A hypereutectic aluminum-silicon alloy with high wear resistance and its preparation method and application
By adjusting the composition of the aluminum-silicon alloy and adopting continuous casting, extrusion, solid solution and aging treatment methods, the problem of insufficient service capability of the traditional hypereutectic aluminum-silicon alloy in a high-speed environment has been solved, and its yield strength and resistance have been improved. Abrasive, suitable for high-speed components.
Patent Information
- Application Number
- CN202410903110.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-08
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-07-08
AI Technical Summary
Traditional hypereutectic aluminum-silicon alloys cannot serve in high-speed environments, and have insufficient tensile strength and wear resistance to be used in high-speed components.
By adjusting the composition of the aluminum-silicon alloy, including Si: 17-20%, Cu: 5-8%, Mg: 0.2-0.25%, Ti: 0.25-0.35%, V: 0.1-0.25%, Fe≤0.3%, using Continuous casting, extrusion, solid solution and aging treatment methods are used to prepare hypereutectic aluminum-silicon alloy with high wear resistance.
The yield strength, tensile strength and hardness of the hypereutectic aluminum-silicon alloy are improved, it can serve in high-speed environments above 12000r/min, and it shows good wear resistance and performance stability in automobile air-conditioning compressors.
Smart Images

Figure CN118441183B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of aluminum alloy continuous casting, and in particular to a hypereutectic aluminum-silicon alloy with high wear resistance, and a preparation method and application thereof. Background Art
[0002] Aluminum alloys are widely used in important parts such as automobiles and aircraft due to their high performance and light weight.
[0003] Hypereutectic aluminum alloy is a type of aluminum alloy, in which the silicon content is greater than 16%. Hypereutectic aluminum alloy has the advantages of small thermal expansion coefficient, high volume stability, high strength, high wear resistance and high corrosion resistance. It is mainly used in contact transmission parts in vehicles such as automobiles, such as air conditioning systems and brake systems. It is the preferred material for key parts with high efficiency, energy saving and light weight.
[0004] The tensile strength of traditional hypereutectic aluminum-silicon alloys is about 200MPa, and the wear test time is relatively short, so they are only used in wear-resistant components with relatively low rotation speeds. However, for components with rotation speeds exceeding 12,000 per minute, traditional hypereutectic aluminum-silicon alloys cannot be used. Summary of the invention
[0005] In view of the above analysis, the present invention aims to provide a hypereutectic aluminum-silicon alloy with high wear resistance and a preparation method and application thereof, so as to solve the problem that the existing hypereutectic aluminum-silicon alloy cannot be used in high-speed components.
[0006] On the one hand, the present invention provides a hypereutectic aluminum-silicon alloy with high wear resistance, which includes, by weight percentage, Si: 17-20%, Cu: 5-8%, Mg: 0.2-0.25%, Ti: 0.25-0.35%, V: 0.1-0.25%, Fe≤0.3%, and Al: balance.
[0007] Furthermore, in terms of weight percentage, it includes Si: 18.5-20%, Cu: 6.5-8%, Mg: 0.2-0.25%, Ti: 0.3-0.35%, V: 0.2-0.25%, Fe≤0.3%, and Al: balance.
[0008] On the other hand, the present invention provides a method for preparing a hypereutectic aluminum-silicon alloy with high wear resistance, comprising the following steps:
[0009] S1: Compounding raw materials according to corresponding proportions, and then smelting the raw materials into alloy liquid;
[0010] S2: A cast rod is prepared by a continuous casting method;
[0011] S3: Extruding the obtained cast rod to obtain an extruded billet;
[0012] S4: subjecting the obtained extruded billet to solution treatment and aging treatment to obtain a hypereutectic aluminum-silicon alloy.
[0013] Furthermore, in step S1, electromagnetic stirring is required during smelting, with a current of 80-100A and a frequency of 30-50Hz.
[0014] Furthermore, in step S2, the continuous casting method adopts horizontal continuous casting, the casting speed of the continuous casting equipment is set to 0.2m / min-0.5m / min, and the temperature is controlled at 710℃-725℃.
[0015] Furthermore, in step S3, the cast rod is heated to 420°C-470°C, the extrusion roller of the extruder is heated to 420°C-470°C, and the extrusion deformation amount is 20-50%.
[0016] Furthermore, in step S4, the heating temperature of the solution treatment is 490-530° C., and the holding time is 2-12 h.
[0017] Furthermore, in step S4, the heating temperature of the aging treatment is 145-185° C., and the holding time is 8-15 hours.
[0018] Furthermore, the yield strength of the hypereutectic aluminum-silicon alloy is above 300 MPa, the tensile strength is above 400 MPa, and the hardness is above 120 HB.
[0019] The hypereutectic aluminum-silicon alloy obtained by the present invention is used to manufacture high-speed wear-resistant components of automobiles, with a speed of more than 12000 r / min.
[0020] Compared with the prior art, the present invention can achieve at least one of the following beneficial effects:
[0021] 1. The hypereutectic aluminum-silicon alloy provided by the present invention is mainly composed of Al, Si and Cu, and is further supplemented with a small amount of Mg, Ti and V. The strength, wear resistance and hardness of the hypereutectic aluminum-silicon alloy can be improved. The hypereutectic aluminum-silicon alloy obtained by the present invention is manufactured into parts or components, which can serve in a high-speed environment.
[0022] 2. The present invention mixes alloy raw materials according to corresponding proportions, and then smelts them to prepare alloy liquid; the alloy liquid solidifies in a crystallizer of a continuous casting device to obtain a cast rod; the obtained cast rod is then extruded to refine the grains and improve the strength; finally, a solid solution and aging treatment is performed to change the internal structure of the extruded billet and refine the grains, so that the final hypereutectic aluminum-silicon alloy has higher strength, wear resistance and hardness.
[0023] 3. The present invention adopts the design of components, and then carries out smelting, horizontal continuous casting, extrusion, solid solution and aging treatment. The obtained hypereutectic aluminum silicon alloy has no defects such as cracks, slag inclusions and pores, and the average size of primary silicon is below 60 microns, and the average content of primary silicon + eutectic silicon is 15%-30%. According to performance tests, the yield strength of the hypereutectic aluminum silicon alloy is above 300MPa, the tensile strength is above 400MPa, and the hardness is above 120HB.
[0024] 4. The hypereutectic aluminum-silicon alloy of the present invention is prepared into a vehicle air-conditioning compressor, the speed is set to 12000r / min, the running time is 2h, and after the test, the cooling capacity of the compressor decreases by no more than 10%, the input power increases by no more than 10%, and the compressor noise increases by no more than 3 dB(A).
[0025] In the present invention, the above-mentioned technical solutions can also be combined with each other to achieve more preferred combination solutions. Other features and advantages of the present invention will be described in the subsequent description, and some advantages can become obvious from the description, or can be understood by practicing the present invention. The purpose and other advantages of the present invention can be realized and obtained through the contents particularly pointed out in the description and the drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] The accompanying drawings are only used for the purpose of illustrating specific embodiments and are not to be considered as limiting the present invention. In the entire drawings, the same reference symbols represent the same components;
[0027] Figure 1 This is a metallographic photograph of the hypereutectic aluminum alloy obtained in Example 1;
[0028] Figure 2 This is a metallographic photograph of the hypereutectic aluminum alloy obtained in Example 8;
[0029] Figure 3 This is a metallographic photograph of the hypereutectic aluminum alloy obtained in Example 9;
[0030] Figure 4 This is a metallographic photograph of the hypereutectic aluminum alloy obtained in Comparative Example 3. DETAILED DESCRIPTION
[0031] The preferred embodiments of the present invention will be described in detail below in conjunction with the accompanying drawings, wherein the accompanying drawings constitute a part of the present invention and are used together with the embodiments of the present invention to illustrate the principles of the present invention, but are not used to limit the scope of the present invention.
[0032] Aluminum alloy has good casting properties and plastic processing properties, good electrical and thermal conductivity, good corrosion resistance and weldability. It can be used as a structural material and is widely used in aerospace, aviation, transportation, construction, electromechanical, light chemical and daily necessities.
[0033] Hypereutectic aluminum alloy is one of the common types of aluminum alloys, and is mainly used in contact transmission parts in vehicles. However, due to its relatively low strength and wear resistance, the existing hypereutectic aluminum alloy can only be used in low-speed parts or components, and cannot be used in high-speed parts or components, such as those above 1200r / min.
[0034] Therefore, the present invention provides a hypereutectic aluminum-silicon alloy with high wear resistance, which includes, by weight percentage, Si: 17-20%, Cu: 5-8%, Mg: 0.2-0.25%, Ti: 0.25-0.35%, V: 0.1-0.25%, Fe≤0.3%, and Al: balance.
[0035] Compared with the prior art, the hypereutectic aluminum-silicon alloy provided by the present invention is mainly composed of Al, Si and Cu, and is further supplemented with a small amount of Mg, Ti and V. It can improve the strength, wear resistance and hardness of the hypereutectic aluminum-silicon alloy. The hypereutectic aluminum-silicon alloy obtained by the present invention is manufactured into parts or components, which can serve in a high-speed environment.
[0036] The elements in the present invention have the following functions:
[0037] Si: Silicon exists in the hypereutectic aluminum-silicon alloy mainly in the form of α+Si eutectic and β(Al3FeSi). The increase of silicon content can improve the fluidity of the alloy melt, and at the same time improve the strength and wear resistance of the hypereutectic aluminum-silicon alloy. However, as the silicon content increases, the plasticity of the hypereutectic aluminum-silicon alloy decreases, so Si in the present invention is 17-20%.
[0038] Cu: Copper is an important alloying element in hypereutectic aluminum-silicon alloys. It can improve the strengthening effect of solution treatment and aging treatment, and the CuAl2 phase precipitated by aging has a significant aging strengthening effect. After cooperating with solution treatment and aging treatment, it can improve the strength and wear resistance of hypereutectic aluminum-silicon alloys. However, when the copper content is too high, the aging strengthening effect will gradually decrease, so the Cu content in the present invention is 5-8%.
[0039] Mg: Magnesium is an important strengthening element in hypereutectic aluminum silicon alloy, which greatly improves the tensile strength of hypereutectic aluminum silicon alloy. In addition, under the condition of containing a certain amount of Si, a long strip of Mg2Si precipitation phase can be generated in the α-Al matrix, which improves the strength and hardness of the hypereutectic aluminum silicon alloy. However, when the magnesium content is too high, it not only leads to an increase in cost, but also gradually reduces the mechanical properties of the hypereutectic aluminum silicon alloy, so Mg in the present invention is 0.2-0.25%.
[0040] Ti: Titanium and aluminum form TiAl2 phase, which becomes the non-spontaneous core during crystallization and plays a role in refining the structure.
[0041] V: Vanadium plays a role in refining the grains in the hypereutectic aluminum-silicon alloy, thereby improving the mechanical properties of the hypereutectic aluminum-silicon alloy, such as plasticity, hardness and strength. However, when the vanadium content is too high, the production cost increases, so in the present invention, V is 0.1-0.25%.
[0042] Specifically, by weight percentage, it includes Si: 18.5-20%, Cu: 6.5-8%, Mg: 0.2-0.25%, Ti: 0.3-0.35%, V: 0.2-0.25%, Fe≤0.3%, and Al: balance.
[0043] The present invention provides a method for preparing a hypereutectic aluminum-silicon alloy with high wear resistance, comprising the following steps:
[0044] S1: Compounding raw materials according to corresponding proportions, and then smelting the raw materials into alloy liquid;
[0045] S2: A cast rod is prepared by a continuous casting method;
[0046] S3: Extruding the obtained cast rod to obtain an extruded billet;
[0047] S4: subjecting the obtained extruded billet to solution treatment and aging treatment to obtain a hypereutectic aluminum-silicon alloy.
[0048] Compared with the prior art, the present invention mixes alloy raw materials according to corresponding proportions, and then smelts them to prepare alloy liquid; the alloy liquid is solidified in a crystallizer of a continuous casting device to obtain a cast rod; the obtained cast rod is then extruded to refine the grains and improve the strength; finally, a solid solution and aging treatment is performed to change the internal structure of the extruded billet and refine the grains, so that the final hypereutectic aluminum-silicon alloy has higher strength, wear resistance and hardness.
[0049] Specifically, in step S1, electromagnetic stirring is required during smelting, with a current of 80-100A and a frequency of 30-50Hz.
[0050] It should be noted that the prepared alloy raw materials are placed in a smelting furnace for smelting, and the smelting temperature is controlled at 800-850°C. When the temperature of the alloy liquid reaches 750-770°C, electromagnetic stirring is applied in the smelting furnace, in which the current needs to be strictly controlled to be 80-100A and the frequency to be 30-50Hz.
[0051] When the parameters are within the above range, the gas in the alloy liquid can be removed and the inclusions can be reduced, the occurrence rate of defects such as pores during solidification can be reduced, and the quality of the alloy liquid can be improved. In addition, electromagnetic stirring using the above parameter range, under the mutual cooperation of current and frequency, can effectively refine the grain size of the hypereutectic aluminum-silicon alloy, improve the mechanical properties of the hypereutectic aluminum-silicon alloy, and reduce the macro-segregation in the hypereutectic aluminum-silicon alloy, and improve the uniformity of the composition.
[0052] Preferably, the current in the present invention may be 80A, 85A, 90A, 95A or 100A.
[0053] Preferably, the frequency in the present invention may be 30 Hz, 40 Hz or 50 Hz.
[0054] Specifically, in step S2, the continuous casting method adopts horizontal continuous casting, the casting speed of the continuous casting equipment is set to 0.2m / min-0.5m / min, and the temperature is controlled at 710℃-725℃.
[0055] It should be noted that the present invention transfers the alloy liquid from the smelting furnace to the intermediate tank of the continuous casting equipment. The intermediate tank is used to temporarily store the alloy liquid and is closely connected to the crystallizer. A gate is installed in the middle to control the flow of molten steel. The crystallizer is placed horizontally and usually consists of two sections. The first section is a beryllium bronze tube with cooling water outside, and the inner wall of the second section is a high-purity graphite material, and the outside is indirectly water-cooled.
[0056] The alloy liquid is cooled down through the crystallizer and gradually solidifies. After solidification, it moves in the horizontal direction. The temperature and pulling speed (i.e., horizontal moving speed) need to be strictly controlled. The temperature is 710℃-725℃ and the pulling speed is 0.2m / min-0.5m / min. When the pulling speed is lower than 0.2m / min, the production efficiency is low; when the pulling speed is higher than 0.5m / min, the surface quality and density of the resulting cast rod are poor, resulting in poor mechanical properties of the cast rod, which affects the microstructure and mechanical properties of the final hypereutectic aluminum-silicon alloy.
[0057] Preferably, the pulling speed may be 0.2 m / min, 0.25 m / min, 0.3 m / min, 0.35 m / min, 0.4 m / min, 0.45 m / min or 0.5 m / min.
[0058] Specifically, in step S3, the cast rod is heated to 420°C-470°C, the extrusion roller of the extruder is heated to 420°C-470°C, the extrusion deformation amount is 20-50%, and then the extruded billet is sent to a cooling water tank for cooling.
[0059] It should be noted that the present invention performs an extrusion operation on the obtained cast rod, and first heats the cast rod and the extrusion roller of the extruder to 420℃-470℃ to prevent microcracks from being generated in the cast rod during the extrusion process, which affects the performance of the final hypereutectic aluminum-silicon alloy. The present invention controls the deformation of the cast rod during the extrusion process to 20-50%, and the hypereutectic aluminum-silicon alloy obtains significant changes in the organizational composition and performance, further refines the grains and improves its wear resistance. When the deformation is less than 20%, the performance improvement is limited; when the deformation is higher than 50%, the microcracks in the extruded billet obtained after extrusion are significantly improved. When there are too many microcracks, the strength of the hypereutectic aluminum-silicon alloy is reduced.
[0060] Preferably, the extrusion deformation amount may be 20%, 25%, 30%, 35%, 40%, 45% or 50%.
[0061] More preferably, the extrusion deformation amount may be 30-40%.
[0062] Specifically, in step S3, the extruded billet is subjected to an annealing process after extrusion, including placing the extruded billet at 250° C.-260° C. for annealing for 10 hours, and then naturally air-cooling it to room temperature again.
[0063] Specifically, in step S4, the heating temperature of the solution treatment is 490-530° C., and the holding time is 2-12 hours.
[0064] Specifically, in step S4, the heating temperature of the aging treatment is 145-185° C., and the insulation time is 8-15 hours.
[0065] It should be noted that the extruded billet is subjected to solution and aging treatment. The purpose of solution treatment is to dissolve Al and Si elements into the Si-rich primary solidification phase, improve the strength of the hypereutectic aluminum-silicon alloy, completely cleave the hypereutectic phase structure in the alloy, enhance the bonding force between grains, and improve the density of the alloy. Aging treatment mainly produces precipitation strengthening effect and strengthens the hardness of the alloy.
[0066] The heating temperature and holding time need to be strictly controlled during the solution treatment process. Only reasonable heating temperature and holding time can effectively change the structure and properties of the extruded billet. When the heating temperature is lower than 490℃, the average grain size of the eutectic silicon particles in the extruded billet cannot be refined; when the heating temperature is higher than 530℃, obvious overburning occurs, resulting in the hardness of the extruded billet or hypereutectic aluminum-silicon alloy.
[0067] When the heating temperature is fixed, as the solution time increases, the hardness of the extruded billet or hypereutectic aluminum-silicon alloy remains basically stable, maintained at 140-150HV; however, as the solution time increases, the size of the eutectic silicon particles in the extruded billet increases and the number decreases, affecting the strength of the extruded billet or hypereutectic aluminum-silicon alloy.
[0068] Preferably, the heating temperature of the solution treatment may be 490°C, 500°C, 510°C, 520°C or 530°C.
[0069] More preferably, the heating temperature of the solution treatment may be 500-520°C.
[0070] Preferably, the holding time of the solution treatment can be 2h, 4h, 6h, 8h, 10h or 12h.
[0071] More preferably, the holding time of the solution treatment can be 2-10 hours.
[0072] More preferably, the holding time of the solution treatment can be 2-6 hours.
[0073] Further preferably, the heating temperature of the solution treatment is 510° C., and the holding time of the solution treatment can be 4 hours.
[0074] Preferably, the heating temperature of the aging treatment may be 145°C, 155°C, 165°C, 175°C or 185°C.
[0075] More preferably, the heating temperature of the aging treatment may be 155-175°C.
[0076] Preferably, the holding time of the aging treatment can be 8h, 9h, 10h, 11h, 12h, 13h, 14h or 15h.
[0077] More preferably, the holding time of the aging treatment can be 10-15h.
[0078] Further preferably, the heating temperature of the aging treatment is 165° C., and the holding time of the aging treatment can be 12 h.
[0079] Specifically, the yield strength of the hypereutectic aluminum-silicon alloy is above 300 MPa, the tensile strength is above 400 MPa, and the hardness is above 120 HB.
[0080] It should be noted that, through the design of the composition, combined with smelting, horizontal continuous casting, extrusion, solid solution and aging treatment, the obtained hypereutectic aluminum-silicon alloy has no defects such as cracks, slag inclusions and pores, and the average size of the primary silicon is below 60 microns, and the average content of primary silicon + eutectic silicon is 15%-30%. According to performance tests, the yield strength of the hypereutectic aluminum-silicon alloy is above 300MPa, the tensile strength is above 400MPa, and the hardness is above 120HB.
[0081] The hypereutectic aluminum-silicon alloy of the present invention is used to manufacture high-speed wear-resistant components of automobiles, such as a speed of more than 12000 r / min.
[0082] In order to more clearly describe the present invention, it is further illustrated by the following examples and comparative examples.
[0083] Example 1
[0084] A preparation method of a hypereutectic aluminum-silicon alloy comprises the following steps:
[0085] S1: Compounding raw materials according to corresponding proportions, and then smelting the raw materials into alloy liquid;
[0086] The chemical composition of the alloy liquid includes Si: 18.5%, Cu: 6.5%, Mg: 0.2%, Ti: 0.3%, V: 0.2%, Fe: 0.22%, Al: balance;
[0087] The prepared alloy raw materials are placed in a smelting furnace for smelting. The smelting temperature is controlled at 820°C. When the temperature of the alloy liquid reaches 750°C, electromagnetic stirring is applied in the smelting furnace. The current needs to be strictly controlled to be 90A and the frequency to be 40Hz.
[0088] S2: A cast rod is prepared by a continuous casting method;
[0089] The continuous casting method adopts horizontal continuous casting, the casting speed of the continuous casting equipment is set to 0.35m / min, and the temperature is controlled at 710℃-725℃;
[0090] S3: Extruding the obtained cast rod to obtain an extruded billet;
[0091] The cast rod and the extrusion roller of the extruder are heated to 450° C., and the extrusion deformation is 35%, and then the extruded billet is sent to a cooling water tank for cooling; then the extruded billet is placed at 250° C. for annealing for 10 hours, and then naturally air-cooled to room temperature again;
[0092] S4: subjecting the obtained extruded billet to a solution treatment and an aging treatment to obtain a hypereutectic aluminum-silicon alloy;
[0093] The heating temperature of the solution treatment is 510°C and the holding time is 4h;
[0094] The heating temperature of the aging treatment is 165° C. and the holding time is 12 h.
[0095] Example 2-3, Comparative Example 1-2
[0096] The distinguishing parameters of Examples 1-3 and Comparative Examples 1-2 are shown in Table 1.
[0097] Table 1 Difference parameters between the examples and the comparative examples
[0098]
[0099] Examples 4-9, Comparative Examples 3-7
[0100] The different parameters of Examples 4-9, Comparative Examples 3-7 and Example 1 are shown in Table 2.
[0101]
[0102] Performance Testing
[0103] The hypereutectic aluminum-silicon alloys obtained in the above Examples 1-9 and Comparative Examples 1-7 were subjected to performance tests, mainly including tensile strength, yield strength, hardness and wear resistance. For the wear resistance test, the prepared sample was placed on a wear resistance tester, and the test parameters were set, including the load force (10N), rotation speed (300rpm) and test time (30 minutes). The weight before and after friction was recorded, and the loss amount and loss percentage were calculated. The greater the loss percentage, the worse the wear resistance. The specific test results are shown in Table 3.
[0104]
[0105] In combination with Examples 1-9 and Comparative Examples 1-7 and Table 3, it can be seen that by adopting the composition and preparation method of Examples 1-9 of the present invention, the obtained hypereutectic aluminum-silicon alloy has higher strength, hardness and wear resistance, with a tensile strength of more than 425 MPa, a yield strength of more than 305 MPa, a hardness of more than 124 HB, and a wear loss percentage of less than 10.4%.
[0106] Reference Figure 1-4 In the hypereutectic aluminum-silicon alloy obtained in Example 1 / 8 / 9, the average size of primary silicon is less than 60 microns, and the average content of primary silicon + eutectic silicon is 15%-30%.
[0107] Combining Examples 1-3 and Comparative Examples 1-2 and Table 3, it can be seen that the hypereutectic aluminum-silicon alloy is mainly composed of Al, Si and Cu, and is supplemented with a small amount of Mg, Ti and V, which can improve the strength, wear resistance and hardness of the hypereutectic aluminum-silicon alloy.
[0108] Application Examples
[0109] The hypereutectic aluminum-silicon alloy obtained in Example 1 is prepared into a vehicle air-conditioning compressor. In the preparation step, die forging is required according to the model of the air-conditioning compressor before solution treatment and aging treatment.
[0110] The prepared automotive air-conditioning compressor was subjected to a durability test, and the test was carried out with reference to GB / T 21360-2018 "Refrigerant Compressors for Automotive Air Conditioning". The speed was set to 12000r / min, and the test time was 2h. After 2h, the compressor cooling capacity, input power, noise and other performance were tested. The compressor cooling capacity decreased by no more than 10%, the input power increased by no more than 10%, and the compressor noise increased by no more than 3 dB(A).
[0111] The hypereutectic aluminum-silicon alloy obtained by the present invention can meet the use requirements of vehicle air-conditioning compressors, can serve in 12000r / min rotation speed parts, and can be used as a wear-resistant component in a high-speed environment.
[0112] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily conceived by any technician familiar with the technical field within the technical scope disclosed by the present invention should be covered within the protection scope of the present invention.
Claims
1. A hypereutectic aluminum-silicon alloy with high wear resistance for manufacturing high-speed wear-resistant components of automobiles, characterized in that: According to weight percentage, Si: 17-20%, Cu: 5-8%, Mg: 0.2-0.25%, Ti: 0.25-0.35%, V: 0.1-0.25%, Fe≤0.3%, Al: balance; The hypereutectic aluminum-silicon alloy is prepared by the following steps: S1: Compound the raw materials according to the corresponding proportions, and then melt the raw materials into alloy liquid; electromagnetic stirring is required during smelting, the current is 80-100A, and the frequency is 30-50Hz; S2: A cast rod is prepared by a continuous casting method; the continuous casting method adopts horizontal continuous casting, the casting speed of the continuous casting equipment is set to 0.2m / min-0.5m / min, and the temperature is controlled at 710℃-725℃; S3: Extruding the obtained cast rod to obtain an extruded billet, wherein the extrusion deformation amount is 20-50%; S4: subjecting the obtained extruded billet to a solution treatment and an aging treatment to obtain a hypereutectic aluminum-silicon alloy; The heating temperature of the solution treatment is 490-530°C, and the holding time is 2-12h; the heating temperature of the aging treatment is 145-185°C, and the holding time is 8-15h; The average size of primary silicon in the hypereutectic aluminum-silicon alloy is below 60 microns, and the average content of primary silicon + eutectic silicon is 15%-30%; the rotation speed is above 12000r / min.
2. The hypereutectic aluminum-silicon alloy with high wear resistance according to claim 1, characterized in that: Calculated by weight percentage, Si: 18.5-20%, Cu: 6.5-8%, Mg: 0.2-0.25%, Ti: 0.3-0.35%, V: 0.2-0.25%, Fe≤0.3%, Al: balance.
3. A method for preparing a hypereutectic aluminum-silicon alloy having high wear resistance as claimed in claim 1 or 2, characterized in that: The following steps are involved: S1: Compounding raw materials according to corresponding proportions, and then smelting the raw materials into alloy liquid; S2: A cast rod is prepared by a continuous casting method; S3: Extruding the obtained cast rod to obtain an extruded billet; S4: subjecting the obtained extruded billet to a solution treatment and an aging treatment to obtain a hypereutectic aluminum-silicon alloy.
4. The method for preparing a hypereutectic aluminum-silicon alloy with high wear resistance according to claim 3, characterized in that: In step S1, electromagnetic stirring is required during smelting, with a current of 80-100A and a frequency of 30-50Hz.
5. The method for preparing a hypereutectic aluminum-silicon alloy with high wear resistance according to claim 3, characterized in that: In step S2, the continuous casting method adopts horizontal continuous casting, the casting speed of the continuous casting equipment is set to 0.2m / min-0.5m / min, and the temperature is controlled at 710℃-725℃.
6. The method for preparing a hypereutectic aluminum-silicon alloy with high wear resistance according to claim 3, characterized in that: In step S3, the cast rod is heated to 420°C-470°C, the extrusion roller of the extruder is heated to 420°C-470°C, and the extrusion deformation amount is 20-50%.
7. The method for preparing a hypereutectic aluminum-silicon alloy with high wear resistance according to claim 3, characterized in that: The yield strength of the hypereutectic aluminum-silicon alloy is above 300 MPa, the tensile strength is above 400 MPa, and the hardness is above 120 HB.
8. A hypereutectic aluminum-silicon alloy as claimed in claim 1 or 2 or a hypereutectic aluminum-silicon alloy obtained according to any one of claims 3 to 7 is used to manufacture high-speed wear-resistant components of automobiles, with a rotation speed of more than 12,000 r / min.
Citation Information
Patent Citations
Al-Si-Cu-Mg wrought aluminum alloy and preparation method thereof
CN111893354A
Piston for internal combustion engine and method of manufacturing the same
CN1545597A