Semiconductor device manufacturing method and semiconductor device

By forming etching openings in the second mask layer offset by a set distance on the substrate during photolithography rework, the problem of poor opening morphology after the photoresist is removed is solved and the quality and uniformity of the openings are improved. sex.

CN118448256BActive Publication Date: 2024-10-18WUHAN XINXIN SEMICON MFG CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410902841.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-08
Publication Date
2024-10-18
Estimated Expiration
2044-07-08

AI Technical Summary

Technical Problem

During the photolithography rework process, the removal of the photoresist and the re-formation of the mask layer lead to poor hole morphology, which affects the quality and uniformity of the holes, especially deep and wide holes.

Method used

By forming a first mask layer on the substrate and removing it to form a shallow groove, and then forming a second mask layer at a position offset by a set distance, the second mask layer is used to etch the substrate to form openings to avoid removal. The shallow grooves in the first mask layer affect the hole morphology.

Benefits of technology

The quality and uniformity of openings are improved, and the problem of non-uniformity of subsequent conductive structures is reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118448256B_ABST
    Figure CN118448256B_ABST
Patent Text Reader

Abstract

The present invention relates to a method for manufacturing a semiconductor device and a semiconductor device. In the manufacturing method, after a first mask layer having a first opening is formed on a substrate, the first mask layer is removed, a shallow groove is formed on the substrate corresponding to the first opening, and then a second mask layer having a second opening is formed, the pattern of the second opening is the pattern of the first opening offset by a set distance, and then the second mask layer is used as a mask to etch the substrate corresponding to the second opening to form an opening. With this manufacturing method, the shallow groove formed on the substrate corresponding to the first opening after removing the first mask layer will not further affect the morphology of the opening, which helps to improve the quality and uniformity of the opening and the subsequent conductive structure formed based on the opening. The semiconductor device can be formed using the above manufacturing method.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of semiconductor technology, and in particular to a method for manufacturing a semiconductor device and a semiconductor device. Background Art

[0002] Photolithography is an important technology in semiconductor manufacturing. The photolithography process usually requires the steps of spin coating photoresist, soft baking, alignment exposure, post-baking, development, hard baking, etching and photoresist removal. After development, if inspection finds that there are certain problems with the photoresist and the pattern, photolithography rework (PR rework) is required to remove the existing photoresist on the substrate before performing the above-mentioned photolithography process.

[0003] During photolithography rework, in order to remove the existing photoresist on the substrate, a process of oxygen plasma ashing (Asher treatment) followed by wet cleaning (WET clean) is usually adopted. However, studies have found that when a new photoresist layer is used as a mask to form openings in the substrate, the opening morphology is poor, which affects the quality and uniformity of the opening and the conductive structure formed based on the opening, especially for openings with a large depth-to-width ratio. Summary of the invention

[0004] Research has found that after forming a patterned mask layer on a substrate, the process of reworking and removing the mask layer (such as photoresist or other mask materials) will cause the surface morphology of the substrate not covered by the mask layer to change, which is an important reason for the poor morphology of the openings formed after the mask layer is remade and based on the remade mask layer. In order to improve the morphology of the openings made after rework and improve the quality and uniformity of the openings, the present invention provides a method for manufacturing a semiconductor device and a semiconductor device.

[0005] The method for manufacturing a semiconductor device provided by the present invention comprises:

[0006] providing a substrate;

[0007] forming a first mask layer on the substrate, wherein the first mask layer has a first opening, and removing the first mask layer, a shallow groove is formed on the substrate corresponding to the first opening;

[0008] forming a second mask layer on the substrate, wherein the second mask layer has a second opening, and a pattern of the second opening is the pattern of the first opening shifted by a set distance; and

[0009] The second mask layer is used as a mask to etch the substrate corresponding to the second opening to form an opening.

[0010] Optionally, the substrate has a photolithography alignment mark, and after the first mask layer is formed on the substrate and before the first opening is formed in the first mask layer, the alignment mark on the mask having the first opening pattern layer is aligned with the photolithography alignment mark on the substrate; after the second mask layer is formed on the substrate and before the second opening is formed in the second mask layer, the alignment mark on the mask having the second opening pattern layer is aligned with the photolithography alignment mark on the substrate, and after alignment, the substrate is offset by the set distance relative to the position during alignment.

[0011] Optionally, the first mask layer and the second mask layer are respectively a first photoresist layer and a second photoresist layer, the first photoresist layer is exposed and developed to form the first opening, and the second photoresist layer is exposed and developed using a mask for exposing the first photoresist layer to form the second opening.

[0012] Optionally, removing the first photoresist layer includes:

[0013] performing an oxygen plasma ashing process to remove at least a portion of the first photoresist layer; and

[0014] A wet cleaning process is performed to remove the first photoresist layer remaining on the surface of the substrate.

[0015] The base chip includes a substrate and a hard mask layer stacked on the surface of the substrate, and the opening extends from the surface of the hard mask layer into the substrate.

[0016] Optionally, after forming the opening, the manufacturing method further comprises:

[0017] forming an isolation oxide layer along the inner wall of the opening; and

[0018] The opening is filled with a conductive material.

[0019] Optionally, the base sheet includes a substrate, a rewiring layer formed on the substrate, and a dielectric layer covering the rewiring layer, and the opening penetrates the dielectric layer and exposes the rewiring layer.

[0020] Optionally, after forming the opening, the manufacturing method further comprises:

[0021] forming an isolation oxide layer along the inner wall of the opening;

[0022] forming an opening in the isolation oxide layer at the bottom wall of the opening to expose the redistribution layer; and

[0023] The opening is filled with a conductive material.

[0024] Optionally, the set distance is greater than or equal to 100 microns.

[0025] On the other hand, the present invention provides a semiconductor device, comprising a substrate and a shallow groove and an opening formed in the substrate, the pattern of the shallow groove being a pattern formed on the substrate before the pattern of the opening is formed and when the first mask layer is removed after a first opening is formed in a first mask layer formed on the substrate, the pattern of the opening being a pattern formed by etching the substrate using a second mask layer having a second opening as a mask, wherein the pattern of the second opening is the pattern of the first opening after being offset by a set distance.

[0026] Optionally, the semiconductor device further includes:

[0027] an isolation oxide layer covering at least the sidewalls of the opening; and

[0028] A conductive material covers the isolation oxide layer and fills the opening.

[0029] Optionally, the semiconductor device is an interposer for 2.5D integration, and the opening passes through the substrate; or, the substrate includes a substrate, a rewiring layer formed on the substrate, and a dielectric layer covering the rewiring layer, and the opening passes through the dielectric layer and exposes the rewiring layer.

[0030] By utilizing the method for manufacturing a semiconductor device provided by the present invention, the position of the opening corresponds to the formation of the second opening, and the pattern of the second opening is the pattern of the first opening in the first mask layer after being offset by a set distance. In this way, the shallow groove formed on the substrate corresponding to the first opening after removing the first mask layer will not further affect the morphology of the opening, which helps to improve the quality and uniformity of the opening and the subsequent conductive structure formed based on the opening.

[0031] The semiconductor device provided by the present invention includes a substrate and a shallow groove and an opening formed in the substrate, the pattern of the opening is a pattern formed by etching the substrate using a second mask layer having a second opening as a mask, and the pattern of the second opening is the pattern of the first opening after being offset by a set distance, so that the morphology of the opening is not affected by the shallow groove, and the morphology of the opening and the quality and uniformity of the conductive structure subsequently formed corresponding to the opening are better. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figures 1 to 7 A cross-sectional schematic diagram of a method for performing photolithography rework and forming an opening filled with a conductive material in a substrate.

[0033] Figure 8 It is a schematic flow chart of a method for manufacturing a semiconductor device according to an embodiment of the present invention.

[0034] Fig. 9 and Fig.10 They are respectively a cross-sectional schematic diagram and a plan schematic diagram after a first opening is formed in a first photoresist layer in a method for manufacturing a semiconductor device according to an embodiment of the present invention.

[0035] Fig.11 and Fig.12 They are respectively a cross-sectional schematic diagram and a plan schematic diagram after removing the first photoresist layer in the method for manufacturing a semiconductor device according to an embodiment of the present invention.

[0036] Fig.13 It is a cross-sectional schematic diagram after forming a second photoresist layer on a substrate in a method for manufacturing a semiconductor device according to an embodiment of the present invention.

[0037] Fig.14 It is a plan view schematically showing a method for manufacturing a semiconductor device according to an embodiment of the present invention after a second photoresist layer is formed on a substrate.

[0038] Fig.15 and Fig.16 They are respectively a cross-sectional schematic diagram and a plan schematic diagram after a second opening is formed in a second photoresist layer in a method for manufacturing a semiconductor device according to an embodiment of the present invention.

[0039] Fig.17 It is a cross-sectional schematic diagram after forming an opening in a substrate in a method for manufacturing a semiconductor device according to an embodiment of the present invention.

[0040] Fig.18 It is a cross-sectional schematic diagram after forming an isolation oxide layer and a conductive material in an opening in a method for manufacturing a semiconductor device according to an embodiment of the present invention. DETAILED DESCRIPTION

[0041] The following is a further detailed description of the method for manufacturing a semiconductor device and a semiconductor device of the present invention in conjunction with the accompanying drawings and specific embodiments. According to the following description, the advantages and features of the present invention will be clearer. It should be understood that the drawings in the specification are all in a very simplified form and are all in non-precise proportions, which are only used to conveniently and clearly assist in explaining the purpose of the embodiments of the present invention. It should be noted that the order of the steps in the method presented herein is not necessarily the only order for performing these steps, some of the steps described may be omitted and / or some other steps not described herein may be added to the method. It should be understood that spatial relative terms are intended to include different orientations in use or operation in addition to the orientation of the device described in the figure. For example, if the structure in the figure is inverted or positioned in other different ways (such as rotation), the exemplary term "on..." may also include "under..." and other orientation relationships.

[0042] For ease of understanding, first combine Figures 1 to 7A method for performing photolithography rework and forming an opening filled with a conductive material in a substrate is described. The method includes the following steps:

[0043] Reference Figure 1 First, a first photoresist layer PR1 is formed on a substrate 100, and exposure and development are performed to form a first opening 10 in the first photoresist layer PR1. The substrate 100 includes, for example, a substrate 110 and a hard mask layer 120 stacked on a surface of the substrate 110.

[0044] Reference Figure 2 After that, since the developed first photoresist layer PR1 does not meet the requirements and needs to be removed, an oxygen plasma ashing process is first performed to remove at least a portion of the first photoresist layer PR1. Under the action of oxygen plasma, the surface of the substrate 100 exposed by the first opening 10 will have characteristics different from the surface of the substrate 100 not exposed;

[0045] Reference Figure 3 Then, wet cleaning is used to remove the remaining first photoresist layer PR1. During this process, the surface of the substrate 100 exposed by the first opening 10 is corroded by the cleaning solution and is lost. The thickness uniformity of the hard mask layer 120 and the surface morphology of the substrate 100 exposed by the first opening 10 are deteriorated. A shallow groove 10a is formed in the area of ​​the substrate 100 exposed by the first opening 10. Since the cleaning solution will corrode laterally, the shallow groove 10a has a cross-sectional morphology that is wide at the top and narrow at the bottom.

[0046] Reference Figure 4 After that, the photoresist is re-spin-coated and exposed and developed to form a second photoresist layer PR2 having a second opening 20 on the substrate 100. Since it is a rework, the second photoresist layer PR2 and the first photoresist layer PR1 are exposed using the same mask, so that the second openings 20 correspond to the first openings 10 one by one and the positions of each group of corresponding first openings 10 and second openings 20 are substantially the same, as shown in FIG. Figure 4 As shown, the second photoresist layer PR2 also covers a portion of the shallow groove 10a;

[0047] Reference Figure 5 Then, using the second photoresist layer PR2 as a mask, a dry etching process is performed to etch the substrate 100 to form an opening 101. During the etching process, the second photoresist layer PR2 at the opening of the opening 101 is removed due to plasma scattering, so that the side wall of the shallow groove 10a is exposed, resulting in enhanced plasma scattering, so that the side wall of the shallow groove 10a is etched, and the width of the opening of the opening 101 is significantly increased compared with the width of the middle and bottom of the opening 101;

[0048] Reference Figure 6After that, the second photoresist layer PR2 is removed, and an isolation oxide layer 130 is formed on the inner wall of the opening 101 by a thermal oxidation process. In the thermal oxidation process, since the width of the opening 101 is large, the amount of process gas entering the opening 101 is also large, resulting in the isolation oxide layer 102 formed on the inner wall of the opening 101 being thicker than the isolation oxide layer formed without photolithography rework;

[0049] Reference Figure 7 Next, a conductive material 140 is deposited to fill the opening 101 and cover the surface of the hard mask layer 120 , and then CMP (chemical mechanical polishing) is performed to fill the remaining conductive material 140 in the opening 101 .

[0050] In the above process, the etching process of removing the first photoresist layer PR1 will cause the formation of a shallow groove 10a in the area of ​​the substrate 100 exposed by the first opening 10, which will deteriorate the surface morphology of the substrate 100 in this area. Moreover, the greater the thickness of the first photoresist layer PR1 and the longer the etching time, the larger the shallow groove 10a will be. The existence of the shallow groove 10a will affect the morphology of the opening 101, resulting in the deterioration of the uniformity of the openings 101 at different positions, and will cause the thickness of the isolation oxide layer 130 to be larger than the set value. The quality and uniformity of the conductive structure formed after filling the conductive material 140 in the opening 101 will also be affected.

[0051] In the method for manufacturing a semiconductor device according to an embodiment of the present application, in order to improve the morphology of the openings made after reworking of a mask layer formed of photoresist and / or other mask materials, after removing the first mask layer having the first opening, the second opening in the second mask layer is used to define the position of the opening, and the pattern of the second opening is the pattern of the first opening after being offset by a set distance, so that the shallow groove formed on the substrate corresponding to the first opening after removing the first mask layer will not further affect the morphology of the opening, which helps to improve the quality and uniformity of the opening and the conductive structure formed based on the opening. The specific description is as follows.

[0052] Fig. 9 and Fig.10 The cross-sectional structure and local plane area of ​​the substrate are shown respectively, wherein Fig. 9 For example, along Fig.10 The cross section taken along the XY line in . Figure 8 , Fig. 9 and Fig.10 In the method for manufacturing a semiconductor device according to an embodiment of the present invention, step S1 is first performed: providing a substrate 200 .

[0053] As an example, the semiconductor device to be manufactured is an interposer for 2.5D integration, and the interposer needs to form openings in the substrate 200 using the semiconductor device manufacturing method of the present invention, so as to further form conductive holes penetrating the substrate 200 later.

[0054] The substrate 200 includes a substrate 210 and a hard mask layer 220 stacked on the surface of the substrate 210. The substrate 210 may be a silicon substrate, a silicon germanium substrate, a silicon carbide substrate, a silicon on insulator (SOI) substrate, a germanium on insulator substrate, a silicon germanium on insulator substrate, or a III-V compound substrate (such as a gallium nitride substrate or a gallium arsenide substrate), or may be other substrates for carrying semiconductor components known to those skilled in the art. The hard mask layer 220 may include at least one of silicon nitride, silicon oxide, and silicon oxynitride. In the following description, the substrate 210 is, for example, a silicon substrate, and the hard mask layer 220 is, for example, silicon oxide.

[0055] like Fig.10 As shown, in order to facilitate the definition of the formation position of the opening, a photolithography alignment mark S is formed on the surface of the substrate 200, and the photolithography alignment mark S can be formed on the surface of the substrate 200 by a photolithography process. In this embodiment, the photolithography alignment mark S is, for example, a zero-layer alignment mark (Zero Mark), that is, before forming the first mask layer described below, the substrate 200 only has a pattern layer corresponding to the zero-layer alignment mark. In another embodiment, the photolithography alignment mark S is, for example, a front-layer alignment mark. In another embodiment, the substrate 200 includes a substrate, a rewiring layer (RDL layer) formed on the substrate, and a dielectric layer covering the rewiring layer. It is necessary to use the method for manufacturing a semiconductor device of the present invention to form an opening in the dielectric layer to expose the rewiring layer, so as to further form a via connected to the rewiring layer.

[0056] Reference Figure 8 , Fig. 9 , Fig.10 , Fig.11 and Fig.12 , step S2 is performed: forming a first mask layer on the substrate 200, the first mask layer having a first opening 10, removing the first mask layer, and forming a shallow groove 10a on the substrate 100 corresponding to the first opening 10. After the first mask layer is formed on the substrate 200 and before the first opening 10 is formed on the first mask layer, aligning the alignment mark on the photomask having the pattern layer of the first opening 10 with the photolithography alignment mark S on the substrate 200.

[0057] The material of the first mask layer may be a mask layer material known in the art, for example, the first mask layer includes at least one of a hard mask layer and a photoresist layer. In the embodiment of the present application, the first photoresist layer PR1 is taken as an example for the first mask layer. After the first photoresist layer PR1 is coated on the substrate 200, the photolithography alignment mark S is used for pre-exposure alignment, and the first photoresist layer PR1 is exposed and developed to form a first opening 10 in the first photoresist layer PR1. In other embodiments, the first opening 10 may be formed in the first mask layer by etching or other processes.

[0058] A first photoresist layer PR1 can be formed on the surface of the hard mask layer 220 by spin coating. The first photoresist layer PR1 can be a positive photoresist or a negative photoresist, and its thickness can be set according to the needs of subsequent etching. As an example, the thickness of the first photoresist layer PR1 is greater than or equal to 5 microns, for example, in the range of 5 microns to 15 microns. During pre-exposure alignment, the alignment mark on the mask with the opening pattern layer is aligned with the photolithography alignment mark S on the substrate 200. After exposure and development, a first opening 10 is formed in the first photoresist layer PR1. The area exposed by the first opening 10 is the area where the opening is planned to be formed in the substrate 200, so the width of the first opening 10 is the designed width of the opening, for example, in the range of 3 microns to 8 microns. Fig.10 As shown, for example, a plurality of first openings 10 are formed in the first photoresist layer PR1.

[0059] The first mask layer may be removed by a method known in the art, such as an etching process. In the embodiment of the present application, removing the first photoresist layer PR1 may include the following process: first, performing an oxygen plasma ashing process (Asher treatment) to remove at least a portion of the first photoresist layer PR1; then, performing a wet cleaning process to remove the remaining first photoresist layer PR1. Fig.11 and Fig.12 ,and Figure 2 and Figure 3 The situation of removing the first photoresist layer PR1 is similar to that shown. Under the action of oxygen plasma, the surface of the substrate 200 exposed by the first opening 10 will have characteristics different from the surface of the unexposed substrate 200. In the process of removing the remaining first photoresist layer PR1 using a wet cleaning process, the surface of the substrate 200 exposed by the first opening will be corroded and lost by the cleaning liquid, and the thickness uniformity of the hard mask layer 120 and the surface morphology of the substrate 200 exposed by the first opening 10 will deteriorate. A shallow groove 10a is formed in the area of ​​the substrate 200 exposed by the first opening 10. Since the cleaning liquid will corrode laterally, the shallow groove 10a has a cross-sectional morphology that is wide at the top and narrow at the bottom.

[0060] Reference Figure 8 , Fig.13 , Fig.14 , Fig.15 and Fig.16 Then, step S3 is performed: a second mask layer is formed on the substrate 200, the second mask layer has a second opening 20, and the pattern of the second opening 20 is the pattern of the first opening 10 after being offset by a set distance. After the second mask layer is formed on the substrate 200 and before the second opening 20 is formed on the second mask layer, the alignment mark on the mask having the pattern layer of the second opening 20 is aligned with the photolithography alignment mark S on the substrate 200, and after the alignment, the substrate 200 is offset by a set distance relative to the position during the alignment.

[0061] The material of the second mask layer can be a mask layer material well known in the art, for example, the second mask layer includes at least one of a hard mask layer and a photoresist layer. In the embodiment of the present application, the second photoresist layer PR2 is used as an example for the second mask layer. After the second photoresist layer PR2 is coated on the substrate 200, the photolithography alignment mark S is used for pre-exposure alignment, and after alignment, the substrate 200 is offset by a set distance relative to the position during alignment. The second photoresist layer PR2 is a reworked photoresist layer, which can be formed on the surface of the hard mask layer 220 by spin coating. The second photoresist layer PR2 and the first photoresist layer PR1 are, for example, the same photoresist. As an example, the thickness of the second photoresist layer PR2 is greater than or equal to 5 microns, for example, in the range of 5 microns to 15 microns. It can be understood that the materials of the first mask layer and the second mask layer can be the same or different.

[0062] In order to avoid the influence of the uneven area (i.e., the area where the shallow groove 10a is formed) caused by the first opening 10 exposing the substrate 200 when removing the first mask layer on the subsequent process, in step S3, after alignment using the photolithography alignment mark S, the substrate 200 covered with the second mask layer is offset relative to the position during alignment, so that the position where the second mask layer is to form the second opening no longer falls on the substrate 200 area corresponding to the above-mentioned first opening 10. The specific offset direction and offset distance can be set according to the requirements of not overlapping the second opening 20 formed subsequently with the first opening 10, not affecting other structures to be manufactured in the semiconductor device, and not affecting the position of the opening to be formed subsequently. As an example, the set distance of the substrate 200 offset relative to the position during alignment is greater than or equal to 100 microns.

[0063] The second opening 20 may be formed in the second mask layer in a manner well known in the art, for example, the second opening 20 may be formed by etching or other processes. In the embodiment of the present application, the second photoresist layer PR2 is exposed and developed to form the second opening 20, and the mask used to expose the second photoresist layer PR2 is the same as the mask used to expose the first photoresist layer PR1, that is, the second photoresist layer PR2 is exposed and developed using the mask used to expose the first photoresist layer PR1, so that the second photoresist layer PR2 has a second opening 20, and the second opening 20 does not overlap with the area of ​​the substrate 200 corresponding to the first opening 10. However, since the second mask layer is offset with the substrate 200 after alignment before exposure, the position where the second mask layer is to form the second opening no longer falls on the area of ​​the substrate 200 corresponding to the first opening 10, and the second opening 20 does not overlap with the area of ​​the substrate 200 corresponding to the first opening 10. As an example, a plurality of second openings 20 are formed in the second mask layer, and each second opening does not overlap with the position of any first opening.

[0064] Reference Figure 8 and Fig.17 Then, step S4 is performed to etch the substrate 200 corresponding to the second opening 20 using the second mask layer as a mask to form an opening 201.

[0065] Among them, the pattern of the shallow groove 10a is a pattern formed on the substrate 200 before the pattern of the opening 201 is formed, when the first mask layer is removed after the first opening 10 is formed in the first mask layer formed on the substrate 200, and the pattern of the opening 201 is a pattern formed by etching the substrate 200 using the second mask layer having the second opening 20 as a mask, wherein the pattern of the second opening 20 is the pattern of the first opening 10 after being offset by a set distance.

[0066] The substrate 200 is etched to form the opening 201, for example, by using a dry etching process. As an example, the hard mask layer 220 may be first etched using a process condition for etching an oxide layer, and then the substrate 210 may be etched using a process condition for etching silicon to form the opening 201 extending from the surface of the hard mask layer 220 to the inside of the substrate 210. The depth of the opening 201 may be set as required, for example, to be a deep hole. Furthermore, the aspect ratio of the opening 201 may be greater than or equal to 15, for example.

[0067] In this embodiment, since the second opening 20 does not overlap with the substrate 200 area corresponding to the first opening 10, that is, the second opening 20 avoids the uneven substrate 200 area corresponding to the first opening 10, the surface of the substrate 200 exposed by the second opening 20 is close to the morphology of the surface of the substrate 200 that has not been reworked by photolithography, and the surface of the substrate 200 exposed by the second opening 20 does not have the shallow groove 10a of the substrate 200 area corresponding to the first opening 10. When etching the substrate 200 corresponding to the second opening 20, compared with Figure 5 In the etching process shown, the scattering of plasma is relatively weak, so that the width of the opening of the formed opening 201 is relatively consistent with the width of the middle and bottom of the opening, and the quality and uniformity of the opening 201 are better.

[0068] In this embodiment, after the second mask layer is exposed, the mask pattern formed meets the process requirements, and thus no rework is required. However, the present invention is not limited thereto. In another embodiment, if the mask pattern formed by the second mask layer does not meet the relevant process requirements, rework can be performed again. The second mask layer can be removed by removing the first mask layer, and a third mask layer can be re-formed. The third mask layer can be aligned before exposure using a photolithography alignment mark S. After alignment, the substrate 200 covered with the third mask layer is offset, and then exposure and development are performed to form a third opening in the third mask layer. Furthermore, by offsetting, the third opening is made to have no overlap with the regions of the substrate 200 corresponding to the first opening 10 and the second opening 20. The third mask layer is then used as a mask to etch the substrate 200 to form an opening. In this way, the opening can be prevented from being formed in the uneven regions of the substrate 200 corresponding to the first opening 10 and the regions of the substrate 200 corresponding to the second opening 20, thereby improving the quality and uniformity.

[0069] Optionally, after forming the opening 201, the opening 201 is used as an alignment mark for a subsequent patterning process; or, during the process of forming the opening 201, a new alignment mark is simultaneously formed in the edge area of ​​the substrate 201, and the subsequent patterning process can use the new alignment mark for alignment.

[0070] After forming the opening 201, the second mask layer can be removed. Fig.18 The method for manufacturing the semiconductor device may further include the following process: forming an isolation oxide layer 230 along the inner wall of the opening 201, wherein the isolation oxide layer 230 is formed by placing the substrate 200 having the opening 201 in a furnace tube using a thermal oxidation process. Figure 5The opening 101 shown in the figure has better quality and uniformity of the opening 201 of the present embodiment, the thickness of the isolation oxide layer 230 is easier to control, and the thickness uniformity of the isolation oxide layer 230 formed in different openings 201 is better; then, the conductive material 240 is filled in the opening 201, and specifically, the conductive material 240 can be deposited so that the conductive material 240 fills the opening 201 and covers the surface of the hard mask layer 220, and then a CMP process is performed to remove the conductive material 240 covering the surface of the hard mask layer 220 and part of the hard mask layer 220, and the remaining conductive material 240 is filled in the opening 201. In addition, optionally, in order to form a via in the substrate 200, after the conductive material 240 is filled in the opening 201, the substrate 210 can be thinned from the back side of the substrate 200 (i.e., the side surface of the substrate 210 away from the hard mask layer 220) to expose the conductive material 240 in the opening 201. In this embodiment, compared with the Figures 5 to 7 As shown in the opening 101, the width uniformity of the opening 201 in this embodiment is better. Under the same thermal oxidation conditions, the thickness of the isolation oxide layer 230 formed in the opening 201 of this embodiment is smaller. When the substrate 210 is thinned from the back side of the substrate 200 to expose the conductive material 240 in the opening 201, the thickness of the isolation oxide layer 230 that needs to be removed is smaller, which can shorten the time of the thinning process and reduce the difficulty.

[0071] As described above, in another embodiment, the substrate 200 includes a substrate, a rewiring layer formed on the substrate, and a dielectric layer covering the rewiring layer. The above steps S1 to S4 can be used to form an opening in the dielectric layer to expose the rewiring layer, wherein, when performing step S3, the photolithography alignment mark corresponding to the rewiring layer can be used to perform pre-exposure alignment, and after alignment, the substrate 200 covering the second mask layer is offset by a set distance relative to the position during alignment, and it is ensured that the offset position can make the second opening formed in step S3 expose the same connection node of the rewiring layer, and the connection node is, for example, a pad of the rewiring layer, that is, by setting a suitable pad size and offset distance, after the substrate 200 is offset in step S3, the formation area of ​​the second opening in the second mask layer and the formation area of ​​the second opening before the offset fall within the same pad range. In this embodiment, after forming the opening 201 penetrating the dielectric layer, the second mask layer is removed, and the following process may also be included: forming an isolation oxide layer along the inner wall of the opening 201; etching the isolation oxide layer on the bottom wall of the opening 201, and forming an opening exposing the rewiring layer in the isolation oxide layer on the bottom wall of the opening 201; then, filling the opening 201 with a conductive material, for example, first depositing a conductive material in the opening 201 and on the surface of the dielectric layer, and then performing a CMP process to remove the conductive material covering the surface of the dielectric layer, and filling the remaining conductive material in the opening 201 to form a via hole connected to the rewiring layer.

[0072] In the method for manufacturing a semiconductor device described in the above embodiment, an opening 201 is formed in the substrate 200 corresponding to the second opening 20 in the second mask layer (for example, the second photoresist layer PR2), and the second opening 20 has no overlap with the area of ​​the substrate 200 corresponding to the first opening 10 in the first mask layer (for example, the first photoresist layer PR1). Therefore, the effect of etching and removing the first mask layer on the area of ​​the substrate 200 corresponding to the first opening 10 will not further affect the morphology of the opening 201, which helps to improve the quality and uniformity of the opening 201 and the subsequent conductive structure (for example, a via in this embodiment) formed based on the opening 201.

[0073] The embodiment of the present invention also includes a semiconductor device, which can be formed by using the method for manufacturing the semiconductor device described in the above embodiment. Figures 8 to 18 The semiconductor device includes a substrate 200 and a shallow groove 10a and an opening 201 formed in the substrate 200. The pattern of the shallow groove 10a is a pattern formed on the substrate 200 before the pattern of the opening 201 is formed, when the first mask layer (for example, a first photoresist layer PR1) is removed after a first opening 10 is formed in the first mask layer formed on the substrate 200, and the pattern of the opening 201 is a pattern formed by etching the substrate 200 using a second mask layer (for example, a second photoresist layer PR2) having a second opening 20 as a mask, wherein the pattern of the second opening 20 is the pattern of the first opening 10 after being offset by a set distance.

[0074] In some embodiments, the semiconductor device may further include an isolation oxide layer 230 covering at least the sidewall of the opening 201 and a conductive material 240 covering the isolation oxide layer 230 and filling the opening 201 .

[0075] In one embodiment, the semiconductor device is used to form an interposer of 2.5D integration, and the opening 201 penetrates the substrate 200, so that the opening 201 and the isolation oxide layer 230 and the conductive material 240 filled therein constitute a via hole penetrating the substrate 200. In another embodiment, the substrate 200 includes a substrate, a rewiring layer formed on the substrate, and a dielectric layer covering the rewiring layer, and the opening 201 penetrates the dielectric layer and exposes the rewiring layer, so that the opening 201 and the conductive material filled therein constitute a via hole penetrating the dielectric layer and connecting the rewiring layer, and the electrical properties of the rewiring layer can be led out.

[0076] In the semiconductor device, the pattern of the opening 201 is offset by a set distance compared to the previous layer pattern corresponding to the lithography alignment mark S, and the morphology of the opening 201 is not affected by rework, which helps to improve the quality of the opening 201 and the quality and uniformity of the subsequent conductive structure (in this embodiment, for example, a via) formed corresponding to the opening 201.

[0077] It should be noted that the embodiments in this specification are described in a progressive manner, and each part focuses on the differences from the previous part. The same and similar parts of each part can be understood by reference.

[0078] The above description is only a description of the preferred embodiment of the present invention, and is not any limitation on the scope of rights of the present invention. Any technical personnel in this field can make possible changes and modifications to the technical solution of the present invention by using the methods and technical contents disclosed above without departing from the spirit and scope of the present invention. Therefore, any simple modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention shall fall within the protection scope of the technical solution of the present invention.

Claims

1. A method for manufacturing a semiconductor device, characterized in that: include: providing a substrate; forming a first mask layer on the substrate, wherein the first mask layer has a first opening, and removing the first mask layer, wherein when the first mask layer is removed, a shallow groove is formed on the substrate corresponding to the first opening; forming a second mask layer on the substrate, wherein the second mask layer has a second opening, the pattern of the second opening is the pattern of the first opening shifted by a set distance, and the substrate regions corresponding to the second opening and the first opening do not overlap; and The second mask layer is used as a mask to etch the substrate corresponding to the second opening to form an opening.

2. The method according to claim 1, characterized in that: The substrate has a photolithography alignment mark, and after forming the first mask layer on the substrate and before forming the first opening on the first mask layer, the alignment mark on the mask having the first opening pattern layer is aligned with the photolithography alignment mark on the substrate; After the second mask layer is formed on the substrate and before the second opening is formed in the second mask layer, the alignment mark on the mask having the second opening pattern layer is aligned with the photolithography alignment mark on the substrate, and after alignment, the substrate is offset by the set distance relative to the position during alignment.

3. The method according to claim 1, characterized in that: The first mask layer and the second mask layer are respectively a first photoresist layer and a second photoresist layer. The first photoresist layer is exposed and developed to form the first opening. The second photoresist layer is exposed and developed using a mask that exposes the first photoresist layer to form the second opening.

4. The method according to claim 3, characterized in that: Removing the first photoresist layer includes: performing an oxygen plasma ashing process to remove at least a portion of the first photoresist layer; and A wet cleaning process is performed to remove the first photoresist layer remaining on the surface of the substrate.

5. The method according to claim 1, characterized in that: The base chip includes a substrate and a hard mask layer stacked on the surface of the substrate, and the opening extends from the surface of the hard mask layer into the substrate.

6. The method according to claim 5, characterized in that: After forming the opening, the manufacturing method further comprises: forming an isolation oxide layer along the inner wall of the opening; and The opening is filled with a conductive material.

7. The method according to claim 1, characterized in that: The base sheet includes a substrate, a rewiring layer formed on the substrate, and a dielectric layer covering the rewiring layer. The opening penetrates through the dielectric layer and exposes the rewiring layer.

8. The method according to claim 7, characterized in that: After forming the opening, the manufacturing method further comprises: forming an isolation oxide layer along the inner wall of the opening; forming an opening in the isolation oxide layer at the bottom wall of the opening to expose the redistribution layer; and The opening is filled with a conductive material.

9. The method according to claim 1, characterized in that: The set distance is greater than or equal to 100 micrometers.

10. A semiconductor device, characterized in that: include: substrate; as well as Shallow grooves and openings are formed in the substrate, the pattern of the shallow grooves is a pattern formed on the substrate corresponding to the first opening when the first mask layer is removed after the first opening is formed in the first mask layer formed on the substrate before the pattern of the openings is formed, the pattern of the openings is a pattern formed by etching the substrate using a second mask layer having a second opening as a mask, wherein the pattern of the second opening is the pattern of the first opening after being offset by a set distance, and the substrate areas corresponding to the second opening and the first opening do not overlap.

11. The semiconductor device according to claim 10, wherein: The semiconductor device further comprises: an isolation oxide layer covering at least the sidewalls of the opening; and A conductive material covers the isolation oxide layer and fills the opening.

12. The semiconductor device according to claim 10, wherein: The semiconductor device is an interposer for 2.5D integration, and the opening passes through the substrate; or, the substrate includes a substrate, a rewiring layer formed on the substrate, and a dielectric layer covering the rewiring layer, and the opening passes through the dielectric layer and exposes the rewiring layer.

Citation Information

Patent Citations

  • Formation method of shallow trench isolation structure and formation method of semiconductor device

    CN115775766A

  • Photoetching reworking method and semiconductor structure

    CN117219494A