Preparation process of cellulose toughened modified polylactic acid composite material
By pre-treating and graft-modifying cotton fibers, blending them with polylactic acid and polycaprolactone, and adding plasticizers and nucleating agents, the problems of brittleness and insufficient heat resistance of polylactic acid resin were solved. Preparation Develop cellulose-toughened modified polylactic acid composite materials with high toughness and high heat resistance, which are suitable for food packaging and degradable plastic straws.
Patent Information
- Application Number
- CN202410896097.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-05
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-07-05
AI Technical Summary
Existing polylactic acid resin products have problems such as brittleness, poor toughness, and insufficient heat resistance. Moreover, the diphenylmethane diisocyanate used in the existing cellulose modification method is toxic and is not suitable for food packaging and degradable plastic straws. application.
By pre-treating and grafting modification of cotton fiber, its compatibility with polylactic acid and polycaprolactone is increased, and the spray method is used to blend and add plasticizer and nucleating agent to improve the toughening and modification of cellulose. Mechanical properties and heat resistance of polylactic acid composites.
Polylactic acid composite materials with high toughness and high heat resistance are prepared, which are suitable for use in fields such as food packaging and degradable plastic straws, avoiding the use of toxic chemicals.
Smart Images

Figure CN118440481B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polymer materials, in particular to a preparation process of a cellulose toughened and modified polylactic acid composite material. Background Art
[0002] Polylactic acid is derived from renewable non-grain crops (such as cassava, sweet sorghum, plant cellulose, etc.). It comes from nature and can be completely degraded by microorganisms in nature after use, eventually generating carbon dioxide and water, which does not pollute the environment and is very beneficial to protecting the natural environment. Polylactic acid has good solvent resistance, is non-toxic and non-irritating, has good biocompatibility, is biodegradable and absorbable, has high strength, is moisture-proof, resistant to oil and fat, has good air permeability, and also has certain bacteria resistance, flame retardancy and UV resistance. It has good plasticity and is easy to process and is suitable for extrusion, molding, casting, melt spinning, solution spinning, blow molding and other processing methods. With the increasing demand for plastics, the use of polylactic acid to replace existing petroleum-based polymer materials is a perfect choice that can solve resource and environmental problems at the same time. Although polylactic acid has many advantages, the current polylactic acid resin products still have the disadvantages of being brittle, poor toughness, and insufficient heat resistance.
[0003] Cellulose is a polysaccharide polymer compound widely found in nature. It has the advantages of being renewable, degradable, non-toxic, environmentally friendly, easy to modify, and low-cost. These characteristics make it have great potential application value. In theory, cellulose, as a natural long fiber, can be dispersed in a polymer matrix by doping to increase the internal friction of the matrix, thereby improving the mechanical properties of the material, especially the tensile properties, and enhancing the application value of the material. However, untreated cellulose not only has a very large molecular weight, but also has many surface hydroxyl groups and an extremely stable structure. It is often incompatible with the polymer matrix and instead causes it to destroy the regular internal structure of the polymer, and the overall mechanical properties are reduced. Therefore, in order to make cellulose disperse well in the matrix, it is necessary to modify its surface. For example, CN107011640B discloses a cellulose-reinforced modified polylactic acid composite material and a preparation method thereof, which is prepared from polylactic acid and modified cellulose. The modified cellulose is at least one of methyl cellulose, ethyl cellulose, hydroxypropyl methyl cellulose, hydroxyethyl cellulose, carboxyethyl cellulose or carboxymethyl cellulose modified with diphenylmethane diisocyanate. However, MDI has certain toxicity. Long-term or high-concentration exposure may cause respiratory irritation, skin allergies and other problems. It is not suitable for use in food packaging and degradable plastic straws. In addition, the heat resistance problem of polylactic acid has not been solved. Summary of the invention
[0004] In order to overcome the shortcomings of the above-mentioned prior art, the purpose of the present invention is to provide a preparation process of cellulose toughened modified polylactic acid composite materials, by modifying cotton fibers and then blending and modifying them with polylactic acid and polycaprolactone respectively, the compatibility of cellulose and polymers is greatly improved, and the probability of cellulose agglomeration is reduced, thereby obtaining a polylactic acid composite material with high toughness and high heat resistance.
[0005] The present invention is achieved through the following technical scheme: a preparation process of a cellulose toughened and modified polylactic acid composite material, comprising the following steps:
[0006] S1. Take 10-20 parts by weight of cotton fiber and dry them in an oven at 100-120°C for 6-12 hours to remove free water, then soak them in a 10%-25% by weight NaOH aqueous solution, ultrasonically treat them for 30-60 minutes, continue soaking for 6-12 hours, filter them, add a 50%-60% by weight NaOH aqueous solution, heat it to 150-160°C, and stir it continuously until the dissolution rate of the cotton fiber is ≥80%, filter the undissolved part, and obtain a cellulose anion intermediate;
[0007] S2. slowly add the acetone solution of triallyl isocyanurate to the cellulose anion intermediate filtrate, stir for a long time at 50-60°C, react for 5-10 hours, add 1 mol / L acetic acid dropwise to the system, maintain the pH value at 9-10, continue to react for 5-10 hours to obtain a modified cellulose precipitate, wash by centrifugation, and redisperse the modified cellulose precipitate in 10-20 parts of water to obtain a modified cellulose dispersion;
[0008] S3. Take 60-70% of the obtained modified cellulose dispersion and spray it on the surface of 80-100 parts of polylactic acid in the form of a spray method, and then cure it at 110-120°C for 20-30 minutes. Then, in the same way, spray the remaining part of the modified cellulose on the surface of 20-50 parts by mass of polycaprolactone in the form of a spray method, and then cure it at 110-120°C for 20-30 minutes. Finally, mix the polylactic acid doped with modified cellulose, polycaprolactone and 5-10 parts by mass of plasticizer, 2-5 parts by mass of nucleating agent and 1-3 parts by mass of lubricant evenly, and then put it into an internal mixer and blend it at 155-170°C and a rotation speed of 60-90r / min for 2-10 minutes. The obtained blend is dried in a vacuum oven at room temperature.
[0009] The blend can be pulverized by a pulverizer and then formed by injection molding, blow molding, extrusion and other processing techniques.
[0010] The present invention pre-treats the cotton fiber by drying it first, then soaks it with an alkali solution with a low mass concentration and performs ultrasonic treatment for the first time, so as to remove colloid and impurities on the surface of the cotton fiber, swell the cotton fiber, improve the wettability of the cotton fiber, and help the subsequent reaction of the cotton fiber. The alkali solution with a high mass concentration is used for high temperature treatment for the second time, so that the cellulose of the cotton fiber is hydrolyzed and a cellulose anion intermediate is generated and dissolved in a solvent, and then the cellulose anion intermediate and triallyl isocyanurate undergo a reversible addition reaction, also known as a Michael reaction, and the generated hydroxide ions are consumed by continuously adding a small amount of acetic acid, so as to improve the grafting rate of triallyl isocyanurate.
[0011] Preferably, the polylactic acid is L-polylactic acid, and the intrinsic viscosity of the L-polylactic acid is in the range of 2 to 4 dL / g.
[0012] Preferably, the intrinsic viscosity of the polycaprolactone is in the range of 0.75 to 2.25 dL / g.
[0013] The intrinsic viscosity can be obtained by testing according to standard GB / T 10247-2008.
[0014] Preferably, the cotton fiber is natural cotton or absorbent cotton.
[0015] Preferably, in step S3, the polylactic acid and polycaprolactone are dried at 100-120° C. for 2-5 hours before the spray treatment.
[0016] Preferably, in step S1, the amount of 10% to 25% NaOH aqueous solution added is enough to completely submerge the cotton fibers, and the amount of 50% to 60% NaOH aqueous solution added is 1.5 to 2 times the volume of the cotton fibers.
[0017] Preferably, the acetone solution of triallyl isocyanurate in step S2 is prepared by dissolving 3 to 5 parts by mass of triallyl isocyanurate in 10 to 20 parts by mass of acetone.
[0018] Preferably, the plasticizer is selected from one or more of tributyrin, tricaprylin, and tricaproin.
[0019] Preferably, the lubricant is selected from one or more of calcium stearate and magnesium stearate.
[0020] Preferably, the nucleating agent is selected from at least one of a hydrazide nucleating agent and a tetrapod-shaped zinc oxide whisker; the hydrazide nucleating agent is selected from TMC-306 and TMC-300.
[0021] More preferably, the nucleating agent is selected from two types of hydrazide nucleating agents and tetrapod-shaped zinc oxide whiskers, and the mass ratio of the hydrazide nucleating agent to the tetrapod-shaped zinc oxide whiskers is 1:(1-3).
[0022] Compared with the prior art, the present invention has the following beneficial effects:
[0023] The present invention provides a preparation process of a cellulose toughened and modified polylactic acid composite material, by pre-treating and grafting cotton fibers, and then blending with polylactic acid and polycaprolactone by spraying, the compatibility of cellulose with polylactic acid and polycaprolactone is greatly improved, and the probability of cellulose agglomeration is reduced. In addition, polycaprolactone, a nucleating agent, a plasticizer and other components and additives that are also doped with modified cellulose are added to the polylactic acid composite material, which can effectively improve the elongation at break and the heat deformation temperature of the polylactic acid composite material, and obtain a polylactic acid composite material with high toughness and high heat resistance, which is particularly suitable for use in the fields of food packaging and degradable plastic straws. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 This is the mechanism diagram of cellulose hydrolysis grafting;
[0025] Figure 2 This is the infrared spectrum of cellulose, triallyl isocyanurate, and modified cellulose. DETAILED DESCRIPTION
[0026] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0027] In the examples, the experimental methods used are conventional methods unless otherwise specified, and the materials, reagents, etc. used are all commercially available unless otherwise specified.
[0028] The raw materials used in the embodiments and comparative examples are described as follows:
[0029] Polylactic acid 1: L-polylactic acid, intrinsic viscosity 2.5 dL / g, model PLLA-25, purchased from Shenzhen Boli Biomaterials;
[0030] Polylactic acid 2: L-polylactic acid, intrinsic viscosity 4 dL / g, model PLLA-40, purchased from Shenzhen Boli Biomaterials;
[0031] Polylactic acid 3: L-polylactic acid, intrinsic viscosity 1.5 dL / g, model PLLA-15, purchased from Shenzhen Boli Biomaterials;
[0032] Polylactic acid 4: L-polylactic acid, intrinsic viscosity 5 dL / g, model PLLA-50, purchased from Shenzhen Boli Biomaterials;
[0033] Polylactic acid 5: racemic polylactic acid, intrinsic viscosity 2.5 dL / g, model PDLLA-25, purchased from Shenzhen Boli Biomaterials;
[0034] Polycaprolactone 1: intrinsic viscosity 1 dL / g, model PCL-10, purchased from Shenzhen Boli Biomaterials;
[0035] Polycaprolactone 2: intrinsic viscosity 2 dL / g, model PCL-20, purchased from Shenzhen Boli Biomaterials;
[0036] Polycaprolactone 3: intrinsic viscosity 0.5 dL / g, model PCL-05, purchased from Shenzhen Boli Biomaterials;
[0037] Polycaprolactone 4: intrinsic viscosity 3.5 dL / g, model PCL-35, purchased from Shenzhen Boli Biomaterials;
[0038] Cotton fiber: fine-staple cotton, produced in Hunan;
[0039] Triallyl isocyanurate (TAIC): 99%, Senfida;
[0040] Diphenylmethane diisocyanate: 98%, Sigma-Aldrich;
[0041] Plasticizer 1: tributyrin, 99%, Sigma-Aldrich;
[0042] Plasticizer 2: tricaprylin, 99%, Sigma-Aldrich;
[0043] Plasticizer 3: dioctyl phthalate, Shandong Jianye Xinfa;
[0044] Nucleating agent 1: tetrapod-shaped zinc oxide whisker, 98%, Wuhan Kemik;
[0045] Nucleating agent 2: hydrazide nucleating agent, TMC-306, Shanxi Chemical Research Institute;
[0046] Lubricant: magnesium stearate, commercially available;
[0047] Unless otherwise specified, the components and raw materials used in the embodiments and comparative examples of the present invention are all commercially available raw materials, and the components and raw materials used in each parallel experiment are all of the same kind.
[0048] Example 1
[0049] A preparation process of a cellulose toughened and modified polylactic acid composite material comprises the following steps, measured by weight:
[0050] S1. Take 10 parts by mass of cotton fiber and dry them in an oven at 120°C for 8 hours to remove free water, then soak them in a 10% by mass NaOH aqueous solution until the cotton fiber is completely submerged, ultrasonically treat for 60 minutes, continue soaking for 6 hours, and then filter, re-add twice the volume of a 10% by mass NaOH aqueous solution and a 55% by mass NaOH aqueous solution, heat to 155°C and stir continuously until the dissolution rate of the cotton fiber is ≥80%, filter the undissolved part, and obtain a cellulose anion intermediate;
[0051] S2. Slowly add the acetone solution of triallyl isocyanurate to the filtrate of the cellulose anion intermediate, and stir for a long time at 55°C. After reacting for 10 hours, add 1 mol / L acetic acid dropwise to the system, maintain the pH value at 9-10, and continue to react for 5 hours to obtain a modified cellulose precipitate, centrifuge and wash, and redisperse the modified cellulose precipitate in 10-20 parts of water to obtain a modified cellulose dispersion; in order to increase the grafting rate, the addition of triallyl isocyanurate should be excessive, and the acetone solution of triallyl isocyanurate is prepared by dissolving 5 parts by mass of triallyl isocyanurate in 20 parts by mass of acetone, wherein, Figure 1 The mechanism diagram of the hydrolysis of cellulose by NaOH to produce cellulose anion intermediates, which then react with triallyl isocyanurate to undergo nucleophilic addition reaction, is given. Figure 2 The infrared spectra of cellulose, triallyl isocyanurate and modified cellulose are given. After the cotton fiber is hydrolyzed with NaOH and grafted with triallyl isocyanurate, a characteristic peak of carbonyl appears at 1732cm-1, which proves the successful grafting modification.
[0052] S3. Take 70% of the obtained modified cellulose dispersion and spray it on the surface of 80 parts by mass of polylactic acid 1 by spray method and then cure it at 120°C for 30 minutes. Then, in the same way, spray the remaining part of the modified cellulose on the surface of 50 parts by mass of polycaprolactone 1 by spray method and then cure it at 120°C for 30 minutes. Finally, mix the polylactic acid 1, polycaprolactone 1 doped with modified cellulose, 10 parts of plasticizer 1, 2.5 parts by mass of nucleating agent 1, 2.5 parts by mass of nucleating agent 2 and 3 parts by mass of lubricant evenly, then put them into a Haake internal mixer and blend them at 166°C and a speed of 80r / min for 10 minutes. The obtained blend is dried in a vacuum oven at room temperature. The blend is crushed by a pulverizer and then formed by injection molding to obtain a cellulose-reinforced modified polylactic acid composite material.
[0053] Example 2
[0054] S1. Take 20 parts by weight of cotton fiber and dry them in an oven at 100°C for 8 hours to remove free water, then soak them in a 25% by weight NaOH aqueous solution, ultrasonically treat them for 30 minutes, continue soaking for 12 hours, filter them, add a 55% by weight NaOH aqueous solution, heat it to 155°C and stir it continuously until the dissolution rate of the cotton fiber is ≥80%, filter the undissolved part, and obtain a cellulose anion intermediate;
[0055] S2. Slowly add the acetone solution of triallyl isocyanurate to the filtrate of the cellulose anion intermediate, and stir for a long time at 55°C. After reacting for 5 hours, add 1 mol / L acetic acid dropwise to the system, maintain the pH value at 9-10, and continue to react for 8 hours to obtain a modified cellulose precipitate, centrifuge and wash, and redisperse the modified cellulose precipitate in 10-20 parts of water to obtain a modified cellulose dispersion; the acetone solution of triallyl isocyanurate is prepared by dissolving 3 parts by mass of triallyl isocyanurate in 10 parts by mass of acetone;
[0056] S3. Take 70% of the obtained modified cellulose dispersion and spray it on the surface of 100 parts by mass of polylactic acid 1 by spray method, and then cure it at 120°C for 30 minutes. Then, in the same way, spray the remaining part of the modified cellulose on the surface of 30 parts by mass of polycaprolactone 1 by spray method, and then cure it at 120°C for 30 minutes. The polylactic acid and polycaprolactone are dried at 100°C for 4 hours before spray treatment. Finally, the polylactic acid 1, polycaprolactone 1 doped with modified cellulose and 5 parts by mass of plasticizer 1, 1 part by mass of nucleating agent 1, 1 part by mass of nucleating agent 2, and 1 part by mass of lubricant are mixed evenly, and then put into a Haake internal mixer and blended for 10 minutes at 166°C and a rotation speed of 80r / min. The obtained blend is dried in a vacuum oven at room temperature. The blend is crushed by a pulverizer and then formed by injection molding to obtain a cellulose-reinforced modified polylactic acid composite material.
[0057] Embodiments 3 to 18
[0058] The preparation method is the same as that of Example 2, except that the components used or the mass fractions of the added components are different. The specific components and their mass fraction formulas are shown in Table 1.
[0059] Table 1 Components and weight parts of Examples 1 to 18
[0060]
[0061] Table 1
[0062]
[0063] Comparative Example 1
[0064] Compared with Example 2, the difference is that in step S1, 20 parts of cotton fibers are taken, without pretreatment, directly added with a 55% by mass NaOH aqueous solution, heated to 155° C. and continuously stirred until the dissolution rate of the cotton fibers is ≥80%, and the undissolved part is filtered to obtain a cellulose anion intermediate; the remaining steps are the same.
[0065] Comparative Example 2
[0066] S1. Take 20 parts of cotton fiber and dry them in an oven at 100℃ for 8 hours to remove free water, then soak them in a 25% by mass NaOH aqueous solution, ultrasonically treat them for 30 minutes, continue soaking for 12 hours, filter them, add a 55% by mass NaOH aqueous solution, heat it to 155℃ and stir it continuously until the dissolution rate of the cotton fiber is ≥80%, filter the undissolved part, and obtain cellulose anions;
[0067] S2. Take 70% of the obtained cellulose anions and spray them on the surface of 100 parts of polylactic acid 1 in the form of a spray method, and then cure them at 120°C for 30 minutes. Then, in the same way, spray the remaining part of the cellulose anions on the surface of 30 parts of polycaprolactone 1 in the form of a spray method and then cure them at 120°C for 30 minutes. Finally, mix the polylactic acid 1 doped with modified cellulose, polycaprolactone 1, 5 parts of plasticizer 1, 1 part of nucleating agent 1, 1 part of nucleating agent 2, and 1 part of lubricant evenly, and then put them into a Haake internal mixer and blend them at 166°C and a speed of 80r / min for 5 minutes. The obtained blend is dried in a vacuum oven at room temperature to obtain a cellulose toughened modified polylactic acid composite material.
[0068] Comparative Example 3
[0069] Compared with Example 2, the difference is that the triallyl isocyanurate in step S2 is replaced by diphenylmethane diisocyanate.
[0070] Comparative Example 4
[0071] Compared with Example 2, the difference is that in step S3, the modified cellulose obtained is sprayed on the surface of 100 parts of polylactic acid 1 in the form of a spray method and then cured at 120° C. for 30 minutes.
[0072] Comparative Example 5
[0073] Compared with Example 2, the difference is that in step S3, the modified cellulose obtained is sprayed on the surface of 100 parts of polylactic acid 1 in the form of a spray method and then cured at 120° C. for 30 minutes without adding polycaprolactone.
[0074] Comparative Example 6
[0075] Compared with Example 2, the difference is that no plasticizer is added.
[0076] Comparative Example 7
[0077] Compared with Example 2, the difference is that no nucleating agent is added.
[0078] Comparative Example 8
[0079] Compared with Example 2, the difference is that in step S3, the modified cellulose is directly mixed and uniformly blended with polylactic acid 1, polycaprolactone 1, plasticizer 1, nucleating agent and lubricant.
[0080] The polylactic acid composite materials prepared in Examples 1-18 and Comparative Examples 1-8 were subjected to the following performance tests, and the results are shown in Table 2, respectively.
[0081] 1. Tensile strength: The products of the embodiments and comparative examples were tested according to ISO 527-2 standard, with a tensile rate of 50 mm / min;
[0082] 2. Elongation at break: The products of the examples and comparative examples were tested according to ISO 527-2 standard, with a tensile rate of 50 mm / min;
[0083] 3. Heat deformation temperature: The products of the embodiment and the comparative example were tested based on the ASTM D648 standard, and the test conditions were 0.45 MPa and 6.4 mm when placed on the side;
[0084] Table 2 Performance tests of embodiments and comparative examples
[0085]
[0086] It can be seen from the embodiments and comparative examples that the cellulose toughened modified polylactic acid composite material obtained by the preparation process of the present invention has a tensile strength ≥100 MPa, an elongation at break ≥102%, and a heat deformation temperature greater than or equal to 85°C, which meets the requirements for food packaging and degradable plastic straws.
[0087] It can be seen from Examples 2 to 5 and 8 to 9 that when the intrinsic viscosity of polylactic acid and polycaprolactone is within a certain range, the mechanical properties and heat resistance of the obtained polylactic acid composite material are better. When the intrinsic viscosity range is too small, the mechanical strength of the composite material is insufficient. When the intrinsic viscosity range is too large, the modified cellulose and other additives are poorly dispersed and the overall performance of the material is poor.
[0088] It can be seen from Examples 2, 10 and 11 that when the plasticizer is selected from tributyrin and tricaprylin, the mechanical properties and heat resistance of the polylactic acid composite material are better. At the same time, tributyrin and tricaprylin are biomass materials, which are greener and safer than conventional plasticizers such as DOP, and meet the requirements for food packaging and degradable plastic straws.
[0089] It can be seen from Examples 12-16 that when the organic nucleating agent is a combination of hydrazides and tetrapod-shaped zinc oxide whiskers, it has a good effect on the mechanical properties and heat resistance of polylactic acid.
[0090] It can be seen from Examples 2, 17 and 18 that when the content of triallyl isocyanurate is low, increasing its content has a great improvement on the mechanical properties and heat resistance, but when the content of triallyl isocyanurate increases to a certain level, because the grafting rate of cellulose is difficult to be more significantly improved, the mechanical properties and heat resistance tend to be stable.
[0091] The preferred embodiments of the present invention disclosed above are only used to help illustrate the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to the specific implementation methods described. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.
Claims
1. A process for preparing a cellulose toughened and modified polylactic acid composite material, characterized in that: The following steps are involved: S1. Dry 10-20 parts by weight of cotton fiber in an oven at 100-120°C for 6-12 hours to remove free water. Then soak the fiber in a 10%-25% aqueous NaOH solution, ultrasonicate it for 30-60 minutes, soak it for another 6-12 hours, and filter it. Add a 50%-60% aqueous NaOH solution, heat it to 150-160°C, and stir it continuously until the cotton fiber dissolves 80% or more. Filter the undissolved portion to obtain a cellulose anion intermediate. The amount of 10%-25% aqueous NaOH solution added is sufficient to completely submerge the cotton fiber, and the amount of 50%-60% aqueous NaOH solution added is 1.5-2 times the volume of the cotton fiber. S2. Slowly add an acetone solution of triallyl isocyanurate to the filtrate of the cellulose anion intermediate under constant stirring at 50-60°C. After reacting for 5-10 hours, 1 mol / L acetic acid is added dropwise to the system while maintaining the pH at 9-10. Continue the reaction for 5-10 hours to obtain a modified cellulose precipitate. Wash the precipitate by centrifugation and redisperse it in 10-20 parts of water to obtain a modified cellulose dispersion. S3. Take 60-70% of the obtained modified cellulose dispersion and spray it on the surface of 80-100 parts of polylactic acid in the form of a spray method, and then cure it at 110-120°C for 20-30 minutes. Then, in the same way, spray the remaining part of the modified cellulose on the surface of 20-50 parts by mass of polycaprolactone in the form of a spray method and then cure it at 110-120°C for 20-30 minutes. Finally, the polylactic acid doped with modified cellulose, polycaprolactone and 5-10 parts by mass of plasticizer, 2-5 parts by mass of nucleating agent and 1-3 parts by mass of lubricant are mixed evenly, and then put into an internal mixer and blended at 155-170°C and a speed of 60-90r / min for 2-10 minutes to obtain a blend, which is dried in a vacuum oven at room temperature. The polylactic acid is L-polylactic acid, and the intrinsic viscosity of the L-polylactic acid is in the range of 2-4dL / g; the intrinsic viscosity of the polycaprolactone is in the range of 0.75-2.25 dL / g; the nucleating agent is selected from two types of hydrazide nucleating agents and tetrapod-shaped zinc oxide whiskers, and the mass ratio of the hydrazide nucleating agent to the tetrapod-shaped zinc oxide whiskers is 1: (1-3).
2. The process for preparing the composite material according to claim 1, wherein: The cotton fiber is natural cotton or absorbent cotton.
3. The process for preparing the composite material according to claim 1, wherein: In step S3, the polylactic acid and polycaprolactone are dried at 100-120° C. for 2-5 hours before being sprayed.
4. The process for preparing the composite material according to claim 1, wherein: The acetone solution of triallyl isocyanurate in step S2 is prepared by dissolving 3 to 5 parts by mass of triallyl isocyanurate in 10 to 20 parts by mass of acetone.
5. The process for preparing the composite material according to claim 1, wherein: The plasticizer is selected from one or more of tributyrin, tricaprylin, and tricaproin; and the lubricant is selected from one or more of calcium stearate and magnesium stearate.
6. The process for preparing the composite material according to claim 1, wherein: The hydrazide nucleating agent is selected from TMC-306 and TMC-300.
Citation Information
Patent Citations
A cellulose-toughened modified polylactic acid composite material and its preparation method
CN107011640B
Preparation process of chitosan oligosaccharide modifying cotton fiber
CN104532571A
Polylactic acid / nanocellulose halogen-free flame-retardant composite material
CN113321910A