A medium pressure corrosion foil
By adding titanium elements to the surface of the aluminum foil and using mixed acid treatment in the multi-stage hole formation and hole expansion process, combined with heat treatment, the problems of uneven distribution of medium-pressure etched foil holes and low capacitance value were solved, and the electrostatic capacity and capacitance were significantly improved. Electrochemical properties improve production efficiency.
Patent Information
- Application Number
- CN202410452088.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-18
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-01-18
AI Technical Summary
When manufacturing medium-pressure etched foils in the existing technology, the hole distribution is uneven and the number of holes is small, resulting in too small capacitance value and low productivity. Moreover, pretreatment with sulfuric acid, hydrochloric acid and phosphoric acid will cause surface color difference and removal of trace elements.
Vacuum coating technology is used to add titanium element to the surface of the aluminum foil, and mixed acids and buffers are used in the multi-stage pore opening and expansion process to form an oxide film and undergo heat treatment to increase hole density and uniformity, and enhance electrostatic capacity and electrochemical characteristics. .
The electrostatic capacity and electrical properties of the medium-voltage etched foil are significantly improved, the uniformity of hole distribution and production efficiency are improved, and the specific capacity and number of holes are increased.
Smart Images

Figure CN118448167B_ABST
Abstract
Description
[0001] This application is a divisional application of application number 2024100722853, application date January 18, 2024, and invention name “A method for manufacturing medium-pressure corrosion foil”. Technical Field
[0002] The invention relates to the technical field of preparation of capacitor etching foil, in particular to a medium-voltage etching foil. Background Art
[0003] With the continuous development of the electronics industry, higher requirements are put forward for the electrostatic capacitance per unit surface area of electrolytic capacitors. Electrolytic capacitors are one of the indispensable components in electronic products. They have the characteristics of excellent performance, large capacity, low price, easy processing, and convenient use. Therefore, they are widely used in electronic equipment, instruments, electromechanical, home appliances and other electronic complete products. As the key material for the production of electrolytic capacitors, medium-voltage corrosion foil, its manufacturing process involves multiple disciplines such as electrochemistry, fluid mechanics, machinery, electronics, electrical, communication engineering, and medical treatment. It has the characteristics of high technical content and high product added value. Among them, the porous structure with high density, high density, and size (pore diameter and pore length) is the key to achieving high specific capacity. The main process of manufacturing medium-voltage corrosion film in the existing technology is to use pre-treatment, pore opening, pore expansion, chemical cleaning, pure water cleaning, drying and other steps for preparation.
[0004] However, the main disadvantages of the existing etching process for manufacturing medium-pressure etching foil are: 1. The medium-pressure etching film prepared by the single-stage pore-forming method has uneven pore distribution, a small number of pores, and a too small capacitance value; 2. The production line speed of the pore-forming etching method is not high, the output per hour is small, and the productivity is low. 3. The existing etching foil pretreatment mainly adopts methods such as sulfuric acid, phosphoric acid and sodium hydroxide. Among them, sulfuric acid and phosphoric acid pretreatment are basically carried out between 65°C and 75°C. Due to the uneven concentration of the solution in the tank, uneven pores are caused, and color difference occurs on the surface, while alkali treatment will remove trace elements that are beneficial to pore formation.
[0005] Therefore, the present invention provides a preparation process for medium-voltage etching foil that can achieve uniform hole size and average unit density of the etching foil, which is of great significance for improving the preparation level of capacitor etching foil. Summary of the invention
[0006] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a medium-voltage corrosion foil. The medium-voltage corrosion foil prepared by the method has higher capacitance and good electrochemical properties.
[0007] To achieve the above object, the present invention provides the following technical solutions:
[0008] A medium-pressure etched foil, the medium-pressure etched foil is based on a method for manufacturing the medium-pressure etched foil, the method for manufacturing the medium-pressure etched foil is characterized by comprising the following steps:
[0009] S1. Pretreatment: placing the aluminum foil in a pretreatment solution at a temperature of 40-55° C. and soaking it for 0.5-1 min to obtain an aluminum foil sheet soaked in the pretreatment solution; placing the aluminum foil sheet soaked in the pretreatment solution in a vacuum chamber of a coating machine for nano-titanium coating;
[0010] S2, primary pore forming: soak the pre-treated aluminum foil in a primary mixed treatment solution at a temperature of 45-60°C for 1-1.5 minutes, drain, and then continue to spray with the primary mixed treatment solution at a spray flow rate of 8-10L / h for 20-30 minutes to obtain an aluminum foil treated with the primary mixed treatment solution;
[0011] S3, secondary hole expansion: the aluminum foil sheet treated with the primary mixed treatment solution in S2 is washed with pure water, and after washing, is placed in a secondary mixed treatment solution at a temperature of 50-60° C. and immersed for 1-3 minutes to obtain an aluminum foil sheet treated with the secondary mixed treatment solution;
[0012] S4, heat treatment: the aluminum foil treated with the secondary mixed treatment solution in S3 is cleaned and then heat treated to form an aluminum oxide film with a thickness of ≤5 nm;
[0013] S5, three-stage pore forming: placing the heat-treated aluminum foil in a three-stage mixed treatment solution at a temperature of 60-75° C. and soaking for 2-5 minutes to obtain an aluminum foil treated with the three-stage mixed treatment solution;
[0014] S6. Post-treatment: The aluminum foil treated with the three-stage mixed treatment solution is placed in a nitric acid solution at a temperature of 40-50° C. and soaked for 2-3 minutes. After being taken out and washed with pure water, a medium-pressure corrosion foil is obtained.
[0015] Preferably, in step S1, the pretreatment solution is a phosphoric acid solution with a mass percentage of 5-10%.
[0016] Preferably, in step S1, the nano-titanium plating treatment is specifically as follows: adjusting the coating vacuum chamber to 5×10~3Pa, 200-250 degrees Celsius, and keeping warm for 20-30min; ventilating argon gas into the coating vacuum chamber to maintain the air pressure at 0-0.4 Pa; connecting the bias power supply, adjusting the bias voltage to 250-280V, and performing discharge cleaning for 20-30 minutes; setting the bias voltage between 120-170V, turning on the ion cleaning of the ion source for 20-30min, turning on the arc source titanium target, adjusting the bias voltage to 150-200V, the target current to 60-80A, and performing ion bombardment on the titanium target for 3-5min; adjusting the vacuum degree to 0.5-0.8Pa, adjusting the bias voltage to 50V-60V, and arc plating for 5-7 minutes.
[0017] Preferably, in step S2, the primary mixed treatment solution is composed of 1-5% sulfuric acid solution, 5-10% hydrochloric acid solution and 5-10% Al 3+ Solution.
[0018] Preferably, in step S4, the heat treatment step is specifically:
[0019] S401, subjecting the aluminum foil treated with the secondary mixed solution to a high-frequency alternating current treatment of 500-1000 Hz, with a current density of 0.05-0.1 A / cm 2 , the electrolyte is 0.5-1.5mol / L oxalic acid solution, and the solution temperature is 50-60℃;
[0020] S402, placing the aluminum foil sheet treated by high-frequency alternating current at a temperature of 100-120°C and baking it for 0.5-1min to obtain a heat-treated aluminum foil sheet.
[0021] Preferably, in step S3, the secondary mixed treatment solution is composed of 5-10% nitric acid solution, 0.5-1% graphene, 0.5-1% buffer and 5-10% Al 3+ Solution.
[0022] Preferably, in step S5, the tertiary mixed treatment solution is composed of 5-10% nitric acid solution, 3-5% sulfuric acid solution, 0.5-1% buffer and 5-10% Al 3+ Solution.
[0023] Preferably, the buffer is one of sodium polypropylene sulfonate, sodium glycolate or sodium polyacrylate.
[0024] Preferably, the Al 3+ The solution is one or more of aluminum nitrate, aluminum chloride, and aluminum sulfate.
[0025] Preferably, the primary pore needs to apply 10-20A / dm 2 The current density of the direct current is 6-8A / dm 2 The current density of direct current.
[0026] Compared with the prior art, the present invention has the following beneficial effects:
[0027] (1) The present invention uses vacuum coating technology during pretreatment to add a trace amount of titanium element on the surface of the aluminum foil, so that a certain amount of Al-Ti micro batteries are generated in the corrosion pores, thereby enhancing the corrosion resistance of the aluminum foil, increasing the pore density, and reducing the high dielectric constant composite oxide film generated after the hole corrosion, thereby increasing the specific capacity. At the same time, under the action of acid mixed acid, the pore generation efficiency is effectively improved and the specific capacity is increased;
[0028] (2) The present invention uses mixed acid solution for treatment during the pore making and hole expansion process. The functions of sulfuric acid and phosphoric acid are both to dissolve the oxide film. Phosphoric acid is less soluble in the oxide film than sulfuric acid. It can not only dissolve the oxide film formed on the surface of the primary pore, but also protect the hole structure from collapse. In addition, the present invention uses a buffer during the pore making and hole expansion process, which can not only protect the inside of the hole produced by the primary pore making, but also protect the surface of the hole at the same time, preventing the two adjacent holes from merging due to the dissolution of the hole wall. The uniformity of the hole can be improved, which can significantly enhance the electrostatic capacity and electrical characteristics of the medium-voltage corrosion foil.
[0029] (3) The present invention adopts a specific heat treatment, and the loose treatment of the oxide film formed by the heat treatment well protects the holes formed in the pores, and effectively activates the active sites in the pores that have not been successfully pore-formed, thereby realizing the controllable operation of the hole distribution and the number of holes in the corrosion foil. The holes in the prepared corrosion foil have good controllability, and the uniformity of the hole distribution is significantly improved, which can significantly improve the quality and production efficiency of the medium-pressure corrosion foil. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 The present invention is a flow chart of the method for manufacturing the medium-pressure corrosion foil;
[0031] Figure 2 This is a surface SEM image of the medium-pressure corrosion foil sample prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0032] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0033] Unless otherwise specified, the materials, reagents, etc. used in the embodiments of the present invention can be obtained from commercial sources.
[0034] Example 1
[0035] S101, pretreatment: placing the aluminum foil in a 5% by mass phosphoric acid solution at a temperature of 40° C. and soaking it for 0.5 min to obtain an aluminum foil sheet soaked in the pretreatment solution; placing the aluminum foil sheet soaked in the pretreatment solution in a vacuum chamber of a coating machine for nano-titanium coating;
[0036] S102, primary pore formation: the pre-treated aluminum foil is placed in a primary mixed treatment solution prepared by 1% sulfuric acid solution, 5% hydrochloric acid solution and 5% aluminum nitrate solution and immersed for 1 minute at a temperature of 45°C and a current density of 10A / dm is continuously applied. 2 The direct current is drained, and then the primary mixed treatment solution is continuously sprayed for 20 minutes at a spray flow rate of 8 L / h to obtain an aluminum foil sheet treated with the primary mixed treatment solution;
[0037] S103, secondary hole expansion: the aluminum foil treated with the primary mixed treatment solution is washed with pure water, and after washing, it is placed in a secondary mixed treatment solution prepared by mixing 5% by mass nitric acid solution, 0.5% by mass graphene, 0.5% by mass buffer and 5% by mass aluminum nitrate solution for 1 minute at a temperature of 50°C and a continuous current density of 6A / dm 2 A direct current is applied to obtain an aluminum foil sheet treated with a secondary mixed treatment solution;
[0038] S104, heat treatment: the aluminum foil that has been treated with the secondary mixed solution is subjected to a 500 Hz high frequency alternating current treatment with a current density of 0.05 A / cm 2 , the electrolyte is 0.5 mol / L oxalic acid solution, the solution temperature is 50°C; the aluminum foil treated by high-frequency alternating current is placed at a temperature of 100°C and baked for 0.5 min to obtain a heat-treated aluminum foil;
[0039] S105, three-stage pore forming: placing the heat-treated aluminum foil in a three-stage mixed treatment solution prepared by mixing 5% by mass nitric acid solution, 3% by mass sulfuric acid solution, 0.5% by mass buffer and 5% by mass aluminum nitrate solution for 2 minutes at a temperature of 60° C. to obtain an aluminum foil treated with the three-stage mixed treatment solution;
[0040] S106, post-treatment: the aluminum foil treated with the three-stage mixed treatment solution is placed in a nitric acid solution at a temperature of 40°C and soaked for 2 minutes, taken out and washed with pure water to obtain a medium-pressure corrosion foil.
[0041] Example 2
[0042] S201, pretreatment: placing the aluminum foil in a 10% by mass phosphoric acid solution at a temperature of 55° C. and soaking it for 1 minute to obtain an aluminum foil sheet soaked in the pretreatment solution; placing the aluminum foil sheet soaked in the pretreatment solution in a vacuum chamber of a coating machine for nano-titanium coating;
[0043] S202, primary pore formation: the pre-treated aluminum foil is placed in a primary mixed treatment solution prepared by 5% sulfuric acid solution, 10% hydrochloric acid solution and 10% aluminum sulfate solution and immersed for 1.5 minutes at a temperature of 60°C and a current density of 20A / dm is continuously applied. 2 The direct current is drained, and then the primary mixed treatment solution is continuously sprayed for 30 minutes at a spray flow rate of 10 L / h to obtain an aluminum foil sheet treated with the primary mixed treatment solution;
[0044] S203, secondary hole expansion: the aluminum foil treated with the primary mixed treatment solution is washed with pure water, and after washing, it is placed in a secondary mixed treatment solution prepared by mixing 10% by mass nitric acid solution, 1% by mass graphene, 1% by mass buffer and 10% by mass aluminum sulfate solution for 3 minutes at a temperature of 60°C and a continuous current density of 8A / dm 2 A direct current is applied to obtain an aluminum foil sheet treated with a secondary mixed treatment solution;
[0045] S204, heat treatment: the aluminum foil that has been treated with the secondary mixed solution is treated with a high-frequency alternating current of 1000 Hz, with a current density of 0.1 A / cm 2 , the electrolyte is 1.5 mol / L oxalic acid solution, the solution temperature is 60°C; the aluminum foil treated by high-frequency alternating current is placed at a temperature of 120°C and baked for 1 minute to obtain a heat-treated aluminum foil;
[0046] S205, three-stage pore forming: placing the heat-treated aluminum foil in a three-stage mixed treatment solution prepared by mixing 10% nitric acid solution, 5% sulfuric acid solution, 1% buffer and 10% aluminum sulfate solution by mass percentage, and soaking for 5 minutes at a temperature of 75° C. to obtain an aluminum foil treated with the three-stage mixed treatment solution;
[0047] S206, post-treatment: the aluminum foil treated with the three-stage mixed treatment solution is placed in a nitric acid solution at a temperature of 50°C and soaked for 3 minutes, taken out and washed with pure water to obtain a medium-pressure corrosion foil.
[0048] Example 3
[0049] S301, pretreatment: placing the aluminum foil in a phosphoric acid solution with a mass percentage of 8% at a temperature of 45° C. and soaking it for 0.7 min to obtain an aluminum foil sheet soaked in the pretreatment solution; placing the aluminum foil sheet soaked in the pretreatment solution in a vacuum chamber of a coating machine for nano-titanium coating;
[0050] S302, primary pore formation: the aluminum foil after pretreatment is placed in a primary mixed treatment solution prepared by 3% sulfuric acid solution, 7% hydrochloric acid solution and 8% aluminum nitrate solution by mass percentage and immersed for 1.2 minutes at a temperature of 50°C and a current density of 15A / dm 2 The direct current is drained, and then the primary mixed treatment solution is continuously sprayed for 25 minutes at a spray flow rate of 9 L / h to obtain an aluminum foil sheet treated with the primary mixed treatment solution;
[0051] S303, secondary hole expansion: the aluminum foil treated with the primary mixed treatment solution is washed with pure water, and after washing, it is placed in a solution containing 7% by mass of nitric acid solution, 0.8% by mass of graphene, 0.8% by mass of buffer and 7% by mass of Al 3+ The solution was mixed and immersed in the secondary mixed treatment solution prepared by solution mixing for 2 minutes at a temperature of 55°C and a current density of 7A / dm 2 A direct current is applied to obtain an aluminum foil sheet treated with a secondary mixed treatment solution;
[0052] S304, heat treatment: the aluminum foil that has been treated with the secondary mixed solution is treated with 800Hz high-frequency alternating current with a current density of 0.09A / cm 2 , the electrolyte is 0.8 mol / L oxalic acid solution, the solution temperature is 55°C; the aluminum foil treated by high-frequency alternating current is placed at a temperature of 110°C and baked for 0.7 minutes to obtain a heat-treated aluminum foil;
[0053] S305, third-level pore formation: place the heat-treated aluminum foil in a solution containing 7% nitric acid solution, 4% sulfuric acid solution, 0.8% buffer and 8% Al3+ The aluminum foil is immersed in a three-stage mixed treatment solution prepared by mixing the solutions for 3 minutes at a temperature of 70° C. to obtain an aluminum foil treated with the three-stage mixed treatment solution;
[0054] S306, post-treatment: the aluminum foil treated with the three-stage mixed treatment solution is placed in a nitric acid solution at a temperature of 45°C and soaked for 3 minutes, taken out and washed with pure water to obtain a medium-pressure corrosion foil.
[0055] Comparative Example 1
[0056] There are the following differences between Comparative Example 1 and Example 1. The only difference is that in Comparative Example 1, step S101 described in Example 1 is omitted, and the step of placing the aluminum foil in the vacuum chamber of the coating machine for nano-titanium coating is cancelled. Other components, materials and their preparation process are the same as those in Example 1.
[0057] Comparative Example 2
[0058] There are the following differences between Comparative Example 2 and Example 1, the only difference is: in Comparative Example 2, step S104 described in Example 1 is omitted, and the heat treatment of the aluminum foil that has completed the secondary mixed solution treatment is cancelled. Other components, materials and their preparation process are the same as those in Example 1.
[0059] Comparative Example 3
[0060] Comparative Example 3 is different from Example 1 in the following ways: In Comparative Example 3, step S102 in Example 1 is replaced, and the primary mixed treatment solution is replaced with a 5% hydrochloric acid solution, and other components, materials and preparation processes are the same as those in Example 1.
[0061] Comparative Example 4
[0062] Comparative Example 4 is different from Example 1 in the following ways: In Comparative Example 4, step S103 in Example 1 is omitted, and the addition of the buffer in the secondary mixed treatment solution is cancelled; the other components, materials and preparation processes are the same as those in Example 1.
[0063] The medium voltage corrosion foils prepared in Examples 1-3 and Comparative Examples 1-4 were subjected to scanning electron microscope analysis and electrostatic capacitance detection and analysis, and their electrochemical properties were evaluated by analyzing and comparing the detection results.
[0064] The test results are as follows:
[0065] The bending strength and 240V capacity of the anode foils prepared in the examples and comparative examples were tested according to the JCC testing standard; the number and diameter of holes in the corrosion foils were obtained by counting 1000 times SEM images of the corrosion foil surface after polishing by 10 μm.
[0066] The test data is shown in Table 1:
[0067]
[0068] From the data in the above table, it can be seen that the electrostatic capacitance, bending strength and hole uniformity of Examples 1-3 are significantly better than those of Comparative Examples 1-4. In terms of the bending strength and electrostatic capacitance of the medium-pressure corrosion film, the main focus is on the improvement of the electrostatic capacitance (unit capacitance) of the pressure-resistant corrosion film. The bending strength of the product can reach more than 65, which can meet the needs of related products. The thickness of the medium-pressure corrosion-resistant film will cause the volume of the medium-pressure corrosion film to become larger, but when the thickness becomes thinner, it will also affect the improvement of the specific capacitance. For example, in Comparative Example 4, the number and uniformity of the holes decrease, and the electrostatic capacitance of the corresponding intermediate pressure-etching film also decreases significantly. Obviously, the manufacturing method of the medium-pressure corrosion foil disclosed in the present invention can improve the comprehensive balance effect of bending strength, electrostatic capacitance and hole uniformity and quantity, especially the electrostatic capacitance.
[0069] Although the embodiments of the present invention have been disclosed as above, they are not limited to the applications listed in the specification and the implementation modes. They can be fully applied to various fields suitable for the present invention. For those skilled in the art, additional modifications can be easily implemented. Therefore, without departing from the general concept defined by the claims and the scope of equivalents, the present invention is not limited to specific details.
Claims
1. A medium-pressure etched foil, wherein the medium-pressure etched foil is based on a method for manufacturing a medium-pressure etched foil, wherein the method for manufacturing the medium-pressure etched foil is characterized in that: The steps include: S1. Pretreatment: placing the aluminum foil in a pretreatment solution at a temperature of 40-55° C. and soaking it for 0.5-1 min to obtain an aluminum foil sheet soaked in the pretreatment solution; placing the aluminum foil sheet soaked in the pretreatment solution in a vacuum chamber of a coating machine for nano-titanium coating; S2, primary pore formation: place the pre-treated aluminum foil in the primary mixed treatment solution at a temperature of 45-60°C and soak for 1-1.5 minutes, and continuously apply a current density of 10-20A / dm 2 The direct current is drained, and then the primary mixed treatment solution is continuously sprayed for 20-30 minutes at a spray flow rate of 8-10 L / h to obtain an aluminum foil sheet treated with the primary mixed treatment solution; S3, secondary pore formation: The aluminum foil treated with the primary mixed treatment solution in S2 is washed with pure water, and after washing, it is placed in a secondary mixed treatment solution at a temperature of 50-60°C and immersed for 1-3 minutes, and a current density of 6-8A / dm is continuously applied. 2 A direct current is applied to obtain an aluminum foil sheet treated with a secondary mixed treatment solution; S4, heat treatment: the aluminum foil treated with the secondary mixed treatment solution in S3 is washed with pure water and then heat treated to form an aluminum oxide film with a thickness of ≤5 nm; S5, three-stage hole expansion: placing the heat-treated aluminum foil in a three-stage mixed treatment solution at a temperature of 60-75° C. and soaking it for 2-5 minutes to obtain an aluminum foil treated with the three-stage mixed treatment solution; S6, post-treatment: the aluminum foil treated with the three-stage mixed treatment solution is placed in a nitric acid solution at a temperature of 40-50° C. and soaked for 2-3 minutes, and then taken out and washed with pure water to obtain a medium-pressure corrosion foil; In step S1, the pretreatment solution is a phosphoric acid solution with a mass percentage of 5-10%; In step S4, the heat treatment step is specifically: S101, the aluminum foil that has been treated with the secondary mixed solution is first treated with a high-frequency alternating current of 500-1000 Hz, with a current density of 0.05-0.1 A / cm 2 , the electrolyte is 0.5-1.5mol / L oxalic acid solution, and the solution temperature is 50-60℃; S102, placing the aluminum foil sheet treated by high-frequency alternating current at a temperature of 100-120° C. and baking for 0.5-1 min to obtain a heat-treated aluminum foil sheet.
2. A medium voltage corrosion foil according to claim 1, characterized in that: In step S1, the nano-titanium plating treatment is specifically as follows: adjusting the coating vacuum chamber to 5×10~3Pa, 200-250 degrees Celsius, and keeping warm for 20-30 minutes; ventilating argon gas into the coating vacuum chamber to maintain the pressure at 0-0.4 Pa; connecting the bias power supply, adjusting the bias voltage to 250-280V, and performing discharge cleaning for 20-30 minutes; Set the bias voltage between 120-170V, turn on the ion cleaning of the ion source for 20-30 minutes, turn on the arc source titanium target, adjust the bias voltage to 150-200V, the target current to 60-80A, and bombard the titanium target with ions for 3-5 minutes; adjust the vacuum degree to 0.5-0.8Pa, adjust the bias voltage to 50V-60V, and perform arc plating for 5 to 7 minutes.
3. The medium voltage corrosion foil according to claim 1, characterized in that: In step S2, the primary mixed treatment solution is composed of 1-5% by mass of sulfuric acid solution, 5-10% by mass of hydrochloric acid solution and 5-10% by mass of Al 3+ The solution is prepared by mixing.
4. The medium voltage corrosion foil according to claim 1, characterized in that: In step S3, the secondary mixed treatment solution is composed of 5-10% nitric acid solution, 0.5-1% graphene, 0.5-1% buffer and 5-10% Al 3+ Solution.
5. The medium voltage corrosion foil according to claim 1, characterized in that: In step S5, the three-stage mixed treatment solution is composed of 5-10% nitric acid solution, 3-5% sulfuric acid solution, 0.5-1% buffer and Al 3+ Solution.
6. A medium voltage corrosion foil according to claim 4 or 5, characterized in that: The buffer is one of sodium polypropylene sulfonate, sodium glycolate or sodium polyacrylate.
7. A medium voltage corrosion foil according to claim 3, 4 or 5, characterized in that: The Al 3+ The solution is one or more of aluminum nitrate, aluminum chloride, and aluminum sulfate.
Citation Information
Patent Citations
Capacitor aluminium foil and its preparing method
CN101071684A
Method for manufacturing medium and high-voltage anodic aluminum foil
CN101964256A