A kind of negative electrode lead paste of ultra-low temperature lead-acid battery and preparation method thereof

By adding barium sulfate, sodium ligninsulfonate, hydrolyzed tannin, nanographene and nanographyne to the lead-acid battery negative electrode lead paste, combined with the synergistic effect of lead stannate, the low-temperature performance improvement in the existing technology is solved. The demand for lead-acid batteries has achieved high-efficiency low-temperature performance and cycle life improvement.

CN118472263BActive Publication Date: 2024-11-01TIANNENG BATTERY GROUP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410924170.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-11
Publication Date
2024-11-01
Estimated Expiration
2044-07-11

AI Technical Summary

Technical Problem

Although there are a variety of negative electrode additives in the prior art that can improve the low-temperature performance of lead-acid batteries, new additives are still needed to find to further improve the low-temperature performance.

Method used

Using additives including barium sulfate, sodium lignin sulfonate, hydrolyzed tannin, nanographene, nanographyne and lead nanostanate, ultra-low temperature lead battery negative electrode lead paste is prepared through grinding and dry mixing, and using nanographyne Synergistic effects with lead nanostanate improve electrochemical properties.

Benefits of technology

It significantly improves the room temperature capacity, low-temperature high-current discharge capacity and cycle life of lead-acid batteries, and improves the low-temperature performance and electrochemical reaction speed.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention discloses a negative lead paste for an ultra-low temperature lead-acid battery and a preparation method thereof. The negative lead paste for an ultra-low temperature lead-acid battery comprises lead powder, dilute sulfuric acid, water and an additive. Based on 1000 parts of the lead powder, the additive component comprises: 8 to 10 parts of barium sulfate, 2.5 to 4 parts of sodium lignin sulfonate, 3 to 5 parts of hydrolyzed tannin, 1 to 2 parts of nano-graphene, 1.5 to 3 parts of nano-graphene, 1 to 2 parts of nano-lead stannate, and 0.8 to 1.2 parts of polyester staple fibers. In the present application, nano-lead stannate and nano-graphene are pretreated before use, and are physically interlocked and uniformly mixed, which can solve the agglomeration problem of lead stannate, make the lead stannate uniformly mixed, and play a better role.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of lead-acid batteries, and in particular relates to an ultra-low temperature lead-acid battery negative electrode lead paste and a preparation method thereof. Background Art

[0002] The low temperature capacity of lead-acid batteries is a key performance indicator. The low temperature performance of lead-acid batteries mainly depends on the negative plate. Under low temperature conditions, the main failure mode of the negative plate is passivation and shrinkage. Adding appropriate additives to the negative active material is one of the main solutions.

[0003] Commonly used negative electrode additives such as sodium lignin sulfonate are a type of anionic surfactant that is easily adsorbed on the negative electrode sponge metal lead with a large surface area. When sodium lignin sulfonate is adsorbed on the negative electrode sponge metal lead, the negative electrode surface energy can be reduced, thereby inhibiting the surface shrinkage of the negative electrode active material during the charge and discharge cycle, maintaining the porosity and high dispersion of the negative electrode sponge metal lead, and improving the electrochemical performance of the negative electrode. Especially during high-rate discharge and low-temperature discharge, it delays the passivation of the negative electrode.

[0004] For example, the invention application with publication number CN108598472A discloses a low-temperature resistant lead-acid battery negative electrode lead paste and a preparation method thereof, wherein the negative electrode lead paste is composed of lead powder, negative electrode additive, water and synthetic paste acid, and the negative electrode additive comprises 0.5-1.0 parts of strontium sulfate or barium sulfate, 0.1-0.15 parts of sodium lignin sulfonate, 0.4-0.8 parts of humic acid, 0.3-0.6 parts of calcite extract, 0.6-1.2 parts of synthetic mixing agent, 0.1-0.2 parts of carbon nanotubes, 0.05-0.1 parts of nano Ketjen black, 0.1-0.15 parts of conductive carbon fiber, and 0.1-0.5 parts of sodium hydroxymethyl cellulose, based on 100 parts by weight of lead powder. The low-temperature discharge capacity of the battery produced by the negative electrode lead paste of the present invention can be increased by 10%-25%, and the service life in a low-temperature environment can be increased by 20%-30%.

[0005] For another example, the invention application with publication number CN112786843A discloses a negative lead paste and negative plate for a lead-acid battery for low temperature, wherein the negative lead paste is composed of lead powder, additives, water and hydrated acid, and the additives are composed of 0.5-1.0 parts of PE short fibers, 0.5-1.0 parts of sodium carboxymethyl cellulose, 3.0-5.0 parts of modified magnesium trisilicate, 4.0-6.0 parts of sodium stearate, 2.0-3.0 parts of Teflon solution, 0.5-1.5 parts of stannous sulfate, 1.0-2.0 parts of superconducting carbon black, 8-12 parts of ultrafine barium sulfate, 2.5-4.0 parts of lignin, and 1-2 parts of humic acid. The present invention can greatly improve the low temperature performance of the lead-acid battery by adding special additives to the negative lead paste.

[0006] Although many negative electrode additives that can improve the low-temperature performance of lead-acid batteries have been disclosed in the prior art, it is still of great significance to find new negative electrode additives that can improve the low-temperature performance. Summary of the invention

[0007] In view of the above-mentioned deficiencies in the prior art, the present invention provides a negative electrode lead paste for an ultra-low temperature lead-acid battery and a preparation method thereof.

[0008] The invention firstly provides an additive for negative electrode lead paste of an ultra-low temperature lead-acid battery, which comprises, by weight, 8-10 parts of barium sulfate, 2.5-4 parts of sodium lignin sulfonate, 3-5 parts of hydrolyzed tannin, 1-2 parts of nano-graphene, 1.5-3 parts of nano-graphene, 1-2 parts of nano-lead stannate and 0.8-1.2 parts of polyester staple fibers.

[0009] Preferably, the fiber length of the polyester staple fiber is 3 to 3.5 mm.

[0010] The present invention further provides an ultra-low temperature lead-acid battery negative electrode lead paste, comprising lead powder, dilute sulfuric acid, water and additives. Based on 1000 parts of the lead powder, the additive components comprise: 8-10 parts of barium sulfate, 2.5-4 parts of sodium lignin sulfonate, 3-5 parts of hydrolyzed tannin, 1-2 parts of nano-graphene, 1.5-3 parts of nano-graphene, 1-2 parts of nano-lead stannate and 0.8-1.2 parts of polyester staple fibers.

[0011] Preferably, based on 1000 parts of lead powder, the amount of dilute sulfuric acid is 70-90 parts, and the amount of water is 100-125 parts. The density of the dilute sulfuric acid is 1.3-1.5 g / cm 3 More preferably, the density of the dilute sulfuric acid is 1.4 g / cm 3 .

[0012] Preferably, the oxidation degree of the lead powder is 73% to 80%. In the present application, the oxidation degree of the lead powder can be the oxidation degree conventionally used in the prior art.

[0013] Preferably, the fiber length of the polyester staple fiber is 3 to 3.5 mm.

[0014] The present invention further provides a method for preparing the negative electrode lead paste of the ultra-low temperature lead-acid battery, comprising the following steps:

[0015] (1) mixing and grinding the formulated amounts of nano-graphene, nano-graphene and nano-lead stannate to obtain a uniform mixture;

[0016] (2) Put the formulated amount of lead powder, barium sulfate, sodium lignin sulfonate, hydrolyzed tannin, polyester staple fiber and the mixture obtained in step (1) into a paste mixer for dry mixing, then first pour water, add the formulated amount of water and stir, then pour acid, add the formulated amount of dilute sulfuric acid and stir, and after mixing, obtain the negative electrode lead paste of the ultra-low temperature lead-acid battery.

[0017] Preferably, the mixing and grinding in step (1) uses a grinder, and the mixing and grinding time is 20 to 30 minutes.

[0018] The present invention also provides an ultra-low temperature lead-acid battery, comprising a negative electrode plate, wherein the negative electrode plate comprises a negative electrode lead paste, and the negative electrode lead paste uses the ultra-low temperature lead-acid battery negative electrode lead paste.

[0019] Hydrolyzed tannins are esters of gallic acid, or phenolic acid derived from gallic acid, and polyols, and polyols and phenolic acid produced under the action of acids, bases or enzymes. According to the different polyphenolic acid produced by the hydrolysis reaction, most hydrolyzed tannins can be further divided into gallotannins and ellagitannins. In the present application, ellagitannins are preferably used.

[0020] Sodium lignin sulfonate and tannin are both excellent negative electrode expanders for lead-acid batteries, and have the advantage of good low-temperature performance. Sodium lignin sulfonate is an internationally used low-temperature expander. The tannins and tannin extracts used in traditional domestic ultra-low temperature formulas all utilize the tannin components in these two substances to promote low-temperature and high-current discharge of batteries. However, due to the influence of early scientific and technological levels, the purification of tannin components is a big problem. Therefore, the use of tannin compounds as low-temperature expanders will be better than using tannin extracts and tannins.

[0021] Graphdiyne is a new all-carbon nanostructured material after fullerene, carbon nanotubes and graphene. It has abundant carbon chemical bonds, large conjugated system, wide interplanar spacing and excellent chemical stability. The uniform pore structure, excellent electronic conductivity and chemical stability of Graphdiyne give Graphdiyne high capacity, excellent rate performance and excellent electrochemical properties in terms of cycle life. The main function of nanographdiyne in the present invention is conductivity.

[0022] Lead stannate is a new type of functional material. It not only has excellent ferroelectric and dielectric properties, but also has small particle size, large specific surface area, and many surface atoms. The surface atoms have unsaturated properties due to incomplete coordination. There are many lattice defects in the nanocrystals, which become highly active reaction centers, making it have excellent properties that conventional materials cannot match in catalysis and adsorption. Lead stannate has good adsorption and catalysis, which can promote chemical reactions, increase the speed of charge and discharge electrochemical reactions, increase the electrochemical reaction speed of batteries at low temperatures, and improve the charge and discharge capacity of batteries at low temperatures.

[0023] In the present application, nano-graphene and nano-lead stannate are simultaneously added to the negative electrode lead paste, and the use of the two in the battery and their synergistic effect improve the low-temperature charging and discharging capacity of the battery.

[0024] In the present application, nano-lead stannate and nano-graphene are pretreated before use and physically interlocked and uniformly mixed, which can solve the agglomeration problem of lead stannate and make the lead stannate uniformly mixed to better play its role. DETAILED DESCRIPTION

[0025] Example 1

[0026] In the following preparation methods, each substance is added by weight.

[0027] (1) Premixing of new substances

[0028] 2 parts of nano-graphene, 3 parts of nano-graphene, and 2 parts of nano-lead stannate were put into a grinder, and the grinder was turned on for 30 minutes to obtain a uniformly ground nano-uniform mixture A.

[0029] (2) Ointment

[0030] Put 1000 parts of lead powder (oxidation degree is 78%), 10 parts of barium sulfate, 4 parts of sodium lignin sulfonate, 5 parts of hydrolyzed tannin (ellagic tannin), 0.8 parts of polyester staple fiber and mixture A into a lead powder machine, dry stir for 3 minutes, then pour in 125 parts of pure water for 5 minutes, stir for 3 minutes after pouring, then pour in 90 parts of dilute sulfuric acid for 10 minutes, and continue stirring for 15 minutes after pouring.

[0031] Example 2

[0032] In the following preparation methods, each substance is added by weight.

[0033] (1) Premixing of new substances

[0034] 1 part of nano-graphene, 1.5 parts of nano-graphene, and 1 part of nano-lead stannate were put into a grinder, and the grinder was turned on for 20 minutes to obtain a uniformly ground nano-uniform mixture A.

[0035] (2) Ointment

[0036] Put 1000 parts of lead powder (oxidation degree is 78%), 8 parts of barium sulfate, 2.5 parts of sodium lignin sulfonate, 3 parts of hydrolyzed tannin (ellagic tannin), 1 part of polyester staple fiber and mixture A into a lead powder machine, dry stir for 3 minutes, then pour in 100 parts of pure water for 5 minutes, stir for 3 minutes after pouring, then pour in 70 parts of dilute sulfuric acid for 10 minutes, and continue stirring for 10 minutes after pouring.

[0037] Example 3

[0038] In the following preparation methods, each substance is added by weight.

[0039] (1) Premixing of new substances

[0040] 1.5 parts of nano-graphene, 2 parts of nano-graphene, and 1.5 parts of nano-lead stannate were put into a grinder, and the grinder was turned on for 25 minutes to obtain a uniformly ground nano-uniform mixture A.

[0041] (2) Ointment

[0042] Put 1000 parts of lead powder (oxidation degree is 78%), 9 parts of barium sulfate, 3 parts of sodium lignin sulfonate, 4 parts of hydrolyzed tannin (ellagic tannin), 1.2 parts of polyester staple fiber and mixture A into a lead powder machine, dry stir for 3 minutes, then pour in 110 parts of pure water for 5 minutes, stir for 3 minutes after pouring, then pour in 80 parts of dilute sulfuric acid for 10 minutes, and continue stirring for 15 minutes after pouring.

[0043] Comparative Example 1

[0044] In the following preparation methods, each substance is added by weight.

[0045] (1) Premixing of new substances

[0046] 1.5 parts of nano-graphene and 2 parts of nano-graphene were put into a grinder, and the grinder was turned on for 25 minutes to obtain a uniform nano-mixture A.

[0047] (2) Ointment

[0048] Put 1000 parts of lead powder (oxidation degree is 78%), 9 parts of barium sulfate, 3 parts of sodium lignin sulfonate, 4 parts of hydrolyzed tannin (ellagic tannin), 1.2 parts of polyester staple fiber and mixture A into a lead powder machine, dry stir for 3 minutes, then pour in 110 parts of pure water for 5 minutes, stir for 3 minutes after pouring, then pour in 80 parts of dilute sulfuric acid for 10 minutes, and continue stirring for 15 minutes after pouring.

[0049] Comparative Example 2

[0050] In the following preparation methods, each substance is added by weight.

[0051] (1) Premixing of new substances

[0052] 1.5 parts of nano-graphene and 1.5 parts of nano-lead stannate were put into a grinder, and the grinder was turned on for 25 minutes to obtain a uniformly ground nano-mixture A.

[0053] (2) Ointment

[0054] Put 1000 parts of lead powder (oxidation degree is 78%), 9 parts of barium sulfate, 3 parts of sodium lignin sulfonate, 4 parts of hydrolyzed tannin (ellagic tannin), 1.2 parts of polyester staple fiber and mixture A into a lead powder machine, dry stir for 3 minutes, then pour in 110 parts of pure water for 5 minutes, stir for 3 minutes after pouring, then pour in 80 parts of dilute sulfuric acid for 10 minutes, and continue stirring for 15 minutes after pouring.

[0055] Comparative Example 3

[0056] In the following preparation methods, each substance is added by weight.

[0057] Put 1000 parts of lead powder (oxidation degree is 78%), 9 parts of barium sulfate, 3 parts of sodium lignin sulfonate, 4 parts of hydrolyzed tannin (ellagic tannin), 1.2 parts of polyester staple fiber and 1.5 parts of nano-graphene into a lead powder machine, dry stir for 3 minutes, then pour in 110 parts of pure water for 5 minutes, stir for 3 minutes after pouring, then pour in 80 parts of dilute sulfuric acid for 10 minutes, and continue stirring for 15 minutes after pouring.

[0058] Test Example 1

[0059] A negative electrode plate prepared with the negative electrode lead paste in each embodiment and comparative example was used to equip a 6-DZF-20 battery for testing.

[0060] (1) 2h rate discharge (normal temperature capacity): According to Article 5.5 of the national battery standard GB / T22199-2017, after the battery is fully charged, it should be kept at a temperature of 25±2℃ for 1~24h, and discharged at a constant current of 10A until the battery voltage reaches 10.5V. The 2h rate capacity Ca should reach the C2 standard within three cycles.

[0061] (2) Low-temperature, high-current discharge: According to Article 5.9 of the national battery standard GB / T22199-2017, the battery was placed in a -18°C low-temperature box for 12 hours, and then discharged at a current of 10A in a -18°C environment. The discharge was terminated when the battery voltage reached 10.5V, and the average discharge time was recorded.

[0062] (3) Cycle life: In accordance with Article 5.12 of the national battery standard GB / T22199-2017, in an environment with a temperature of 25±5℃, discharge at a current of 10A for 1.6h, and then charge at a constant voltage of 16V (current limit 4A) for 6.4h as one cycle. When the terminal voltage of the battery is lower than 10.5V for three consecutive times after discharging for 1.6h, the battery cycle life is terminated. The total cycle life is not less than 350 times.

[0063] The test results are shown in Table 1 below.

[0064] Table 1

[0065]

[0066] From the results in Table 1, it can be seen that the use of lead stannate and the additive graphyne of the present invention can promote the room temperature capacity to increase by about 8%, the low temperature and large current discharge to increase by about 10%, and the cycle life to increase by about 8%, and the effect is significant.

Claims

1. An additive for negative electrode lead paste of ultra-low temperature lead-acid battery, It is characterized in that Calculated by weight, it includes: 8-10 parts of barium sulfate, 2.5-4 parts of sodium lignin sulfonate, 3-5 parts of hydrolyzed tannin, 1-2 parts of nano-graphene, 1.5-3 parts of nano-graphene, 1-2 parts of nano-lead stannate, and 0.8-1.2 parts of polyester staple fibers.

2. The additive according to claim 1, It is characterized in that The fiber length of the polyester staple fiber is 3 to 3.5 mm.

3. A method for preparing negative electrode lead paste for ultra-low temperature lead-acid battery, It is characterized in that The raw materials for preparing the negative electrode lead paste of the ultra-low temperature lead-acid battery include lead powder, dilute sulfuric acid, water and additives. Based on 1000 parts of the lead powder, the additive components include: 8-10 parts of barium sulfate, 2.5-4 parts of sodium lignin sulfonate, 3-5 parts of hydrolyzed tannin, 1-2 parts of nano-graphene, 1.5-3 parts of nano-graphene, 1-2 parts of nano-lead stannate, and 0.8-1.2 parts of polyester staple fibers. The preparation method comprises the following steps: (1) mixing and grinding the formulated amounts of nano-graphene, nano-graphene and nano-lead stannate to obtain a uniform mixture; (2) Put the formulated amount of lead powder, barium sulfate, sodium lignin sulfonate, hydrolyzed tannin, polyester staple fiber and the mixture obtained in step (1) into a paste mixer for dry mixing, then first pour water, add the formulated amount of water and stir, then pour acid, add the formulated amount of dilute sulfuric acid and stir, and after mixing, obtain the negative electrode lead paste of the ultra-low temperature lead-acid battery.

4. The preparation method according to claim 3, It is characterized in that Based on 1000 parts of lead powder, there are 70-90 parts of dilute sulfuric acid and 100-125 parts of water. The density of the dilute sulfuric acid is 1.3-1.5 g / cm 3 .

5. The preparation method according to claim 3, It is characterized in that The oxidation degree of the lead powder is 73% to 80%.

6. The preparation method according to claim 3, It is characterized in that The fiber length of the polyester staple fiber is 3 to 3.5 mm.

7. The preparation method according to claim 3, It is characterized in that The mixing and grinding in step (1) is performed using a grinder, and the mixing and grinding time is 20 to 30 minutes.

8. An ultra-low temperature lead-acid battery, It is characterized in that The invention comprises a negative electrode plate, wherein the negative electrode plate comprises a negative electrode lead paste, and the negative electrode lead paste is prepared by the preparation method according to any one of claims 3 to 7.