode, the irreversible capacity loss in the first cycle is high, consuming too much sodium ions and affecting the subsequent electrochemical performance of the battery.
[0007] Third, during the use of sodium-ion batteries that use Prussian blue as the positive electrode material, transition metals may dissolve, affecting the SEI film and thus the electrochemical performance. At this time, the electrolyte of the sodium-ion battery may react with its own impurities or with the positive and negative electrode materials to produce gases mainly composed of CO2, which affects the battery's electrochemical performance and safety performance.
[0008] In summary, it is necessary to find a suitable positive electrode to improve the first-cycle coulombic efficiency, long-cycle performance and safety performance of sodium-ion batteries. Summary of the invention
[0009] The object of the present invention is to provide a positive electrode sheet, a preparation method and an application thereof. By providing a functional layer containing a functional compound with specific groups on the surface of the positive electrode material layer away from the current collector, the metal dissolution in the positive electrode material can be avoided, the carbon dioxide generated by the side reaction of the positive electrode material and the electrolyte can be absorbed, and water can also be absorbed, thereby improving the electrochemical performance, safety performance and service life of the battery.
[0010] To achieve the object of the present invention, the following technical solutions are adopted:
[0011] In the first aspect, the present invention provides a positive electrode sheet, which includes a current collector and a coating provided on at least one surface of the current collector. The coating includes a positive electrode material layer provided on the surface of the current collector, and a functional layer provided on the side of the positive electrode material layer away from the current collector;
[0012] The functional layer includes a functional compound, and the functional compound includes an amide group and a -COO - group.
[0013] Preferably, the functional compound further includes sodium ions.
[0014] Preferably, the functional compound includes a sodium salt of an organic acid containing an amide group.
[0015] Preferably, the sodium salt of the organic acid containing an amide group includes any one or at least two combinations of sodium lauroamphoacetate, sodium lauroylsarcosinate or sodium cocoyl glycinate.
[0016] Preferably, the surface density ratio of the functional layer to the positive electrode material layer is (1-4):(5-9).
[0017] Preferably, the positive electrode material layer includes a Prussian blue-based positive electrode material.
[0018] Preferably, the Prussian blue-based positive electrode material includes Na x M1[M2(CN)6] y ·zH2O, where 0 < x ≤ 2, 0.8 ≤ y < 1, 0 < z ≤ 20, M1 and M2 are transition metal elements, and the transition metal elements include any one or at least two combinations of Fe, Mn, Cu, Ni or Co.
[0019] Preferably, the positive electrode material layer further includes a first conductive agent and a first binder.
[0020] Preferably, the mass ratio of the Prussian blue-based positive electrode material, the first conductive agent and the first binder is (90-94):(1-6):(2-4).
[0021] Preferably, the first conductive agent includes any one of SP (conductive carbon black), acetylene black, Ketjen black or conductive graphite, or a combination of at least two thereof.
[0022] Preferably, the first binder includes any one of PVDF (polyvinylidene fluoride), SBR (styrene butadiene rubber), CMC (sodium carboxymethyl cellulose), LA (polyacrylates) or PAA (polyacrylic acid), or a combination of at least two thereof.
[0023] Preferably, the functional layer further includes a second conductive agent and a second binder.
[0024] Preferably, the mass ratio of the functional compound, the second conductive agent and the second binder is (90-94):(1-6):(2-4).
[0025] Preferably, the second conductive agent includes any one of SP, acetylene black, Ketjen black or conductive graphite, or a combination of at least two thereof.
[0026] Preferably, the second binder includes any one of PVDF, SBR, CMC, LA or PAA, or a combination of at least two thereof.
[0027] In a second aspect, the present invention provides a method for preparing the positive electrode sheet as described in the first aspect, the preparation method comprising the following steps:
[0028] (1) coating a positive electrode material layer slurry on at least one side of a current collector, and obtaining a positive electrode material layer on at least one side of the current collector after drying;
[0029] (2) coating the functional layer slurry on the surface of the positive electrode material layer in step (1), and drying to obtain the positive electrode sheet;
[0030] The functional layer slurry includes a functional compound, wherein the functional compound includes an amide group and a -COO - Group.
[0031] Preferably, the thickness of the positive electrode material layer slurry coating in step (1) is 40-60 μm.
[0032] Preferably, the thickness of the functional layer slurry coating in step (2) is 3-6 μm.
[0033] Preferably, the positive electrode material layer slurry includes a Prussian blue positive electrode material, a first conductive agent, a first binder and a solvent.
[0034] Preferably, the functional layer slurry comprises a functional compound, a second conductive agent, a second binder and a solvent.
[0035] Preferably, the drying temperature in step (1) is 100-150°C.
[0036] Preferably, the drying temperature in step (2) is 100-150°C.
[0037] Preferably, the drying in step (2) includes first heating and then vacuum drying, so as to remove moisture from the electrode.
[0038] In a third aspect, the present invention provides a sodium ion battery, comprising the positive electrode sheet as described in the first aspect, or the positive electrode sheet prepared by the preparation method as described in the second aspect.
[0039] Preferably, the sodium ion battery further comprises a diaphragm, and the functional layer in the positive electrode plate is arranged on a side of the positive electrode plate close to the diaphragm.
[0040] Compared with the prior art, the present invention has the following beneficial effects:
[0041] The present invention arranges a functional layer on the surface of the positive electrode material away from the current collector. The amide group contained in the functional compound in the functional layer promotes the film formation of the positive electrode amide CEI film and inhibits the dissolution of transition metals in the positive electrode material. At the same time, the amide group can absorb CO2 during the use of the battery, which is beneficial to the electrochemical performance and safety performance of the battery. In addition, the -COO - After absorbing water, the group exhibits polyanion characteristics, which makes the functional layer have a certain viscosity. While absorbing water, it also enhances the viscosity between the positive electrode material and the separator, which is beneficial to the long-term use of the battery and extends the battery life. DETAILED DESCRIPTION
[0042] In a specific embodiment, the present invention provides a positive electrode plate, the positive electrode plate comprising a current collector and a coating disposed on at least one side of the current collector, the coating comprising a positive electrode material layer disposed on the surface of the current collector, and a functional layer disposed on a side of the positive electrode material layer away from the current collector;
[0043] The functional layer includes a functional compound, wherein the functional compound includes an amide group and a -COO - Group.
[0044] The present invention provides a functional layer on the surface of the positive electrode material layer away from the current collector, and the functional compound in the functional layer includes an amide group and -COO -The amide group can promote the formation of positive electrode amide CEI film, which can inhibit the dissolution of transition metals in the positive electrode material and enhance the surface oxidation resistance. At the same time, the amide group can absorb CO2 generated by the side reaction between the positive electrode material and the electrolyte during the use of the battery, which is beneficial to improving the electrochemical performance and safety performance of the battery. The -COO - The group can absorb water, and after absorbing water it exhibits polyanion properties, which makes the functional layer have a certain viscosity. Therefore, while absorbing water it also enhances the viscosity between the positive electrode material and the separator, which is beneficial to the long-term use of the battery and extends the battery life.
[0045] The CEI membrane mentioned in the present invention refers to the positive electrode electrolyte interface membrane, which is a complex mixture formed in the sodium ion battery and is located between the positive electrode and the electrolyte; the SEI membrane refers to the solid electrolyte interface membrane, which is a passivation layer covering the surface of the electrode material formed when the negative electrode material and the electrolyte react at the solid-liquid interface during the first charge and discharge process of the sodium ion battery.
[0046] Preferably, the functional compound further comprises sodium ions.
[0047] The functional compound of the present invention preferably also contains sodium ions, which can be used to additionally supplement sodium ions during the first cycle to compensate for the irreversible capacity loss in the first cycle and improve the coulombic efficiency in the first cycle.
[0048] Preferably, the functional compound comprises a sodium salt of an organic acid containing an amide group.
[0049] The functional compound of the present invention preferably contains an amide group, -COO - Group and sodium ion, therefore, the functional compound is preferably a sodium salt of an organic acid containing an amide group.
[0050] Preferably, the organic acid sodium salt containing an amide group includes any one of sodium lauroyl amphoacetate, sodium lauroyl sarcosinate or sodium cocoyl glycinate, or a combination of at least two thereof.
[0051] The specific organic acid sodium salt containing an amide group used in the present invention is different from other organic acid sodium salts containing an amide group, -COO - The compound of the group and sodium ion is more stable to high temperature, acid and alkali.
[0052] Preferably, the surface density ratio of the functional layer to the positive electrode material layer is (1-4):(5-9), for example, it can be 1:9, 1:7, 2:5, 3:7.5, 4:7 or 4:5, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0053] The areal density ratio of the functional layer to the cathode material layer in the present invention affects the performance of the functional layer and the cathode material. If the ratio of the areal density is too small, the effect of the functional layer is not obvious. If the ratio of the areal density is too large, it affects the performance of the cathode material.
[0054] Preferably, the cathode material layer includes a Prussian blue-based cathode material.
[0055] The cathode material in the present invention is preferably a Prussian blue-based cathode material that matches the functional layer. Since the Prussian blue-based cathode material has coordinated water, a functional compound is required to cooperate in water absorption.
[0056] Preferably, the Prussian blue-based cathode material includes Na x M1[M2(CN)6] y ·zH2O, where 0 < x ≤ 2, for example, it can be 0.1, 0.5, 1, 1.5 or 2, 0.8 ≤ y < 1, for example, it can be 0.8, 0.85, 0.9, 0.95 or 0.99, 0 < z ≤ 20, for example, it can be 1, 5, 10, 15 or 20, and M1 and M2 are transition metal elements, and the transition metal elements include any one or a combination of at least two of Fe, Mn, Cu, Ni or Co.
[0057] Preferably, the cathode material layer further includes a first conductive agent and a first binder.
[0058] Preferably, the mass ratio of the Prussian blue-based cathode material, the first conductive agent and the first binder is (90 - 94):(1 - 6):(2 - 4), for example, it can be 90:6:4, 92:4:4 or 94:4:2, but is not limited to the listed values, and other unlisted values within the numerical range are equally applicable.
[0059] Preferably, the first conductive agent includes any one or a combination of at least two of SP, acetylene black, Ketjen black or conductive graphite.
[0060] Preferably, the first binder includes any one or a combination of at least two of PVDF, SBR, CMC, LA or PAA.
[0061] Preferably, the functional layer further includes a second conductive agent and a second binder.
[0062] Preferably, the mass ratio of the functional compound, the second conductive agent and the second binder is (90 - 94):(1 - 6):(2 - 4), for example, it can be 90:6:4, 92:4:4 or 94:4:2, but is not limited to the listed values, and other unlisted values within the numerical range are equally applicable.
[0063] Preferably, the second conductive agent includes any one of SP, acetylene black, Ketjen black or conductive graphite, or a combination of at least two thereof.
[0064] Preferably, the second binder includes any one of PVDF, SBR, CMC, LA or PAA, or a combination of at least two thereof.
[0065] In a specific embodiment, the present invention provides a method for preparing a positive electrode sheet as described in a specific embodiment, and the preparation method comprises the following steps:
[0066] (1) coating a positive electrode material layer slurry on at least one side of a current collector, and obtaining a positive electrode material layer on at least one side of the current collector after drying;
[0067] (2) coating the functional layer slurry on the surface of the positive electrode material layer in step (1), and drying to obtain the positive electrode sheet;
[0068] The functional layer slurry includes a functional compound, wherein the functional compound includes an amide group and a -COO - Group.
[0069] Preferably, the thickness of the positive electrode material layer slurry coating in step (1) is 40-60 μm, for example, 40 μm, 45 μm, 50 μm, 55 μm or 60 μm, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0070] Preferably, the thickness of the functional layer slurry coating in step (2) is 3-6 μm, for example, 3 μm, 4 μm, 5 μm or 6 μm, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0071] Preferably, the positive electrode material layer slurry includes a Prussian blue positive electrode material, a first conductive agent, a first binder and a solvent.
[0072] Preferably, the functional layer slurry comprises a functional compound, a second conductive agent, a second binder and a solvent.
[0073] Preferably, the drying temperature in step (1) is 100-150°C, for example, 100°C, 120°C, 140°C or 150°C, and the drying time is 0.5-12h, for example, 0.5h, 1h, 5h, 10 or 12h, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0074] Preferably, the drying temperature in step (2) is 100-150°C, for example, 100°C, 120°C, 140°C or 150°C, and the drying time is 0.5-2h, for example, 0.5h, 1h, 1.5 or 2h, but is not limited to the listed values, and other values within the numerical range not listed are also applicable.
[0075] Preferably, the drying in step (2) includes first heating and then vacuum drying, so as to remove moisture from the electrode.
[0076] In a specific embodiment, the present invention provides a sodium ion battery, which includes the positive electrode plate, or the positive electrode plate prepared by the preparation method.
[0077] Preferably, the sodium ion battery further comprises a diaphragm, and the functional layer in the positive electrode plate is arranged on a side of the positive electrode plate close to the diaphragm.
[0078] Since -COO in the functional compound - The group absorbs water so that the functional layer has a certain viscosity, thereby enhancing the viscosity between the positive electrode material and the separator. Therefore, the functional layer in the positive electrode sheet is preferably close to the separator side.
[0079] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0080] Example 1
[0081] This embodiment provides a positive electrode plate, the positive electrode plate comprising an aluminum foil and a coating disposed on both sides of the aluminum foil, the coating comprising a positive electrode material layer disposed on the surface of the aluminum foil, and a functional layer disposed on a side of the positive electrode material layer away from the aluminum foil;
[0082] The functional layer comprises a functional compound, SP and PVDF in a mass ratio of 90:6:4, wherein the functional compound is sodium lauroylamphoacetate;
[0083] The positive electrode material layer includes a Prussian blue positive electrode material, SP and PVDF in a mass ratio of 90:6:4. The Prussian blue positive electrode material is Na 1.73 Fe[Fe(CN)6]3·8H2O;
[0084] The surface density ratio of the functional layer to the positive electrode material layer is 1:9;
[0085] The method for preparing the positive electrode sheet comprises the following steps:
[0086] (1) Sodium lauroamphoacetate, SP and PVDF were weighed in a mass ratio of 90:6:4, and NMP (N-methylpyrrolidone) was added in a mass ratio of sodium lauroamphoacetate to N-methylpyrrolidone of 1:2, and the mixture was dispersed at a high speed and mixed to obtain slurry A;
[0087] (2) Prussian blue cathode material, SP and PVDF were weighed in a mass ratio of 90:6:4, and NMP was added in an amount of 1:2.2 of the mass ratio of the Prussian blue cathode material to NMP, and the mixture was dispersed at a high speed and mixed to obtain slurry B;
[0088] (3) Setting the coating machine parameters so that the coating thickness is 40 μm, slurry B is evenly coated on the aluminum foil, and the electrode after coating is dried by forced air at 110°C for 0.5 h to obtain electrode A;
[0089] (4) According to the functional layer, it is 20g / m 2 The surface density of the positive electrode material layer is 180g / m 2 The surface density is 100%, and the slurry A is evenly coated on the dried electrode piece A to make the coating thickness of the functional layer 3 μm. The coated electrode piece is blow-dried at 110° C. for 0.5 h, and then vacuum-dried at 120° C. for 12 h to obtain the positive electrode piece.
[0090] Example 2
[0091] This embodiment provides a positive electrode plate, the positive electrode plate comprising an aluminum foil and a coating disposed on one surface of the aluminum foil, the coating comprising a positive electrode material layer disposed on the surface of the aluminum foil, and a functional layer disposed on a side of the positive electrode material layer away from the aluminum foil;
[0092] The functional layer comprises a functional compound, SP and PVDF in a mass ratio of 94:4:2, wherein the functional compound is sodium lauroyl sarcosine;
[0093] The positive electrode material layer includes a Prussian blue positive electrode material, SP and PVDF in a mass ratio of 94:4:2, and the Prussian blue positive electrode material is Na4Fe(CN)6·10H2O;
[0094] The surface density ratio of the functional layer to the positive electrode material layer is 4:7;
[0095] The method for preparing the positive electrode sheet comprises the following steps:
[0096] (1) Sodium lauroyl sarcosine, SP and PVDF were weighed in a mass ratio of 94:4:2, and NMP was added in a mass ratio of sodium lauroyl sarcosine to N-methylpyrrolidone of 1:2, and the mixture was dispersed at a high speed and mixed to obtain slurry A;
[0097] (2) Prussian blue cathode material, SP and PVDF were weighed in a mass ratio of 94:4:2, and NMP was added in an amount of 1:2.2 of the mass ratio of the Prussian blue cathode material to NMP, and the mixture was dispersed at a high speed and mixed to obtain slurry B;
[0098] (3) Setting the coating machine parameters so that the coating thickness is 60 μm, slurry B is evenly coated on the aluminum foil, and the electrode after coating is dried by forced air at 110°C for 0.5 h to obtain electrode A;
[0099] (4) According to the functional layer, the 2 The surface density of the positive electrode material layer is 140g / m 2 The slurry A is evenly coated on the dried electrode piece A to make the coating thickness of the functional layer 6 μm, and the coated electrode piece is blow-dried at 110° C. for 0.5 h, and then vacuum-dried at 120° C. for 12 h to obtain the positive electrode piece.
[0100] Example 3
[0101] This embodiment provides a positive electrode plate, the positive electrode plate comprising an aluminum foil and a coating disposed on both sides of the aluminum foil, the coating comprising a positive electrode material layer disposed on the surface of the aluminum foil, and a functional layer disposed on a side of the positive electrode material layer away from the aluminum foil;
[0102] The functional layer comprises a functional compound, SP and PVDF in a mass ratio of 92:5:3, wherein the functional compound is sodium lauroamphoacetate;
[0103] The positive electrode material layer includes a Prussian blue positive electrode material, SP and PVDF in a mass ratio of 92:5:3. The Prussian blue positive electrode material is Na 1.79 Fe[Fe(CN)6]·0.16H2O;
[0104] The ratio of the surface density of the functional layer to the surface density of the positive electrode material layer is 2:5;
[0105] The method for preparing the positive electrode sheet comprises the following steps:
[0106] (1) Sodium lauroyl amphoacetate, SP and PVDF were weighed in a mass ratio of 92:5:3, and NMP was added in a mass ratio of sodium lauroyl amphoacetate to N-methylpyrrolidone of 1:2, and the mixture was dispersed at a high speed and mixed to obtain slurry A;
[0107] (2) Prussian blue cathode material, SP and PVDF were weighed in a mass ratio of 92:5:3, and NMP was added in an amount of 1:2.2 of the mass ratio of the Prussian blue cathode material to NMP, and the mixture was dispersed at a high speed and mixed to obtain slurry B;
[0108] (3) Setting the coating machine parameters so that the coating thickness is 50 μm, slurry B is evenly coated on the aluminum foil, and the electrode after coating is dried by forced air at 110°C for 0.5 h to obtain electrode A;
[0109] (4) According to the functional layer, it is 60g / m 2 The surface density of the positive electrode material layer is 150g / m 2 The slurry A is evenly coated on the dried electrode piece A to make the coating thickness of the functional layer 5 μm, and the coated electrode piece is blow-dried at 110° C. for 0.5 h, and then vacuum-dried at 120° C. for 12 h to obtain the positive electrode piece.
[0110] Example 4
[0111] This embodiment provides a positive electrode plate, in which the surface density ratio of the functional layer to the positive electrode material layer is 1:10, and the surface density of the functional layer is 20 g / m 2 The surface density of the positive electrode material layer is 200 g / m 2 Except for this, the rest are the same as in Example 1.
[0112] Example 5
[0113] This embodiment provides a positive electrode sheet, in which the surface density ratio of the functional layer to the positive electrode material layer is 5:5, and the surface density of the functional layer is 100 g / m 2 The surface density of the positive electrode material layer is 100 g / m 2 Except for this, the rest are the same as in Example 1.
[0114] Example 6
[0115] This embodiment provides a positive electrode plate, which is the same as that of Embodiment 1 except that the functional compound is butyl ester pendant amide.
[0116] Example 7
[0117] This embodiment provides a positive electrode plate, which is the same as that of Embodiment 1 except that the functional compound is sodium cocoyl glycinate.
[0118] Example 8
[0119] This embodiment provides a positive electrode plate, which is the same as that of Embodiment 1 except that the functional compound is sodium N-decanoyl glutamate.
[0120] Example 9
[0121] This embodiment provides a positive electrode plate, which is the same as that of embodiment 1 except that the Prussian blue positive electrode material is replaced by a layered oxide positive electrode material. The layered oxide positive electrode material is Na 2 / 3Ni 1 / 3 Mn 2 / 3 O2.
[0122] Example 10
[0123] This embodiment provides a positive electrode plate, which is the same as that of embodiment 1 except that the mass of the Prussian blue positive electrode material is replaced by a polyanion positive electrode material. The polyanion positive electrode material is Na 2 / 3FePO4.
[0124] Comparative Example 1
[0125] This comparative example provides a positive electrode plate, which is the same as Example 1 except that it does not contain a functional layer.
[0126] Comparative Example 2
[0127] This comparative example provides a positive electrode plate, which is the same as Example 1 except that the functional compound is benzamide.
[0128] Comparative Example 3
[0129] This comparative example provides a positive electrode plate, which is the same as Example 1 except that the functional compound is ethyl acetate.
[0130] The above examples and comparative examples were used to prepare the battery:
[0131] Preparation of positive electrode sheet: After rolling, the positive electrode sheets obtained in the above embodiments and comparative examples were punched into positive electrode sheets with a diameter of φ14 mm (φ represents the diameter) using a punching machine;
[0132] Preparation of negative electrode sheet: negative electrode hard carbon material, conductive carbon black, binder PVDF and solvent NMP are mixed in a ratio of 8:1:1 to make negative electrode slurry, the negative electrode slurry is evenly coated on copper foil in a certain proportion, and vacuum dried at 80°C, the negative electrode sheet is rolled and then punched into a φ16mm negative electrode sheet by a punching machine;
[0133] The diaphragm was Whatman GF / D glass fiber, and the electrolyte was 1 mol / L NaPF6 in diglyme.
[0134] Battery preparation: Assemble the full battery in the order of positive electrode shell, positive electrode sheet, separator, negative electrode sheet, nickel foam and negative electrode shell. Clamp the assembled full battery with insulating tweezers and place it on a packaging machine for sealing. Finally, let the packaged full battery stand for 24 hours to allow the electrolyte to fully infiltrate the electrode materials before conducting electrochemical tests.
[0135] Test method:
[0136] First cycle capacity test: The sodium ion batteries prepared in the embodiment and the comparative example were respectively taken and first cycle capacity tests were performed under the test conditions of 25°C, 0.2 C rate, 4.8 V charge cut-off voltage, and 2.0 V discharge cut-off voltage.
[0137] 1C / 1C cycle life test: The sodium ion batteries prepared in the embodiment and the comparative example were respectively taken and divided under the test conditions of 0.2 C rate, charge cut-off voltage 4.8 V, and discharge cut-off voltage 2.0 V at 25°C, and then a 1C / 1C cycle test was performed at 25°C (charge cut-off voltage 4.8 V, discharge cut-off voltage 2.0 V).
[0138] CO2 gas content test: The sodium ion battery made by the embodiment and the comparative example and cycled for three weeks was subjected to a needle-piercing gas production test to measure the gas production and the gas composition. The test process is: leave it at 25°C for 5 min, discharge it at 1 C to 2.0 V, leave it for 10 min, charge it at 1 C constant current and constant voltage to 4.8 V, the cut-off current is 0.05 C, leave it for 10 min, leave the battery at 25°C for 2 h, test the single-point internal pressure by needle-piercing, collect gas, and test the gas composition.
[0139] The measured initial charge and discharge capacity, coulomb efficiency, 1C / 1C cycle life and CO2 gas content after three weeks of cycling of the button battery are shown in Table 1:
[0140] Table 1
[0141]
[0142] From the above table we can see that:
[0143] (1) It can be seen from Examples 1-3 and Comparative Example 1 that the functional layer of the present invention can prevent the dissolution of metal in the positive electrode material, absorb the carbon dioxide generated by the side reaction between the positive electrode material and the electrolyte, and absorb water to replenish sodium ions. Therefore, the setting of the functional layer of the present invention can improve the first-cycle charge and discharge specific capacity, first-cycle coulomb efficiency and cycle life of the battery, and can also reduce the carbon dioxide content in the battery; It can be seen from Examples 1 and Comparative Examples 2-3 that the functional compound in Comparative Example 2 is benzamide containing only amide groups, and the functional compound in Comparative Example 3 is -COO - The functional compounds described in Examples 1-3 also contain amide groups, -COO - The groups and sodium ions can prevent the dissolution of metals in the positive electrode materials, absorb carbon dioxide and water, and replenish sodium ions, which can simultaneously improve the cycle life of the battery and reduce the gas production of the battery.
[0144] (2) It can be seen from Examples 1 and 4-5 that the surface density ratio of the functional layer and the positive electrode material layer of the present invention will affect the performance of the functional layer and the positive electrode material. If the surface density ratio is too small, such as in Example 4, the effect of the functional layer will not be obvious. If the surface density ratio is too large, the volatilization of the positive electrode material performance will be affected, thereby affecting the battery's first-cycle charge and discharge capacity, first-cycle coulomb efficiency, cycle life and CO2 gas content; It can be seen from Examples 1 and 6 that when the functional compound of the present invention contains sodium ions, the functional compound can also act as a sodium supplement to additionally supplement sodium ions, thereby improving the battery's first-cycle coulomb efficiency, cycle life and first-cycle charge and discharge capacity.
[0145] (3) It can be seen from Examples 1 and 7-8 that the functional compound of the present invention is preferably sodium lauroyl amphoacetate, sodium lauroyl sarcosinate or sodium cocoyl glycinate, which is more effective than other functional compounds containing amide groups, -COO - The compound of the group and sodium ion is more stable to high temperature, acid and alkali, and can promote the effect of the functional layer, thereby improving the first-cycle charge and discharge specific capacity, the first-cycle coulomb efficiency and the cycle life of the battery; it can be seen from Example 1 and Examples 9-10 that the functional layer of the present invention is preferably matched with the Prussian blue positive electrode material. Due to the presence of coordinated water in the Prussian blue positive electrode material, the functional compound is required to absorb water. The water-absorbing functional layer has a certain viscosity, which can enhance the viscosity between the positive electrode material and the diaphragm, thereby improving the battery cycle performance, while also improving the first-cycle charge and discharge specific capacity and the first-cycle coulomb efficiency, and reducing the carbon dioxide content in the battery.
[0146] In summary, the present invention provides a positive electrode plate and a preparation method and application thereof. The positive electrode plate prevents metal dissolution in the positive electrode material by arranging a functional layer containing a specific group functional compound on the surface of the positive electrode material layer away from the current collector, absorbs carbon dioxide generated by the side reaction of the positive electrode material and the electrolyte, and can also absorb water, thereby improving the electrochemical performance, safety performance and service life of the battery.
[0147] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention are within the protection scope and disclosure scope of the present invention.
Claims
1. A positive electrode sheet, characterized in that: The positive electrode sheet includes a current collector and a coating disposed on at least one side of the current collector, wherein the coating includes a positive electrode material layer disposed on the surface of the current collector, and a functional layer disposed on a side of the positive electrode material layer away from the current collector; The functional layer includes a functional compound, wherein the functional compound includes an amide group and a -COO - Group; The functional compound also includes sodium ions; The functional compound includes a sodium salt of an organic acid containing an amide group.
2. The positive electrode sheet according to claim 1, characterized in that: The organic acid sodium salt containing an amide group includes any one of sodium lauroyl amphoacetate, sodium lauroyl sarcosinate or sodium cocoyl glycinate, or a combination of at least two thereof.
3. The positive electrode sheet according to claim 1 or 2, characterized in that: The surface density ratio of the functional layer to the positive electrode material layer is (1-4):(5-9).
4. The positive electrode sheet according to claim 1 or 2, characterized in that: The positive electrode material layer includes a Prussian blue positive electrode material; The Prussian blue-based cathode material includes Na x M1[M2(CN)6] y ·zH2O, where 0 < x ≤ 2, 0.8 ≤ y < 1, 0 < z ≤ 20, and M1 and M2 are transition metal elements.
5. The positive electrode sheet according to claim 4, characterized in that: The positive electrode material layer further includes a first conductive agent and a first binder; The mass ratio of the Prussian blue positive electrode material, the first conductive agent and the first binder is (90-94):(1-6):(2-4).
6. The positive electrode sheet according to claim 1 or 2, characterized in that: The functional layer further includes a second conductive agent and a second binder; The mass ratio of the functional compound, the second conductive agent and the second binder is (90-94):(1-6):(2-4).
7. A method for preparing a positive electrode sheet according to any one of claims 1 to 6, characterized in that: The preparation method comprises the following steps: (1) coating a positive electrode material layer slurry on at least one side of a current collector, and drying the slurry to obtain a positive electrode material layer on at least one side of the current collector; (2) coating the functional layer slurry on the surface of the positive electrode material layer in step (1), and obtaining the positive electrode sheet after drying; The functional layer slurry includes a functional compound, wherein the functional compound includes an amide group and a -COO - Group.
8. The preparation method according to claim 7, characterized in that: The thickness of the positive electrode material layer slurry coating in step (1) is 40-60 μm; And / or, the thickness of the functional layer slurry coating in step (2) is 3-6 μm.
9. A sodium ion battery, characterized in that: The sodium ion battery comprises the positive electrode sheet as described in any one of claims 1 to 6, or the positive electrode sheet prepared by the preparation method as described in claim 7 or 8.
10. The sodium ion battery according to claim 9, characterized in that: The sodium ion battery further includes a diaphragm, and the functional layer in the positive electrode plate is arranged on a side of the positive electrode plate close to the diaphragm.