A method for temporarily extending the setting time of water-stable mixture

By adding white sugar and modified straw to the water-stabilized mixture, the setting time is extended, the problem of waste and strength loss caused by construction delays is solved, the mechanical properties and corrosion resistance of the mixture are improved, and it is suitable for high temperature environments and long distances. Construction of water-stabilized layer for transportation.

CN118439841BActive Publication Date: 2024-10-25POLY CHANGDA ENGINEERING CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410903706.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-08
Publication Date
2024-10-25
Estimated Expiration
2044-07-08

AI Technical Summary

Technical Problem

In the construction of water-stabilized mixtures, the construction delay time is too long, which exceeds the initial setting time of cement, making it difficult to unload, resulting in waste and strength loss. In addition, factors such as high temperature environment and long-distance transportation increase construction costs and waste of resources. .

Method used

By adding white sugar to the water-stable mixture to adsorb tricalcium silicate particles, preventing the formation of hydrated calcium silicate crystals, prolonging the setting time, and using straw as the basic material, through the modification of polydopamine and boron nitride, Improve the hydrophilicity and interfacial properties of straw, and enhance the mechanical properties and corrosion resistance of the mixture.

Benefits of technology

It effectively extends the setting time of the water-stabilized mixture, improves its mechanical properties and corrosion resistance, reduces construction costs and waste of resources, and is suitable for water-stabilized layer construction in high-temperature environments and long-distance transportation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention relates to a method for temporarily extending the setting time of a water-stabilized mixture, and belongs to the technical field of building materials. The invention discloses a method for temporarily extending the setting time of a water-stabilized mixture, wherein white sugar is added to the mixture, and a large number of polyhydroxyl groups contained in the white sugar will be adsorbed on tricalcium silicate particles that have not yet been hydrated, thereby destroying the hydrated calcium silicate crystals formed on the surface, preventing the formation of crystals, and playing a role in extending the setting time; in addition, straw is used as a basic material, and its surface is modified using polydopamine and boron nitride, so that catechol and amino groups are introduced into the surface of the modified straw, the surface hydrophilicity of the straw is improved, the interface performance between the straw and the mixture is enhanced, and the mechanical properties of the mixture are improved, and the loading of boron nitride enhances the corrosion resistance of the mixture.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of building materials and relates to a method for temporarily prolonging the setting time of a water-stabilized mixture. Background Art

[0002] Water-stabilized mixture has the advantages of high strength and stiffness, good water stability, frost resistance, and good overall stability. It is widely used in highway base and subbase structures of various levels at home and abroad. However, in the construction of the water-stabilized layer of the pavement, the construction delay time is often too long, exceeding the initial setting time of the cement, making it difficult to unload the material, resulting in waste or shutdown. When the construction delay time is too long, rolling will also destroy the cement colloid that has been formed, which will not only consume additional compaction work and affect the compaction degree, but also damage the cement binder that has been formed, and its gelling effect cannot be exerted, resulting in strength loss. When encountering projects with limited transportation distance and weather, measures such as increasing the amount of cement are often the only way to compensate for the strength loss caused by time delay, which increases construction costs and causes a certain amount of resource waste. Therefore, it is necessary to extend the allowable retention time for the construction of water-stabilized mixtures to solve the technical problems of long-distance transportation and continuous paving of two layers of water-stabilized layers in high temperature environments. Summary of the invention

[0003] The present invention relates to a method for temporarily extending the setting time of a water-stabilized mixture, and belongs to the technical field of mixtures. The present invention discloses a method for temporarily extending the setting time of a water-stabilized mixture, wherein white sugar is added to the mixture, and a large number of polyhydroxyl groups contained in the white sugar will be adsorbed on tricalcium silicate particles that have not yet been hydrated, thereby destroying the hydrated calcium silicate crystals formed on the surface, preventing the formation of crystals, and playing a role in extending the setting time; in addition, straw is used as a basic material, and its surface is modified using polydopamine and boron nitride, so that catechol and amino groups are introduced into the surface of the modified straw, the surface hydrophilicity of the straw is improved, and the interface performance between the straw and the mixture is enhanced, thereby improving the mechanical properties of the mixture, and at the same time, the loading of boron nitride enhances the corrosion resistance of the mixture.

[0004] The purpose of the present invention can be achieved through the following technical solutions:

[0005] A method for temporarily extending the setting time of a water-stabilized mixture, the method specifically comprising: stirring cement clinker, fly ash, mineral powder, gypsum, silica powder and water at a rotation speed of 1000-1200 rpm, then adding modified straw and white sugar and continuing stirring to obtain a temporarily extended water-stabilized mixture.

[0006] Furthermore, the mixture comprises the following raw materials in parts by weight: 60-70 parts of cement clinker, 10-20 parts of fly ash, 10-16 parts of mineral powder, 1-3 parts of gypsum, 1-3 parts of silicon powder, 10-20 parts of modified straw, 1-5 parts of white sugar, and 150-200 parts of water.

[0007] Furthermore, the preparation method of the modified straw comprises the following steps:

[0008] A1: The straw is dried, cut and crushed, soaked in an acetone solution, subjected to ultrasonic treatment, the solution is removed and the straw is washed with distilled water, and then dried to obtain pretreated straw;

[0009] A2: dopamine is mixed and dissolved with deionized water, and tris(hydroxymethyl)aminomethane hydrochloride) is added to adjust the pH value to obtain a mixed solution;

[0010] A3: The pretreated straw is mixed with the mixed solution and subjected to ultrasonic treatment, turned over every 30 minutes, and then filtered. The solid is washed with distilled water and placed in a drying oven to dry to obtain the modified straw primary product;

[0011] A4: Boron nitride is stirred and mixed with water and ethanol solution, and then polyethylene glycol is added, and ammonia water is added dropwise and stirred continuously to form a mixed solution a;

[0012] A5: The modified straw primary product is immersed in the mixed solution a and simultaneously subjected to ultrasonic treatment. After the solution is removed, the modified straw is dried to obtain the modified straw.

[0013] Furthermore, in step A1, the straw is one of rice straw, corn straw, cotton straw and wheat straw, the solid-liquid ratio of the straw to the acetone solution is 1-3:20-25 g / mL, the mass concentration of the acetone solution is 20-30%, and the ultrasonic treatment time is 2-3 h.

[0014] Furthermore, in the step A2, the solid-liquid ratio of dopamine to deionized water is 2-3:1 g / L, and the pH value is 8-9.

[0015] Furthermore, in step A3, the solid-liquid ratio of the pretreated straw to the mixed liquid is 1-5:0.1 g / L, the time and temperature of the ultrasonic treatment are 20-24 h and 20-30° C., respectively, and the temperature and time of the drying are 40-55° C. and 10-16 h, respectively.

[0016] Furthermore, in step A4, the solid-liquid ratio of the total volume of boron nitride to water, ethanol solution, polyethylene glycol, and ammonia water is 10-20:0.5 g / L, wherein the volume ratio of water, ethanol solution, polyethylene glycol, and ammonia water is 1:1:0.5:0.01, the mass concentration of the ethanol solution is 75%, and the mass concentration of the ammonia water is 26%.

[0017] Furthermore, in step A5, the solid-liquid ratio of the modified straw primary product to the mixed solution a is 1-3:0.5 g / L, the ultrasonic time is 5-6 h, and the drying time and temperature are 30-40 min and 100-130° C. respectively.

[0018] Beneficial effects of the present invention:

[0019] 1. The main components of the mixture are tricalcium silicate, dicalcium silicate, tricalcium aluminate and tetracalcium aluminoferrate. When an appropriate amount of water is added to cement, these minerals will undergo a hydration reaction and eventually form hydrated calcium silicate crystals. By adding white sugar to the mixture, the large amount of polyhydroxy groups it contains will be adsorbed on the tricalcium silicate particles that have not yet hydrated, thereby destroying the hydrated calcium silicate crystals formed on the surface, preventing the formation of crystals, and playing a role in extending the setting time;

[0020] 2. The present invention uses straw as a base material and uses polydopamine and boron nitride to modify its surface, so that catechol and amino groups are introduced into the surface of the modified straw, the surface hydrophilicity of the straw is improved, the interface performance between the straw and the mixture is enhanced, and then the mechanical properties of the mixture are improved. At the same time, the loading of boron nitride enhances the corrosion resistance of the mixture. DETAILED DESCRIPTION

[0021] In order to further illustrate the technical means and effects adopted by the present invention to achieve the predetermined invention purpose, the specific implementation methods, structures, features and effects of the present invention are described in detail below in combination with embodiments.

[0022] Example 1

[0023] A method for temporarily extending the setting time of a water-stabilized mixture, the method specifically comprising: stirring cement clinker, fly ash, mineral powder, gypsum, silica powder and water at a rotation speed of 1000 rpm, then adding modified straw and white sugar and continuing stirring to obtain a temporarily extended water-stabilized mixture.

[0024] The mixture comprises the following raw materials in parts by weight: 60 parts of cement clinker, 10 parts of fly ash, 10 parts of mineral powder, 1 part of gypsum, 1 part of silicon powder, 10 parts of modified straw, 1 part of white sugar, and 150 parts of water.

[0025] The preparation method of the modified straw comprises the following steps:

[0026] A1: The straw is dried, cut and crushed, soaked in an acetone solution, subjected to ultrasonic treatment, the solution is removed and the straw is washed with distilled water, and then dried to obtain pretreated straw;

[0027] A2: dopamine is mixed and dissolved with deionized water, and tris(hydroxymethyl)aminomethane hydrochloride) is added to adjust the pH value to obtain a mixed solution;

[0028] A3: The pretreated straw is mixed with the mixed solution and subjected to ultrasonic treatment, turned over every 30 minutes, and then filtered. The solid is washed with distilled water and placed in a drying oven to dry to obtain the modified straw primary product;

[0029] A4: Boron nitride is stirred and mixed with water and ethanol solution, and then polyethylene glycol is added, and ammonia water is added dropwise and stirred continuously to form a mixed solution a;

[0030] A5: The modified straw primary product is immersed in the mixed solution a and simultaneously subjected to ultrasonic treatment. After the solution is removed, the modified straw is dried to obtain the modified straw.

[0031] In step A1, the straw is rice straw, the solid-liquid ratio of the straw to the acetone solution is 1:20 g / mL, the mass concentration of the acetone solution is 20%, and the ultrasonic treatment time is 2 h.

[0032] In the step A2, the solid-liquid ratio of dopamine to deionized water is 2:1 g / L, and the pH value is 8.

[0033] In the step A3, the solid-liquid ratio of the pretreated straw to the mixed liquid is 1:0.1 g / L, the time and temperature of the ultrasonic treatment are 20 h and 20° C., and the temperature and time of the drying are 40° C. and 10 h.

[0034] In step A4, the solid-liquid ratio of boron nitride to the total volume of water, ethanol solution, polyethylene glycol, and ammonia water is 10:0.5 g / L, wherein the volume ratio of water, ethanol solution, polyethylene glycol, and ammonia water is 1:1:0.5:0.01, the mass concentration of the ethanol solution is 75%, and the mass concentration of the ammonia water is 26%.

[0035] In the step A5, the solid-liquid ratio of the modified straw primary product to the mixed solution a is 1:0.5 g / L, the ultrasonic time is 5 h, and the drying time and temperature are 30 min and 100° C. respectively.

[0036] The cement clinker is purchased from: cement clinker / Hanyou, the fly ash is purchased from: fly ash / Benno, the mineral powder is purchased from: mineral powder / Aohong, and the silica powder is purchased from: silica powder /

[0037] Hanxinzun-7440-21-3.

[0038] Example 2

[0039] A method for temporarily extending the setting time of a water-stabilized mixture, the method specifically comprising: stirring cement clinker, fly ash, mineral powder, gypsum, silica powder and water at a rotation speed of 1100 rpm, then adding modified straw and white sugar and continuing stirring to obtain a temporarily extended water-stabilized mixture.

[0040] The mixture comprises the following raw materials in parts by weight: 65 parts of cement clinker, 15 parts of fly ash, 13 parts of mineral powder, 2 parts of gypsum, 2 parts of silicon powder, 15 parts of modified straw, 3 parts of white sugar, and 175 parts of water.

[0041] The preparation method of the modified straw comprises the following steps:

[0042] A1: The straw is dried, cut and crushed, soaked in an acetone solution, subjected to ultrasonic treatment, the solution is removed and the straw is washed with distilled water, and then dried to obtain pretreated straw;

[0043] A2: dopamine is mixed and dissolved with deionized water, and tris(hydroxymethyl)aminomethane hydrochloride) is added to adjust the pH value to obtain a mixed solution;

[0044] A3: The pretreated straw is mixed with the mixed solution and subjected to ultrasonic treatment, turned over every 30 minutes, and then filtered. The solid is washed with distilled water and placed in a drying oven to dry to obtain the modified straw primary product;

[0045] A4: Boron nitride is stirred and mixed with water and ethanol solution, and then polyethylene glycol is added, and ammonia water is added dropwise and stirred continuously to form a mixed solution a;

[0046] A5: The modified straw primary product is immersed in the mixed solution a and simultaneously subjected to ultrasonic treatment. After the solution is removed, the modified straw is dried to obtain the modified straw.

[0047] In step A1, the straw is corn straw, the solid-liquid ratio of the straw to the acetone solution is 2:23 g / mL, the mass concentration of the acetone solution is 25%, and the ultrasonic treatment time is 2.5 h.

[0048] In the step A2, the solid-liquid ratio of dopamine to deionized water is 2.5:1 g / L, and the pH value is 8.5.

[0049] In the step A3, the solid-liquid ratio of the pretreated straw to the mixed liquid is 3:0.1 g / L, the time and temperature of the ultrasonic treatment are 22 h and 25° C., and the temperature and time of the drying are 50° C. and 13 h.

[0050] In step A4, the solid-liquid ratio of boron nitride to the total volume of water, ethanol solution, polyethylene glycol, and ammonia water is 15:0.5 g / L, wherein the volume ratio of water, ethanol solution, polyethylene glycol, and ammonia water is 1:1:0.5:0.01, the mass concentration of the ethanol solution is 75%, and the mass concentration of the ammonia water is 26%.

[0051] In the step A5, the solid-liquid ratio of the modified straw primary product to the mixed solution a is 2:0.5 g / L, the ultrasonic time is 5.5 h, and the drying time and temperature are 35 min and 115° C. respectively.

[0052] The cement clinker is purchased from: cement clinker / Hanyou, the fly ash is purchased from: fly ash / Benno, the mineral powder is purchased from: mineral powder / Aohong, and the silica powder is purchased from: silica powder /

[0053] Hanxinzun-7440-21-3.

[0054] Example 3

[0055] A method for temporarily extending the setting time of a water-stabilized mixture, the method specifically comprising: stirring cement clinker, fly ash, mineral powder, gypsum, silica powder and water at a rotation speed of 1200 rpm, then adding modified straw and white sugar and continuing stirring to obtain a temporarily extended water-stabilized mixture.

[0056] The mixture comprises the following raw materials in parts by weight: 70 parts of cement clinker, 20 parts of fly ash, 16 parts of mineral powder, 3 parts of gypsum, 3 parts of silicon powder, 20 parts of modified straw, 5 parts of white sugar, and 200 parts of water.

[0057] The preparation method of the modified straw comprises the following steps:

[0058] A1: The straw is dried, cut and crushed, soaked in an acetone solution, subjected to ultrasonic treatment, the solution is removed and the straw is washed with distilled water, and then dried to obtain pretreated straw;

[0059] A2: dopamine is mixed and dissolved with deionized water, and tris(hydroxymethyl)aminomethane hydrochloride) is added to adjust the pH value to obtain a mixed solution;

[0060] A3: The pretreated straw is mixed with the mixed solution and subjected to ultrasonic treatment, turned over every 30 minutes, and then filtered. The solid is washed with distilled water and placed in a drying oven to dry to obtain the modified straw primary product;

[0061] A4: Boron nitride is stirred and mixed with water and ethanol solution, and then polyethylene glycol is added, and ammonia water is added dropwise and stirred continuously to form a mixed solution a;

[0062] A5: The modified straw primary product is immersed in the mixed solution a and simultaneously subjected to ultrasonic treatment. After the solution is removed, the modified straw is dried to obtain the modified straw.

[0063] In step A1, the straw is cotton straw, the solid-liquid ratio of the straw to the acetone solution is 3:25 g / mL, the mass concentration of the acetone solution is 30%, and the ultrasonic treatment time is 3 h.

[0064] In the step A2, the solid-liquid ratio of dopamine to deionized water is 3:1 g / L, and the pH value is 9.

[0065] In the step A3, the solid-liquid ratio of the pretreated straw to the mixed liquid is 5:0.1 g / L, the time and temperature of the ultrasonic treatment are 24 h and 30° C., and the temperature and time of the drying are 55° C. and 16 h.

[0066] In step A4, the solid-liquid ratio of the total volume of boron nitride to water, ethanol solution, polyethylene glycol, and ammonia water is 20:0.5 g / L, wherein the volume ratio of water, ethanol solution, polyethylene glycol, and ammonia water is 1:1:0.5:0.01, the mass concentration of the ethanol solution is 75%, and the mass concentration of the ammonia water is 26%.

[0067] In the step A5, the solid-liquid ratio of the modified straw primary product to the mixed solution a is 3:0.5 g / L, the ultrasonic time is 6 hours, and the drying time and temperature are 40 minutes and 130° C. respectively.

[0068] The cement clinker is purchased from: cement clinker / Hanyou, the fly ash is purchased from: fly ash / Benno, the mineral powder is purchased from: mineral powder / Aohong, and the silica powder is purchased from: silica powder /

[0069] Hanxinzun-7440-21-3.

[0070] Comparative Example 1

[0071] On the basis of Example 2, white sugar was removed from the raw material components, and other conditions were consistent with Example 2.

[0072] Comparative Example 2

[0073] On the basis of Example 2, the amount of white sugar added to the raw material components of the temporary extended water-stabilized mixture is 10 parts by weight, and other conditions are consistent with Example 2.

[0074] Comparative Example 3

[0075] Based on Example 2, a method for temporarily prolonging the setting time of a water-stabilized mixture is provided. The method is specifically as follows: cement clinker, fly ash, mineral powder, gypsum, silica powder and water are stirred at a rotation speed of 1100 rpm, and then modified straw a and white sugar are added and stirred continuously to obtain a temporarily prolonging water-stabilized mixture.

[0076] The mixture comprises the following raw materials in parts by weight: 65 parts of cement clinker, 15 parts of fly ash, 13 parts of mineral powder, 2 parts of gypsum, 2 parts of silicon powder, 15 parts of modified straw, 3 parts of white sugar, and 175 parts of water.

[0077] The preparation method of the modified straw a comprises the following steps:

[0078] A1: The straw is dried, cut, and crushed, soaked in an acetone solution, subjected to ultrasonic treatment, the solution is removed, and the straw is washed with distilled water, and then dried to obtain pretreated straw a;

[0079] A2: dopamine is mixed and dissolved with deionized water, and tris(hydroxymethyl)aminomethane hydrochloride) is added to adjust the pH value to obtain a mixed solution;

[0080] A3: The pretreated straw a is mixed with the mixed solution and subjected to ultrasonic treatment, turned over every 30 minutes, and then filtered. The solid is washed with distilled water and placed in a drying oven to dry to obtain modified straw a.

[0081] In step A1, the straw is corn straw, the solid-liquid ratio of the straw to the acetone solution is 2:23 g / mL, the mass concentration of the acetone solution is 25%, and the ultrasonic treatment time is 2.5 h.

[0082] In the step A2, the solid-liquid ratio of dopamine to deionized water is 2.5:1 g / L, and the pH value is 8.5.

[0083] In the step A3, the solid-liquid ratio of the pretreated straw a to the mixed liquid is 3:0.1 g / L, the time and temperature of the ultrasonic treatment are 22 h and 25° C., and the temperature and time of the drying are 50° C. and 13 h.

[0084] The cement clinker is purchased from: cement clinker / Hanyou, the fly ash is purchased from: fly ash / Benno, the mineral powder is purchased from: mineral powder / Aohong, and the silica powder is purchased from: silica powder /

[0085] Hanxinzun-7440-21-3.

[0086] Comparative Example 4

[0087] Based on Example 2, a method for temporarily prolonging the setting time of a water-stabilized mixture is provided. Specifically, the method comprises: stirring cement clinker, fly ash, mineral powder, gypsum, silica powder and water at a rotation speed of 1100 rpm, and then adding modified straw b and white sugar and continuing to stir to obtain a temporarily prolonging water-stabilized mixture.

[0088] The mixture comprises the following raw materials in parts by weight: 65 parts of cement clinker, 15 parts of fly ash, 13 parts of mineral powder, 2 parts of gypsum, 2 parts of silicon powder, 15 parts of modified straw, 3 parts of white sugar, and 175 parts of water.

[0089] The preparation method of the modified straw b comprises the following steps:

[0090] A1: The straw is dried, cut and crushed, soaked in an acetone solution, subjected to ultrasonic treatment, the solution is removed and the straw is washed with distilled water, and then dried to obtain pretreated straw b;

[0091] A2: Boron nitride is stirred and mixed with water and ethanol solution, and then polyethylene glycol is added, and ammonia water is added dropwise and stirred continuously to form a mixed solution a;

[0092] A3: The pretreated straw b is immersed in the mixed solution a and simultaneously subjected to ultrasonic treatment. After the solution is removed, the modified straw b is obtained by drying.

[0093] In step A1, the straw is corn straw, the solid-liquid ratio of the straw to the acetone solution is 2:23 g / mL, the mass concentration of the acetone solution is 25%, and the ultrasonic treatment time is 2.5 h.

[0094] In step A2, the solid-liquid ratio of the total volume of boron nitride to water, ethanol solution, polyethylene glycol, and ammonia water is 15:0.5 g / L, wherein the volume ratio of water, ethanol solution, polyethylene glycol, and ammonia water is 1:1:0.5:0.01, the mass concentration of the ethanol solution is 75%, and the mass concentration of the ammonia water is 26%.

[0095] In the step A3, the solid-liquid ratio of the pretreated straw b to the mixed solution a is 2:0.5 g / L, the ultrasonic time is 5.5 h, and the drying time and temperature are 35 min and 115° C. respectively.

[0096] The cement clinker is purchased from: cement clinker / Hanyou, the fly ash is purchased from: fly ash / Benno, the mineral powder is purchased from: mineral powder / Aohong, and the silica powder is purchased from: silica powder /

[0097] Hanxinzun-7440-21-3.

[0098] Performance Testing

[0099] 1. According to the setting time and 28d compressive strength tested in patent CN108046651B, Examples 1-3 and Comparative Examples 1-4 were tested respectively.

[0100] The above test results are shown in Table 1.

[0101] Table 1 Test results

[0102]

[0103] From the data analysis in Table 1, it can be concluded that the setting time of Examples 1-3 is greater than that of Comparative Example 1 and less than that of Comparative Example 2, and the 28d compressive strength / MPa of Examples 1-3 are greater than that of Comparative Examples 1-4. In Comparative Example 1, no white sugar was added, and its setting time was fast and the compressive strength decreased; in Comparative Example 2, the amount of white sugar added was greater than that of the embodiment, and its setting time was slowed down, and the strength decreased due to the delayed cement hydration reaction; in Comparative Example 3, the straw was not modified with polydopamine, and its hydrophilicity was lower than that of the embodiment, and the mechanical properties decreased; in Comparative Example 4, the straw was not surface loaded with boron nitride, and its corrosion resistance decreased, and then the mechanical properties were affected after a period of time.

[0104] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technical personnel in this field can make some changes or modify the technical contents disclosed above into equivalent embodiments without departing from the scope of the technical solution of the present invention. However, any brief modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention are still within the scope of the technical solution of the present invention.

Claims

1. A method for temporarily extending the setting time of a water-stable mixture, characterized in that: The method specifically comprises: stirring cement clinker, fly ash, mineral powder, gypsum, silica powder and water at a rotation speed of 1000-1200 rpm, then adding modified straw and white sugar and continuing stirring to obtain a temporary extended water-stable mixture; The mixture comprises the following raw materials in parts by weight: 60-70 parts of cement clinker, 10-20 parts of fly ash, 10-16 parts of mineral powder, 1-3 parts of gypsum, 1-3 parts of silicon powder, 10-20 parts of modified straw, 1-5 parts of white sugar, and 150-200 parts of water; The preparation method of the modified straw comprises the following steps: A1: The straw is dried, cut and crushed, soaked in an acetone solution, subjected to ultrasonic treatment, the solution is removed and the straw is washed with distilled water, and then dried to obtain pretreated straw; A2: dopamine is mixed and dissolved with deionized water, and tris(hydroxymethyl)aminomethane hydrochloride) is added to adjust the pH value to obtain a mixed solution; A3: The pretreated straw is mixed with the mixed solution and subjected to ultrasonic treatment, turned over every 30 minutes, and then filtered. The solid is washed with distilled water and placed in a drying oven to dry to obtain the modified straw primary product; A4: Boron nitride is stirred and mixed with water and ethanol solution, and then polyethylene glycol is added, and ammonia water is added dropwise and stirred continuously to form a mixed solution a; A5: The modified straw primary product is immersed in the mixed solution a, and ultrasonic treatment is performed at the same time, and the solution is removed and then dried to obtain the modified straw; In step A1, the straw is one of rice straw, corn straw, cotton straw and wheat straw, the solid-liquid ratio of the straw to the acetone solution is 1-3:20-25 g / mL, the mass concentration of the acetone solution is 20-30%, and the ultrasonic treatment time is 2-3 h.

2. A method for temporarily prolonging the setting time of a water-stable mixture according to claim 1, characterized in that: In the step A2, the solid-liquid ratio of dopamine to deionized water is 2-3:1 g / L, and the pH value is 8-9.

3. A method for temporarily prolonging the setting time of a water-stable mixture according to claim 1, characterized in that: In step A3, the solid-liquid ratio of the pretreated straw to the mixed liquid is 1-5:0.1 g / L, the time and temperature of the ultrasonic treatment are 20-24 h and 20-30° C., and the temperature and time of the drying are 40-55° C. and 10-16 h.

4. A method for temporarily prolonging the setting time of a water-stable mixture according to claim 1, characterized in that: In step A4, the solid-liquid ratio of the total volume of boron nitride to water, ethanol solution, polyethylene glycol, and ammonia water is 10-20:0.5 g / L, wherein the volume ratio of water, ethanol solution, polyethylene glycol, and ammonia water is 1:1:0.5:0.01, the mass concentration of the ethanol solution is 75%, and the mass concentration of the ammonia water is 26%.

5. A method for temporarily prolonging the setting time of a water-stable mixture according to claim 1, characterized in that: In the step A5, the solid-liquid ratio of the modified straw primary product to the mixed solution a is 1-3:0.5 g / L, the ultrasonic time is 5-6 hours, and the drying time and temperature are 30-40 minutes and 100-130° C. respectively.

Citation Information

Patent Citations

  • A concrete super retarder

    CN108046651B

  • Preparing technology of high-performance straw fiber plastic-wooden composite material

    CN102604403A

  • Anti-dry shrinkage cement stabilized macadam base material for roads

    CN114409338A