Plastic particles modified from waste plastics and preparation method thereof

By modifying waste plastics, combined with compatibilizers and flame retardants, modified plastic particles with high mechanical properties and good flame retardant properties are formed, which solves the shortcomings of waste plastics in mechanical properties and environmental degradation, and achieves the Higher biodegradation rates and lower environmental pollution.

CN118459998BActive Publication Date: 2024-11-05JIANGSU KESHANG NEW ENERGY TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410928281.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-11
Publication Date
2024-11-05
Estimated Expiration
2044-07-11

AI Technical Summary

Technical Problem

When processing waste plastics, the prior art causes the material to decline mechanical properties, insufficient flame retardant properties, poor impact strength, easy to crack at low temperatures, high water absorption, low service life in humid environments, not easy to degrade, causing environmental hazards. question.

Method used

By using long-chain hexamethylene diisocyanate to modify the waste plastic under the action of hydroxyethanol, combined with the compatibilizer SEPS and silane coupling agent, the type and dosage of plasticizers are adjusted, and inorganic porous materials and halogen are used. Antimony system flame retardant uses wood powder and PHBV to form pore and crack networks, improving the mechanical properties and biodegradation rate of plastics.

Benefits of technology

It significantly improves the mechanical properties of waste plastics, enhances low temperature resistance, improves hydrophobicity, improves flame retardant performance, significantly improves biodegradation rate, and reduces environmental pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118459998B_ABST
    Figure CN118459998B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of polymer materials, specifically to a plastic particle modified from waste plastics and a preparation method thereof. The plastic particle is prepared by reacting modified waste plastics with a matrix to obtain a plastic matrix, and adding a plasticizer, an antioxidant, a flame retardant, and a silane coupling agent to melt and extrude the plastic particle. The present invention treats waste plastics through modification, and the modified waste plastic obtained has high mechanical strength and is resistant to low temperatures; the mechanical properties of the obtained plastic particles are significantly improved through the synergistic effect of the plasticizer and the compatibilizer; the water contact angle of the obtained plastic particles is 108.6° through the grafting and end-capping of the silane coupling agent, and the hydrophobicity is high; the flame retardancy of the particles is improved by the synergistic effect of the flame retardant of inorganic substances and halogen antimony system, while maintaining the mechanical properties; the matrix formed by the cross-linking of wood powder and polymers is used, and the 90-day biodegradation rate of the obtained plastic particles is 58.4%, the biodegradation speed is fast, and environmental pollution is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer materials, in particular to plastic particles modified from waste plastics and a preparation method thereof. Background Art

[0002] Plastic particles are a kind of synthetic polymer compound, commonly known as plastic or resin, which can change shape freely. They are materials made by synthesizing or condensing monomer raw materials, and are composed of synthetic resins and additives such as fillers, plasticizers, stabilizers, lubricants, and colorants. Plastics are generally divided into two types: thermoplastic and thermosetting. Thermoplastic materials soften after heating, harden into shape after cooling, and can soften and change properties repeatedly. Thermosetting materials solidify into a certain shape after heating. If the temperature is too high, it will destroy the internal structure of the molecules, and destroy the structure and performance of the plastic.

[0003] With the rapid development of social economy, people use various plastic products in their daily life. These plastic products are not easy to degrade after being discarded. Randomly discarding them will cause pollution problems. Therefore, the recycling of these discarded plastic products is a technical problem that needs to be solved; these waste plastics are difficult to degrade in the natural environment and can only be treated by incineration or burial. However, a lot of harmful gases will be produced during the incineration process, causing great harm to the environment. During the burial process, toxic substances in some plastic materials will seep out, causing secondary pollution and affecting the utilization value of the land.

[0004] Patent CN201610966970.6 discloses a nano PVC transparent profile and a preparation method thereof, comprising PVC, nano zinc oxide, butyl benzyl phthalate, polypropylene adipate and other additives. The invention adds plasticizers such as butyl benzyl phthalate and polypropylene adipate to improve the properties of plastics. However, the addition of plasticizers causes the soft PVC to become brittle during use, and has poor impact strength, making it difficult to preserve; especially under low temperature conditions, as the temperature decreases, the soft PVC becomes harder and more brittle, and the impact strength decreases rapidly.

[0005] Patent CN201410550006.6 discloses rigid inorganic particle modified polyvinyl chloride plastic particles, including polyvinyl chloride, inorganic rigid particles, montmorillonite, stabilizer, plasticizer, lubricant and antioxidant, wherein the inorganic rigid particles are one of nano calcium carbonate or nano calcium sulfite, however, the preparation process of nano particles is complicated and the cost is relatively high.

[0006] Patent CN201510561627.9 discloses a polypropylene composite plastic particle, including PP, PC, EPDM rubber and ethylene-butylene elastomer mixture and modification additives. The prepared plastic particles have high flame retardancy and high mechanical properties, but the plastic particles prepared by the above process are not high in strength and are prone to breakage during use.

[0007] During the use of plastic products, they are affected by light, heat, oxygen and external forces, and the polymer chain structure will change, and the performance of plastic products will deteriorate irreversibly. The existing waste plastic recycling technology mainly crushes the plastic and then regenerates it by hot melt. However, the added value of directly using waste plastics for granulation and then producing is low, and only some products with poor performance can be obtained. At this time, according to the idea of ​​traditional polymer modification, some performance defects of waste plastics can be modified and regenerated, which can greatly improve the performance of waste plastics and achieve the purpose of reuse. Common modification methods for waste plastics include chemical modification and physical modification.

[0008] However, the flame retardant properties of recycled plastics are also quite different from those of new plastics, so it is necessary to improve the flame retardant system to compensate for the flame retardant properties of recycled plastics. Traditional general-purpose plastic flame retardants are mainly divided into two categories: inorganic hydroxides and organic halogenated hydrocarbons. However, inorganic hydroxide flame retardants are used in large quantities, which damages the mechanical properties of general-purpose plastic materials; organic halogenated hydrocarbon flame retardants are added in small quantities, but they generate toxic volatile gases after combustion, polluting the environment.

[0009] At the same time, recycled plastics have shortcomings such as poor impact strength, high and low temperature resistance, and continuous bending pressure bearing performance, poor hardness, strength, resilience, wear resistance, and easy aging. Only melting treatment results in the performance of recycled plastics failing to meet the use standards. When waste plastics are reused and processed into recycled plastics, the proportion of materials in the waste plastics does not change much, and the materials are not modified, which can easily cause the strength and service life of the recycled plastics to deteriorate.

[0010] In summary, with the development of polymer material industry, plastics have been widely used in various fields and become an important part of people's lives. However, the existing technology uses crushing and melting to regenerate waste plastics. While improving the properties of plastics by improving additives, it will inevitably damage the mechanical properties of plastic materials. In addition, plastics have insufficient flame retardancy, poor impact strength, easy to crack at low temperatures, high water absorption, low service life in humid environments, and are not easy to degrade. The shortcomings of environmental damage cannot be effectively solved.

[0011] Therefore, a plastic particle modified from waste plastics and a preparation method thereof are proposed. Summary of the invention

[0012] The object of the present invention is to provide a plastic particle modified from waste plastic and a preparation method thereof. The waste plastic is modified by using long-chain hexamethylene diisocyanate under the action of hydroxyethanol, and the prepared modified waste plastic has a brittle temperature of -48°C, a bending strength of 53.6MPa, and a notched impact strength of 28.8KJ / m 2 , maintain the mechanical properties of waste plastics and improve low temperature resistance; use a compatibilizer SEPS to modify waste plastics and add a plasticizer for synergistic effect. By adjusting the type and amount of the plasticizer, the tensile strength of the plastic particles obtained is 29.4MPa, and the elongation at break is 235%, thereby improving the mechanical properties of the plastic particles; by using a silane coupling agent to graft the obtained plastic particles, the hydrogen bonding effect of the polar groups in the wood powder on the water molecules is reduced, and the water contact angle of the obtained plastic particles is 108.6°, showing obvious hydrophobicity; inorganic porous materials and halogen antimony system flame retardant systems are selected for synergistic effect, and the impact strength of the obtained plastic particles is 26.8KJ / m2, and the limiting oxygen index is 34. While having good flame retardancy, the mechanical properties are maintained; the present invention utilizes wood powder and PHBV to form interconnected pores and crack networks during the biodegradation process; the 90-day biodegradation rate of the obtained plastic particles is 58.4%, showing a significantly improved biodegradation rate and reducing environmental pollution.

[0013] To achieve the above object, the present invention provides the following technical solutions:

[0014] A method for preparing plastic particles modified from waste plastics, characterized in that the method for preparing the plastic particles comprises the following steps:

[0015] S1 pre-treats waste plastics, heats, extrudes, and cools to obtain recycled plastics; adds 5-50 parts of chain transfer agent and catalyst 1 to 100 parts of the recycled plastics, reacts at 110°C for 4 hours, and rotary evaporates to obtain a reaction system; dissolves the reaction system solvent, adds 10-40 parts of isocyanate and catalyst 2 to react at 80°C for 2 hours to obtain modified plastics; adds the modified plastics to a continuous mixer, adds a compatibilizer under stirring conditions, and mixes at 110°C for 30 minutes to obtain plastic glue; melts and plasticizes the plastic glue in a twin-screw extruder to obtain granules to obtain modified waste plastics;

[0016] S2: drying the polymer and 20-80 parts of wood powder for 12 hours, stirring at 400 r / min for 30 minutes, and sieving to obtain a matrix;

[0017] S3: drying 50 parts of the modified waste plastic and 100-200 parts of the matrix at 100°C for 4 hours to obtain a dried material; adding the dried material into a three-necked flask, dissolving it in acetonitrile, adding catalyst 2, reacting at 80°C for 2 hours, separating and centrifuging, and drying at 60°C for 3 hours to obtain a plastic matrix; adding the plastic matrix into a continuous mixer, adding 20-50 parts of a plasticizer, 10 parts of an antioxidant 1010, and 5-25 parts of a flame retardant under stirring conditions, and mixing at 140°C and 500r / min for 30 minutes to obtain a rubber compound; melt-plasticizing and granulating the rubber compound in a twin-screw extruder to obtain modified plastic particles;

[0018] 100 parts of the modified plastic particles are added into a three-necked flask, acetone and acetic acid are added to dissolve, the temperature is raised to 60-100° C. at 100 r / min, 5-20 parts of a silane coupling agent are added, and the reaction is refluxed for 4-8 hours to obtain a reaction solution; the reaction solution is cooled, separated by centrifugation, rinsed with acetone, and dried at 80° C. for 2 hours to obtain plastic particles.

[0019] Preferably, the waste plastic is selected from one or a mixture of polyvinyl chloride (PVC), polyethylene (PE), polypropylene (PP), polystyrene (PS), and acrylonitrile-butadiene-styrene copolymer (ABS).

[0020] Preferably, the isocyanate is selected from toluene diisocyanate, lysine diisocyanate, isophorone diisocyanate, terephthalylidene diisocyanate, and hexamethylene diisocyanate.

[0021] Preferably, the chain transfer agent is selected from one of mercaptoethanol, hydroxyethanol and aminoethanol; the amount of the chain transfer agent is 10-40 parts.

[0022] Preferably, the polymer is selected from one of polylactic acid, polyethylene, polyhydroxybutyl pentyl ester, and polyhydroxyalkanoate; the amount of the polymer is 100 parts.

[0023] Preferably, the compatibilizer is selected from one of styrene-(ethylene / propylene)-styrene copolymer, ethylene-glycidyl methacrylate, maleic anhydride functionalized ethylene copolymer, and nano-silica; and the amount of the compatibilizer is 10 parts.

[0024] Preferably, the silane coupling agent is selected from one of 3-aminopropyltriethoxysilane, 3-(2,3-epoxypropyloxy)propyltrimethoxysilane, methacryloxypropyltriethoxysilane and N-(2-aminoethyl)-3-aminopropyltrimethoxysilane.

[0025] Preferably, the flame retardant is selected from one or a mixture of expanded vermiculite, organic bentonite, porous boron nitride, expanded flame retardant, antimony trioxide, and decabromodiphenylethane.

[0026] Preferably, the intumescent flame retardant includes 2 parts of ammonium polyphosphate, 6 parts of dipentaerythritol, and 2 parts of melamine.

[0027] Preferably, the plasticizer is selected from one of trioctyl trimellitate, dioctyl adipate, diisononyl phthalate and di(2-ethylhexyl) phthalate.

[0028] Preferably, the first catalyst is azobisisobutyronitrile, and the amount used is 2 parts; the second catalyst is dibutyltin dilaurate, and the amount used is 2 parts.

[0029] Preferably, the operating parameters of the twin-screw extruder are: inlet temperature of 150°C, head temperature of 245°C, and screw speed of 150r / min.

[0030] A plastic particle modified from waste plastics, characterized in that: the plastic particle comprises the plastic matrix prepared from the modified waste plastics and the matrix, the plasticizer, the antioxidant 1010, the flame retardant, and the silane coupling agent; the plastic particle is prepared by any one of the preparation methods described above; the waste plastic has a brittle temperature of -48°C, a bending strength of 53.6MPa, and a notched impact strength of 28.8KJ / m 2 The tensile strength of the plastic particles is 29.4MPa, and the elongation at break is 235%; the water contact angle of the plastic particles is 108.6°; the impact strength of the plastic particles is 26.8KJ / m 2 , the limiting oxygen index is 34; the 90-day biodegradation rate of the plastic particles is 58.4%.

[0031] Compared with the prior art, the present invention has the following beneficial effects:

[0032] 1. The present invention uses long-chain hexamethylene diisocyanate to modify waste plastics under the action of hydroxyethanol, synthesizes modified waste plastics with terminal isocyanate groups through a series of methods, and adjusts the dosage of isocyanate and chain transfer agent to obtain modified waste plastics with a brittle temperature of -48°C, a flexural strength of 53.6MPa, and a notched impact strength of 28.8KJ / m 2 , effectively improving the mechanical properties of waste plastics and increasing the processability of waste plastics. At the same time, the long straight-chain plastic molecules give the modified waste plastics significantly improved low-temperature resistance.

[0033] 2. The present invention uses a compatibilizer SEPS to modify waste plastics, increase the interfacial compatibility between the modified waste plastics and the matrix, and add a plasticizer for synergistic effect. By adjusting the type and amount of the plasticizer, the obtained plastic particles have a tensile strength of 29.4 MPa and an elongation at break of 235%, showing significantly increased tensile strength and elongation at break, thereby improving the mechanical properties of the plastic.

[0034] 3. The present invention uses a silane coupling agent to carry out a grafting reaction on the prepared plastic particles, thereby reducing the hydrogen bonding effect of the polar groups in the wood powder on the water molecules. Compared with the modification by adding a silane coupling agent before mixing and melt extrusion granulation, the hydrophobicity of the plastic particles is significantly improved; by screening the grafting reaction temperature and time, using 10 parts of KH-570 as a silane coupling agent, reacting at 90°C for 6 hours, the water contact angle of the prepared plastic particles is 108.6°, showing obvious hydrophobicity.

[0035] 4. The present invention improves the flame retardant properties of plastic particles by using flame retardants, selects inorganic porous materials and halogen antimony system flame retardant system to work synergistically, avoids the uneven distribution of molecules caused by the large amount of inorganic materials, and reduces the amount of components of the halogen antimony system; the plastic particles prepared by using 15 parts of porous boron nitride-loaded antimony trioxide and decabromodiphenylethane have an impact strength of 26.8KJ / m 2 The limiting oxygen index is 34, and it has good flame retardancy while maintaining mechanical properties.

[0036] 5. The present invention uses a matrix prepared by cross-linking a polymer PHBV with wood powder and modified waste plastics, mixes them under the action of additives such as plasticizers, and melt-extrudes and granulates them to obtain plastic particles. After the wood powder and PHBV are compounded, a network of interconnected pores and cracks is formed during the biodegradation process. The 90-day biodegradation rate of the obtained plastic particles is 58.4%, which shows a significantly improved biodegradation rate and reduces environmental pollution. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] Figure 1 This is a graph showing the effect of plasticizers on the tensile strength of plastic particles. DETAILED DESCRIPTION

[0038] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0039] If the specific conditions are not specified in the examples, the experiments were carried out under conventional conditions or conditions recommended by the manufacturer. If the manufacturers of the reagents or instruments are not specified, they are all conventional products that can be purchased commercially.

[0040] The SEPS described in the present invention is a styrene-(ethylene / propylene)-styrene copolymer, CAS: 132778-07-5.

[0041] The GMA described in the present invention is ethylene-glycidyl methacrylate, CAS: 106-91-2.

[0042] The MAC described in the present invention is a maleic anhydride functionalized ethylene copolymer.

[0043] The TOTM described in the present invention is trioctyl trimellitate, CAS: 25103-12-2.

[0044] The DOA described in the present invention is dioctyl adipate, CAS: 123-79-5.

[0045] The DINP described in the present invention is diisononyl phthalate, CAS: 68515-48-0.

[0046] The DOP described in the present invention is di(2-ethylhexyl) phthalate, CAS: 117-84-0.

[0047] The Sd2O3 described in the present invention is antimony trioxide, CAS: 1309-64-4.

[0048] The DBDPE described in the present invention is decabromodiphenyl ethane, CAS: 84852-53-9.

[0049] The KH-550 described in the present invention is 3-aminopropyltriethoxysilane, CAS: 919-30-2.

[0050] The KH-560 described in the present invention is 3-(2,3-epoxypropoxy)propyltrimethoxysilane, CAS: 2530-83-8.

[0051] The KH-570 described in the present invention is methacryloxypropyltriethoxysilane, CAS: 2530-85-0.

[0052] The KH-792 described in the present invention is N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, CAS: 1760-24-3.

[0053] The PHBV described in the present invention is polyhydroxybutyrate pentyl.

[0054] The PHA described in the present invention is polyhydroxyalkanoate.

[0055] See also Figure 1 The present invention provides a plastic particle modified from waste plastic and a preparation method thereof, and the technical scheme is as follows: Example 1

[0056] Preparation of modified waste plastics:

[0057] 100 parts of waste plastic raw materials were crushed and passed through a 40-mesh sieve to obtain a crushed raw material; the crushed raw material was added to a mixed solvent of methanol and dichloromethane in a volume ratio of 1:1 for washing, and rinsed with distilled water for multiple times to obtain a washed raw material; the washed raw material was demagnetized using an electromagnetic iron remover to obtain a de-impurity raw material; the de-impurity raw material was heated and extruded using a co-melting extruder, and cooled to obtain a recycled plastic; 25 parts of a chain transfer agent, mercaptoethanol, and toluene were added to 100 parts of the recycled plastic, and the mixture was stirred evenly; 2 parts of azobisisobutyronitrile were slowly added dropwise under 110°C oil bath conditions, and the mixture was kept at 110°C for reaction for 4 hours under nitrogen protection, and the solvent was removed by rotary evaporation to obtain a reaction system; toluene solvent was added to the reaction system to dissolve, and the mixture was heated under nitrogen protection. 25 parts of toluene diisocyanate and 2 parts of dibutyltin dilaurate were added, and the mixture was reacted in an oil bath at 80°C for 2 hours. After the reaction solution was cooled, anhydrous n-heptane was added to precipitate, the solvent was filtered out, and the mixture was rinsed with anhydrous n-heptane for 3 times. The mixture was dried in a vacuum drying oven at 60°C for 3 hours to obtain a modified plastic. The modified plastic was added to a continuous mixer, and 10 parts of a compatibilizer styrene-(ethylene / propylene)-styrene copolymer were added in sequence under stirring. The mixture was stirred at 110°C and 500r / min and mixed for 30 minutes to obtain a uniformly mixed plastic glue. The plastic glue was melt-plasticized and granulated in a twin-screw extruder, with an inlet temperature of 150°C, a die head temperature of 245°C, and a screw speed of 150r / min to obtain a modified waste plastic.

[0058] Example 2-13 The preparation method and parameter conditions are similar to those of Example 1, with the differences shown in Table 1.

[0059]

[0060] Comparative Example 1 The preparation method and parameter conditions are the same as those of Example 1, except that toluene diisocyanate is not added.

[0061] Comparative Example 2 The preparation method and parameter conditions are the same as those of Example 1, except that the chain transfer agent mercaptoethanol is not added.

[0062] Comparative Example 3 The preparation method and parameter conditions are the same as those of Example 1, except that the waste plastics are not subjected to modification treatment.

[0063] Example 14 Low temperature resistance and mechanical properties test

[0064] Determination of plastic brittle temperature: Performance test was carried out with a type A testing machine according to the measurement method in GB / T5470-2008. Plastic samples with a length of 20 mm, a width of 2.5 mm, and a thickness of 2 mm of the modified waste plastics prepared in Examples 1-13 and Comparative Examples 1-3 were used; ten samples were made for each group of test objects, and the punch was swung once at a test speed of 200 cm / s±20 cm / s to impact the samples. The temperature at which 5 of the samples were damaged was the brittle temperature. The test results are shown in Table 1.

[0065] A universal mechanical testing machine 3366 purchased from Instron, Germany, was used to test the bending strength of the modified waste plastics prepared in Examples 1-13 and Comparative Examples 1-3, with reference to the determination method of GB / T9341-2000 "Test method for bending properties of plastics", and the test speed was 5 mm / min; the notched impact strength was tested with reference to GB / T1843-2008, and the test was carried out at a temperature of 23°C and a humidity of 50%. The test results are shown in Table 2.

[0066]

[0067] Conclusion: From the results in Table 2, it can be seen that the low temperature resistance and mechanical strength of the waste plastics recycled in Comparative Examples 1-3 are significantly reduced. The waste plastics without the addition of isocyanate and chain transfer agent modification have a brittle temperature of -15°C and a notched impact strength of 12.1 KJ / m 2, poor impact strength, easy to break, and easy to crack under low temperature conditions, resulting in overall plastic fracture, affecting application; It can be seen from the results of Examples 1-5 that when different types of diisocyanates are added to the system, the low-temperature strength of the prepared modified waste plastics is significantly improved, while the bending strength is enhanced and the impact strength is increased. Due to the use of chain transfer agents and olefinic bonds in waste plastics for addition condensation to obtain exposed hydroxyl structures, isocyanates are used as chain extenders to extend the chain structure of waste plastics, and the long-chain structure effectively improves the low-temperature resistance of plastics. However, lysine diisocyanate has a branched ester structure that reduces the low-temperature resistance of the material, reduces the impact strength through the exposed ester group, and reduces the mechanical properties; Aromatic and alicyclic isocyanates can increase the rigid structure of the plastic system, increase impact resistance, and improve impact strength, but the introduction of the rigid structure increases the conjugated effect of the system, and the interaction of the conjugated groups forms entanglements. At the same time, the stability of the rigid structure reduces the bending performance of the plastic, increases the brittleness of the structure, and is easy to crack under low temperature conditions, reducing The use scope of the plastic is reduced; it can be seen from the results of Examples 3 and 6-7 that the use of different chain transfer agents has little effect on the low temperature resistance of the structure. Due to the difference in bond energy, the impact resistance of the material is affected. Since the bond energy of the carbon-sulfur bond is less than that of the carbon-oxygen bond and greater than that of the carbon-nitrogen bond, the impact resistance of the material increases with the increase of the bond energy; it can be seen from the results of Examples 8-13 that due to the reaction of the chain transfer agent with the olefin bond of the plastic, the plastic structure is finally extended by isocyanate to increase the overall performance of the plastic, so as to increase the amount of isocyanate and chain transfer agent, the low temperature resistance and mechanical properties of the material increase accordingly, but as the amount ratio of isocyanate and chain transfer agent increases, the excess isocyanate will be cross-linked in the plastic structure, reducing the impact strength of the plastic; at the same time, the excess chain transfer agent increases the exposed hydroxyl group, further reducing the low temperature resistance of the material; in summary, the brittle temperature of the waste plastic modified with 25 parts of hexamethylene diisocyanate and 25 parts of hydroxyethanol is -48°C, the bending strength is 53.6MPa, and the notched impact strength is 28.8KJ / m 2 , with significantly improved low temperature resistance. Embodiment 15

[0068] Preparation of modified waste plastics: Modified waste plastics were prepared by referring to the preparation method and parameter conditions of Example 6.

[0069] 100 parts of the PHBV and 50 parts of wood powder were placed in a vacuum drying oven and dried at 80 kPa and 100° C. for 12 hours to obtain a dry raw material; the dry raw material was added to a high-speed homogenizer and stirred at 400 r / min for 30 minutes, and sieved through 40 meshes to obtain a matrix.

[0070] 50 parts of the modified waste plastic and 150 parts of the matrix are added into a vacuum drying oven, and dried for 4 hours at 80 kPa and 100° C. to obtain a dried material; the dried material is added into a three-necked flask, an acetonitrile dissolving system is added, 2 parts of dibutyltin dilaurate are added, and the reaction is carried out in an oil bath at 80° C. for 2 hours, anhydrous n-heptane is precipitated, the solvent is filtered out, and the plastic matrix is ​​dried at 60° C. in a vacuum drying oven for 3 hours to obtain a plastic matrix; the plastic matrix is ​​added into a continuous mixer, and a plasticizer, an antioxidant 1010, and a flame retardant are added in sequence under stirring conditions, and stirred at 140° C. and 500 r / min, and mixed for 30 minutes to make it uniformly mixed to obtain a rubber compound; the rubber compound is melt-plasticized and granulated in a twin-screw extruder, with an inlet temperature of 150° C., a head temperature of 260° C., and a screw speed of 300 r / min to obtain plastic particles.

[0071] Examples 16-25 Refer to the preparation method and parameter conditions of Example 15, except as listed in Table 3.

[0072] Comparative Example 4 The preparation method and parameter conditions are the same as those of Example 15, except that no plasticizer is added.

[0073] Comparative Example 5 The preparation method and parameter conditions are the same as those of Example 15, except that no compatibilizer is added.

[0074] Example 26 Determination of Mechanical Properties of Plastic Granules

[0075] Using the MT-4000D1 computer tensile testing machine produced by Jiangsu Yangzhou Mingtuo Experimental Machinery Co., Ltd., the plastic particles obtained in Examples 15-25 and Comparative Examples 4-5 were placed in a clamp and clamped, and the clamp was moved at a rate of 500 mm / min to apply tension to the sample until the sample broke, and the test results were recorded. The results are shown in Table 3.

[0076]

[0077] Conclusion: From the results in Table 4, it can be seen that the mechanical properties of the plastic particles prepared without adding plasticizer and compatibilizer in Comparative Examples 4-5 are significantly lower than those in Examples 15-25. Without adding plasticizer, the tensile strength and elongation at break are significantly reduced, which are 15.2MPa and 92% respectively. From Comparative Examples 4-5, it can be seen that plasticizer and compatibilizer can synergistically improve the mechanical properties of plastic particles; from the results of Examples 16 and 23-25, it can be seen that different compatibilizers have obvious differences in improving tensile strength and elongation at break. The addition of nanoparticles can change the interfacial compatibility, but due to the particle size Due to the difference in size, nanoparticles are prone to agglomeration, thereby reducing the interfacial bonding force. The mechanical properties of plastic particles can effectively improve the tensile strength of the particles by using GMA and MAC, but compared with SEPS, the elongation at break is significantly different. Since the styrene chain segment has good compatibility with the plastic matrix, and the ethylene / propylene chain segment in the middle can produce elastic deformation, it can well transmit and disperse the external force when subjected to external force, and also absorb a certain amount of energy, thereby improving the elongation at break of the plastic. The results of Examples 15-18 show that the use of different types of plasticizers has little effect on the mechanical properties of plastic particles. Figure 1 The results show that the amount of plasticizer has a great influence on the transverse and longitudinal tensile strength of the material. This is because the compatibilizer improves the interface compatibility and the tensile strength of the plastic particles, but the long straight chain compatibilizer significantly improves the transverse tensile strength of the plastic. Due to the large relative molecular mass of the TOTM plasticizer and the large number of rigid groups in the molecular structure, as the amount of plasticizer increases, the plasticizer molecules improve the longitudinal tensile strength of the plastic particles, and excessive plasticizers will lead to uneven plasticization effects, resulting in significant differences in transverse and longitudinal tensile strengths; combined with the results of Example 16 and Examples 19-22, it can be seen that as the amount of plasticizer increases, the tensile strength of the plastic gradually increases and tends to remain unchanged, while the elongation at break shows a trend of first increasing and then decreasing as the amount of plasticizer increases. As the amount of plasticizer increases, the interface compatibility changes, the ability to transmit and disperse external forces provided is weakened, and the elongation at break decreases; Comprehensive Table 3, Figure 1 The results show that the plastic particles prepared using 40 parts of TOTM as a plasticizer and SEPS as a compatibilizer have a tensile strength of 29.4 MPa and an elongation at break of 235%, showing significantly improved mechanical properties.

[0078] Example 27: Plastic particles are prepared by referring to the preparation method and parameter conditions of Example 16.

[0079] 100 parts of the plastic particles were added into a three-necked flask, acetone was added for dispersion, 5 ml of acetic acid was used for dissolution, the mixture was stirred evenly at 100 r / min, and the mixture was heated in an oil bath at 60° C. 10 parts of silane coupling agent KH-570 were added, and the mixture was refluxed for 8 hours to obtain a reaction solution; the reaction solution was cooled to room temperature, separated and filtered, the solid was rinsed with acetone for 5 times, and dried in a vacuum drying oven at 80° C. for 2 hours to obtain silane-modified plastic particles.

[0080] Examples 28-39 Refer to the preparation method and parameter conditions of Example 27, the differences are listed in Table 4.

[0081] Comparative Example 6 The preparation method and parameter conditions are the same as those of Example 27, except that no silane modification is added.

[0082] Comparative Example 7 The preparation method and parameter conditions are the same as those of Example 27, except that silane modification is added before continuous mixing.

[0083] Example 40 Hydrophobicity Test

[0084] The silane-modified plastic particles obtained in Examples 28-39 and Comparative Examples 6-7 were tested for hydrophobicity;

[0085] Water contact angle test: 25°C, soak in 80 mL deionized water for 30 minutes with continuous stirring, filter the remaining plastic particles with filter paper, and dry them in a vacuum drying oven at 60°C until they reach a constant weight. The water contact angle of the plastic particles after water absorption treatment is tested using a contact angle tester (OC A50). The test results are shown in Table 4.

[0086]

[0087] Conclusion: From the results in Table 4, it can be seen that the water contact angle of the plastic particles in Comparative Example 6 without adding silane coupling agent modification treatment is 72.5°, showing obvious hydrophilicity. Due to the addition of wood powder, polar groups such as hydroxyl groups are introduced on the surface of the plastic particles. The presence of polar groups forms hydrogen bonds with water molecules under the action of water, further improving the hydrophilicity of the plastic. Since wood powder is easy to absorb moisture and expand under the action of water molecules, the plastic particles are locally subjected to stress cracking, further improving the overall performance of the plastic; Comparative Example 7 is silane-modified before continuous mixing, and the hydrophobicity can be increased by end-capping with hydroxyl groups. However, during mixing and melt extrusion granulation, Si-O bonds form hydrogen bonds with polar groups in the molecule, thereby cross-linking the hydrophobic silane groups inside the plastic particles, reducing the water contact angle and increasing the hydrophilicity; Comparative Example 27 and Examples 37-39 show that the use of different silane coupling agents has little effect on the water contact angle of the plastic particles. Since the KH-560 molecule contains epoxy groups, it needs to absorb during the reaction. Energy is used for ring-opening reaction, and silane coupling reaction is carried out. Therefore, under the same conditions, the silane grafting rate is low, the water contact angle is reduced, and the hydrophobicity is poor. Comparing the results of Example 27 and Examples 34-36, it can be seen that with the increase of the amount of silane coupling agent, the water contact angle gradually increases and tends to be constant. Since the exposed hydroxyl groups of the plastic particles are limited, the silane modification reaches a certain yield, and the system no longer reacts when the amount of silane coupling agent is increased, so the water contact angle tends to be constant; Examples 27-33 are obtained by adjusting the reaction temperature and the reaction The optimal reaction conditions were screened out according to the change of reaction time. When the reaction temperature was low, less silane coupling agent participated in the reaction, the reaction yield was low, and the hydrophobicity of the obtained plastic particles was poor. When the reaction temperature was too high, the boiling point of acetic acid was reached, the solvent evaporated, the acidity in the system decreased, the reaction yield decreased, and the water contact angle also decreased. From the results in Table 4, it can be seen that the water contact angle of the plastic particles obtained by using 10 parts of KH-570 as a silane coupling agent and maintaining the reaction at 90°C for 6h was 108.6°, showing obvious hydrophobicity.

[0088] Example 41 The preparation method and parameter conditions are the same as those of Example 27, except that antimony trioxide and decabromodiphenylethane supported by expanded vermiculite are used as plasticizers.

[0089] Preparation method of antimony trioxide and decabromodiphenylethane loaded with expanded vermiculite:

[0090] 10 parts of antimony trioxide and 10 parts of decabromodiphenylethane were added into a beaker, and toluene was added and stirred to dissolve to obtain a dissolving system. 10 parts of expanded vermiculite were immersed into the dissolving system, and stirred at 200 r / min for 2 hours. The solid was separated by centrifugation, and the solid was vacuum dried at 100° C. for 1 hour to obtain the expanded vermiculite-loaded flame retardant.

[0091] Examples 42-52 Refer to the preparation method and parameter conditions of Example 41, the differences are listed in Table 5.

[0092] Comparative Example 8 The preparation method and parameter conditions are the same as those of Example 41, except that no flame retardant is added.

[0093] Example 53 Flame retardant performance measurement

[0094] The plastic particles prepared in Examples 41-52 and Comparative Example 8 were used to prepare rectangular samples of 40×20×1.5 mm, and the limiting oxygen index of the samples was tested by a CZF-3 horizontal vertical combustion instrument (purchased from Nanjing Jiangning District Analytical Instrument Factory) in accordance with GB / T 2406.2-2009. The test results are shown in Table 5.

[0095]

[0096] Conclusion: From the results in Table 5, it can be seen that by changing the dosage of the flame retardant component, the plastic particles show a significantly changed limiting oxygen index. From the results of Comparative Example 8, it can be seen that the addition of flame retardants can significantly improve the limiting oxygen index of plastic particles and increase the flame retardant properties of plastic particles. From the results of Examples 41-45, it can be seen that the use of halogen antimony system antimony trioxide and decabromodiphenylethane as the flame retardant system has no obvious flame retardant effect due to the limitation of dosage. Since the intumescent flame retardant will expand rapidly during the flame retardant process, it will prevent the spread of fire and increase the flame retardant properties. After the system expands, it will cause the plastic material to become brittle, the intramolecular stress will increase, the impact strength of the plastic will decrease, and the mechanical properties will decrease, affecting the use. Using an inorganic material with a high specific surface area as a load can synergize with the halogen antimony system to increase the flame retardant properties of the plastic. From Examples 50-5 2 The results show that due to the large amount of porous inorganic material added, the interfacial compatibility of the plastic is reduced, the inorganic molecules are unevenly distributed in the system, and are easily affected by external stress, the impact strength of the plastic is reduced, and the mechanical properties of the plastic particles are reduced; although organic halides can improve the flame retardancy while maintaining mechanical properties, they are less environmentally friendly, and excessive use does not make use of the recycling of plastics; through the results of Examples 46-49, it can be seen that with the increase in the amount of flame retardant, the limiting oxygen index gradually increases, the flame retardant performance is improved, but the impact resistance of the plastic gradually increases and then gradually decreases. Due to the inevitable increase of excessive inorganic flame retardant materials, the mechanical properties of the plastic are reduced; Comprehensive Table 5 The results show that the plastic particles prepared using 15 parts of porous boron nitride-loaded antimony trioxide and decabromodiphenylethane have an impact strength of 26.8KJ / m 2 The limiting oxygen index is 34, and it has good flame retardancy while maintaining mechanical properties.

[0097] Examples 54-63 Refer to the preparation method and parameter conditions of Example 27, the differences are listed in Table 6.

[0098] Comparative Example 9 The preparation method and parameter conditions are the same as those of Example 27, except that no wood powder is added to modify the matrix.

[0099] Comparative Example 10 The preparation method and parameter conditions of Example 27 were referred to, except that no matrix was added.

[0100] Example 64 Degradation Performance Test

[0101] Biodegradability test: Using the soil test method, 10 mg of the plastic particles prepared in Examples 54-63 and Comparative Examples 9-10 were taken in a rectangular shape of 40×20×1.5 mm and buried in the soil at a depth greater than 8 cm. The weather and rainfall changes were recorded for 30 days, with an average temperature of 26°C. The mass changes were recorded at 30 days, 60 days, and 90 days. The degradation rate was obtained by comparing the mass reduction with the mass of the original plastic particles. The results are shown in Table 6.

[0102]

[0103] Conclusion: From the results in Table 6, it can be seen that the addition of wood powder modified matrix and the modified waste plastic mixed can significantly improve the degradation ability of the obtained plastic particles. Compared with the comparative example 9, the 90d degradation ability reached more than 50%, showing a significantly improved biodegradability; the comparative example 10 did not add the matrix and the modified waste plastic grafting effect, and the obtained plastic particles had low degradation ability, because the main materials in the waste plastics were polypropylene and polyethylene plastics, and the biodegradability was poor; Examples 54-57 selected polymers of different materials as the synthetic plastic matrix for grafting with wood powder. Since polylactic acid is easily degraded only at high temperatures in soil or compost, and pure polyethylene cannot be biodegraded, PHA is biodegraded through a surface erosion mechanism. When the critical thickness is reached, the overall degradation begins, and the biodegradation rate is slow. Biodegradation requires a sufficiently wide porous passage to enter the internal site, and the environmental moisture is absorbed by the wood and will be in the wood. -The polymer interface produces a local humid environment, which promotes phenomena similar to cracking and local environmental stress cracking, and eventually loosens the interface. After PHBV and wood powder are compounded, the pores and cracks produced by biodegradation allow more water molecules to enter the composite sample, forming a network of interconnected pores and cracks during the biodegradation process, which is the main way for bacteria and fungal hyphae to enter the matrix, showing a significantly improved biodegradation rate; from the results of comparative examples 58-63, it can be seen that with the increase in the amount of wood powder, the biodegradability of the plastic particles slowly increases, but the excessive addition of wood powder introduces a large number of polar groups, which increases the hydrophilicity of the plastic and also reduces the internal stress of the material, affecting the mechanical properties of the plastic particles; from the results of Table 6, it can be seen that using 150 parts of PHBV / wood powder as the matrix, the 90-day biodegradation rate of the prepared plastic particles is 58.4%, showing a significantly improved biodegradability and reducing environmental pollution.

[0104] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for preparing plastic particles modified from waste plastics, characterized in that: The method for preparing the plastic particles comprises the following steps: S1 pre-treats waste plastics, heats, extrudes, and cools to obtain recycled plastics; adds 5-50 parts of a chain transfer agent and 2 parts of azobisisobutyronitrile to 100 parts of the recycled plastics, reacts at 110°C for 4 hours, and rotary evaporates to obtain a reaction system; dissolves the reaction system in toluene, adds 10-40 parts of isocyanate and 2 parts of dibutyltin dilaurate, and reacts at 80°C for 2 hours to obtain modified plastics; adds the modified plastics to a continuous mixer, adds a compatibilizer under stirring conditions, and mixes at 110°C for 30 minutes to obtain plastic glue; melts and plasticizes the plastic glue in a twin-screw extruder to obtain modified waste plastics; S2: drying the polymer and 20-80 parts of wood powder for 12 hours, stirring at 400 r / min for 30 minutes, and sieving to obtain a matrix; S3: drying 50 parts of the modified waste plastic and 100-200 parts of the matrix at 100°C for 4 hours to obtain a dried material; adding the dried material into a flask, dissolving it in acetonitrile, adding 2 parts of dibutyltin dilaurate, reacting at 80°C for 2 hours, separating and centrifuging, and drying at 60°C for 3 hours to obtain a plastic matrix; adding the plastic matrix into a continuous mixer, adding 20-50 parts of a plasticizer, 10 parts of an antioxidant 1010, and 5-25 parts of a flame retardant under stirring conditions, and mixing at 140°C and 500r / min for 30 minutes to obtain a rubber compound; melt-plasticizing and granulating the rubber compound in a twin-screw extruder to obtain modified plastic particles; S4: adding 100 parts of the modified plastic particles into a flask, dissolving them in acetone and acetic acid, heating to 60-100° C., adding 5-20 parts of a silane coupling agent, and refluxing at 100 r / min for 4-8 hours to obtain a reaction solution; cooling the reaction solution, separating and rinsing it, and drying it at 80° C. for 2 hours to obtain plastic particles; The isocyanate is selected from the group consisting of toluene diisocyanate, lysine diisocyanate, isophorone diisocyanate, terephthalylidene diisocyanate, and hexamethylene diisocyanate; The chain transfer agent is selected from one of mercaptoethanol, hydroxyethanol and aminoethanol; the amount of the chain transfer agent is 10-40 parts; The polymer is selected from one of polylactic acid, polyethylene, polyhydroxybutyl pentyl ester, and polyhydroxyalkanoate; the amount of the polymer is 100 parts.

2. The method for preparing plastic particles modified from waste plastics according to claim 1, characterized in that: The compatibilizer is selected from one of styrene-(ethylene-propylene)-styrene copolymer, ethylene-glycidyl methacrylate, maleic anhydride functionalized ethylene copolymer, and nano silicon dioxide; the amount of the compatibilizer is 10 parts.

3. The method for preparing plastic particles modified from waste plastics according to claim 1, characterized in that: The silane coupling agent is selected from one of 3-aminopropyltriethoxysilane, 3-(2,3-epoxypropyloxy)propyltrimethoxysilane, methacryloxypropyltriethoxysilane and N-(2-aminoethyl)-3-aminopropyltrimethoxysilane.

4. The method for preparing plastic particles modified from waste plastics according to claim 1, characterized in that: The flame retardant is selected from one or a mixture of expanded vermiculite, organic bentonite, porous boron nitride, antimony trioxide, and decabromodiphenylethane.

5. The method for preparing plastic particles modified from waste plastics according to claim 1, characterized in that: The flame retardant is selected from intumescent flame retardants.

6. The method for preparing plastic particles modified from waste plastics according to claim 1, characterized in that: The plasticizer is selected from one of trioctyl trimellitate, dioctyl adipate, diisononyl phthalate and di(2-ethylhexyl) phthalate.

7. A plastic particle modified from waste plastics, characterized in that: The plastic particles include a plastic matrix prepared from modified waste plastics and a matrix, a plasticizer, an antioxidant 1010, a flame retardant, and a silane coupling agent; the plastic particles are prepared by the preparation method described in any one of claims 1 to 6; the brittle temperature of the modified waste plastics in the plastic particles is -48°C, the bending strength is 53.6MPa, and the notched impact strength is 28.8KJ / m 2 The tensile strength of the plastic particles is 29.4MPa, and the elongation at break is 235%; the water contact angle of the plastic particles is 108.6°; the impact strength of the plastic particles is 26.8KJ / m 2 , the limiting oxygen index is 34; the 90-day biodegradation rate of the plastic particles is 58.4%.