A Lanthanum-Modified Metal-Organic Framework Magnetic Nanomaterial for Phosphorus Removal, Its Preparation Method and Application

By preparing lanthanum-modified metal-organic framework magnetic nanomaterials for phosphorus removal by combining La-Fe3O4 nanoparticles with ZIF-67, the problem of removing organic and inorganic phosphorus from water was solved, achieving efficient adsorption and catalytic degradation, and easy separation and recycling.

CN118477626BActive Publication Date: 2026-11-17CHINA CONSTR EIGHTH BUREAU SOUTH CHINA CONSTR CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410618777.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-17
Publication Date
2026-11-17
Estimated Expiration
2044-05-17

AI Technical Summary

Technical Problem

Existing technologies are insufficient for efficiently removing organic and inorganic phosphorus from water, and MOF materials are difficult to separate into solid and liquid phases for recycling and reuse in water.

Method used

By combining La-Fe3O4 nanoparticles with ZIF-67 metal-organic framework material, lanthanum-modified metal-organic framework magnetic nanomaterials for phosphorus removal were prepared through magnetic modification. Combining the chelating properties of La and the catalytic activity of ZIF-67, the adsorption of inorganic phosphorus and the catalytic degradation of organic phosphorus were achieved.

Benefits of technology

The efficient adsorption and catalytic degradation of lanthanum-modified metal-organic framework magnetic nanomaterials for phosphorus removal have been achieved. These materials can be easily separated under an external magnetic field, avoiding secondary pollution, and can be widely used to remove various forms of phosphorus from sewage and river and lake sediments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004846070880000081
    Figure BDA0004846070880000081
  • Figure HDA0004846070890000011
    Figure HDA0004846070890000011
  • Figure HDA0004846070890000012
    Figure HDA0004846070890000012
Patent Text Reader

Abstract

This invention provides a lanthanum-modified metal-organic framework magnetic nanomaterial for phosphorus removal, its preparation method, and its application. The invention combines La-Fe3O4 nanoparticles with ZIF-67 metal-organic framework material to obtain a lanthanum-modified metal-organic framework magnetic nanomaterial for phosphorus removal. This material can efficiently adsorb inorganic phosphorus in water and catalytically degrade diazine phosphorus in water. Simultaneously, it can adsorb phosphate ions generated during the reaction in situ, thus avoiding secondary pollution and exhibiting good phosphorus removal performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a nano-phosphorus removal material, and more particularly to a lanthanum-modified metal-organic framework magnetic nano-phosphorus removal material and its preparation method. Background Technology

[0002] Eutrophication is a prevalent environmental problem, with phosphorus (P) being one of the main contributing factors. For the removal of phosphorus species from water, relatively mature methods exist for inorganic phosphates, especially orthophosphates, such as chemical precipitation and adsorption separation. However, organophosphates, particularly organophosphate pesticides, generally have low concentrations in the aquatic matrix, resulting in poor removal efficiency. To address this, a two-step approach is a feasible strategy for deep phosphorus removal: first, converting organophosphates into orthophosphates, followed by precipitation or adsorption. This can typically be achieved through advanced oxidation processes (AOPs), such as heterogeneous catalysts activating oxidants to rapidly degrade organophosphate pesticides into phosphates. Furthermore, considering the strong ability of phosphates to provide isolated electron pairs, metal-based materials can serve as potential phosphate adsorbents. The mechanism of phosphate removal by metal-based materials usually involves the formation of inner-sphere complexes, which provide a stronger driving force for selective phosphate removal. Commonly used metal-based materials can be divided into metal oxides / hydroxides, mixed metal oxides / hydroxides, and metal-support composite materials. Among them, lanthanum (La) and zirconium (Zr) are currently popular metals for developing efficient phosphorus removal adsorption materials.

[0003] Currently, metal-organic frameworks (MOFs) have been widely used and researched in adsorption, separation, catalysis, and sensing due to their excellent properties. For example, ZIF-67, a representative Co-based MOF material, is commonly used to activate potassium permonosulfate (PMS) to oxidize and degrade organic pollutants in water. However, in practical applications, MOFs, due to their powder crystalline structure, are difficult to separate and recycle in solid-liquid processes. Therefore, magnetic modification of MOFs to impart magnetic properties to MOF composites, making them easier to separate from water under an applied magnetic field, has great application potential. Summary of the Invention

[0004] The technical problem to be solved by the present invention is to provide a method for preparing lanthanum-modified metal-organic framework magnetic nanomaterials for phosphorus removal. The lanthanum-modified metal-organic framework magnetic nanomaterials for phosphorus removal prepared by this method can not only efficiently adsorb inorganic phosphorus in water, but also catalytically degrade diazine phosphorus in water. At the same time, it can adsorb phosphate ions generated by the reaction in situ, thereby avoiding secondary pollution and having a good phosphorus removal effect.

[0005] To solve the above-mentioned technical problems, the technical solution of the present invention is as follows:

[0006] A method for preparing a lanthanum-modified metal-organic framework magnetic nanomaterial for phosphorus removal includes the following steps:

[0007] S1. Add FeCl3·6H2O and LaCl3·nH2O to ethylene glycol and stir for 30 min to obtain a precursor solution;

[0008] S2. Add anhydrous sodium acetate and polyethylene glycol to the precursor solution obtained in step S1 to obtain a mixed solution. Seal the mixed solution in an autoclave, then place the autoclave in an oven and react at 150-250℃ for 8-12 hours. Allow it to cool naturally to room temperature to obtain reactant one.

[0009] S3. After magnetic separation, the reactants obtained in step S2 are washed five times with anhydrous ethanol and deionized water, respectively, and then placed in a vacuum drying oven at 40-60℃ for 8-12h to obtain La-Fe3O4 nanoparticles.

[0010] S4. Add 2-methylimidazole to methanol and sonicate for 20 min to obtain solution A. Add Co(NO3)2·6H2O to methanol and sonicate for 20 min to obtain solution B.

[0011] S5. Add the B solution obtained in step S4 to the A solution obtained in step S4, and stir the reaction at room temperature for 24 hours to obtain reactant two;

[0012] S6. After centrifuging the reactant obtained in step S5, wash it five times with methanol and deionized water respectively, and then place it in a vacuum drying oven at 40-60℃ for 8-12h to obtain ZIF-67 metal-organic framework material.

[0013] S7. Add the La-Fe3O4 nanoparticles obtained in step S3, the ZIF-67 metal-organic framework material obtained in step S6, and trisodium citrate to deionized water, stir ultrasonically for 30 min, and react at 100-150℃ for 1-3 h to obtain reactant three.

[0014] S8. After separating the three magnetic properties of the reactants obtained in step S7, wash them five times with methanol and deionized water respectively, and then place them in a vacuum drying oven at 40-60℃ for 8-12 hours to obtain lanthanum-modified metal-organic framework magnetic nano-phosphorus removal material.

[0015] Furthermore, in step S1 of the present invention, the ratio of FeCl3·6H2O, LaCl3·nH2O, and ethylene glycol is (40-80) mmol:(20-40) mmol:1L.

[0016] Further, the ratio of anhydrous sodium acetate, polyethylene glycol, and FeCl3·6H2O in this invention is (150-450) mmol:(5-8) g:15 mmol; in step S2, the autoclave is a stainless steel autoclave with a Teflon liner.

[0017] Furthermore, in step S4 of the present invention, the concentration of 2-methylimidazole in solution A is 10-40 mmol / L, and the concentration of Co(NO3)2·6H2O in solution B is 5-10 mmol / L.

[0018] Furthermore, in step S5 of the present invention, the volume ratio of solution B obtained in step S4 to solution A obtained in step S4 is 1:1.

[0019] Furthermore, in step S7 of the present invention, the ratio of La-Fe3O4 nanoparticles obtained in step S3, ZIF-67 metal-organic framework material obtained in step S6, trisodium citrate, and deionized water is (20-30) mg: (50-60) mg: (100-150) mg: (30-50) mL.

[0020] Another technical problem to be solved by the present invention is to provide a lanthanum-modified metal-organic framework magnetic nanomaterial for phosphorus removal prepared by the above preparation method.

[0021] This invention also provides the application of the above-mentioned lanthanum-modified metal-organic framework magnetic nanomaterials for phosphorus removal in the removal of phosphates and diazinon phosphorus from water.

[0022] Furthermore, the application includes the following steps:

[0023] Lanthanum-modified metal-organic framework magnetic nanomaterials for phosphorus removal were added to an aqueous solution of phosphate or diazinon and reacted at 25-35°C for 20-120 min. The concentration of the aqueous solution of phosphate was 10-50 mg / L, and the concentration of the aqueous solution of diazinon was 5-20 mg / L. The ratio of lanthanum-modified metal-organic framework magnetic nanomaterials for phosphorus removal to aqueous solution of phosphate or diazinon was (0.2-1) g:1 L. The initial pH of the reaction was 3-9. When removing diazinon, potassium persulfate was added at the same time as the lanthanum-modified metal-organic framework magnetic nanomaterials for phosphorus removal. The ratio of potassium persulfate to diazinon was (0.25-2) mmol:1 L.

[0024] Furthermore, the phosphate in the phosphate aqueous solution is sodium dihydrogen phosphate.

[0025] Compared with the prior art, the present invention has the following beneficial effects:

[0026] 1) This invention uses La-Fe3O4 nanoparticles combined with ZIF-67 metal-organic framework material to give the nano-phosphorus removal material magnetic properties, making it easy to separate from water and recycle.

[0027] 2) The lanthanum-modified metal-organic framework magnetic nano-phosphorus removal material prepared by this invention has a large specific surface area and can effectively capture inorganic phosphorus in water by chelating lanthanum with phosphate. The incorporation of lanthanum enhances the capture performance of the nano-phosphorus removal material for phosphate ions in water and improves its adsorption effect.

[0028] 3) ZIF-67 metal-organic framework material can efficiently activate potassium persulfate to generate free radicals to oxidize low concentrations of organophosphorus pesticides. At the same time, the La-Fe3O4 nanoparticles loaded on its surface can adsorb the generated inorganic phosphorus in situ, avoiding secondary pollution. Therefore, the lanthanum modified metal-organic framework magnetic nano-phosphorus removal material of the present invention has excellent adsorption performance and catalytic activity, and can efficiently remove both organic and inorganic phosphorus in water. It can remove phosphorus in various forms in water and can be widely used to remove phosphorus from sewage and river and lake sediments. Attached Figure Description

[0029] The accompanying drawings, which are included to provide a further understanding of the invention and form part of this application, do not constitute an undue limitation of the invention. In the drawings:

[0030] Figure 1 The nitrogen adsorption-desorption isotherm and pore size distribution of the lanthanum-modified metal-organic framework magnetic nano-phosphorus removal material prepared in Example 1 of this invention are shown below.

[0031] Figure 2 The image shows the hysteresis curve of the lanthanum-modified metal-organic framework magnetic nanomaterial for phosphorus removal prepared in Example 1 of this invention. Detailed Implementation

[0032] The present invention will now be described in detail with reference to specific embodiments. The illustrative embodiments and descriptions of the present invention are used to explain the present invention, but are not intended to limit the present invention.

[0033] Example 1

[0034] Lanthanum-modified metal-organic framework magnetic nanomaterials for phosphorus removal were prepared according to the following steps:

[0035] S1. FeCl3·6H2O and LaCl3·nH2O were added to ethylene glycol in a ratio of 62.5mmol:31.25mmol:1L and stirred for 30 min to obtain a precursor solution;

[0036] S2. Add anhydrous sodium acetate and polyethylene glycol to the precursor solution obtained in step S1 to obtain a mixed solution. Seal the mixed solution in an autoclave, and then place the stainless steel autoclave lined with Teflon in an oven. React at 200°C for 10 hours, and then cool naturally to room temperature to obtain reactant one. The ratio of anhydrous sodium acetate, polyethylene glycol and FeCl3·6H2O is 300mmol:6g:15mmol.

[0037] S3. After magnetic separation, the reactants obtained in step S2 were washed five times with anhydrous ethanol and deionized water, respectively, and then placed in a vacuum drying oven at 50°C for 12 hours to obtain La-Fe3O4 nanoparticles.

[0038] S4. Add 2-methylimidazole to methanol and sonicate for 20 min to obtain solution A with a concentration of 30 mmol / L of 2-methylimidazole. Add Co(NO3)2·6H2O to methanol and sonicate for 20 min to obtain solution B with a concentration of 8 mmol / L of Co(NO3)2·6H2O.

[0039] S5. Add the B solution obtained in step S4 to the A solution obtained in step S4 at a volume ratio of 1:1, and stir at room temperature for 24 hours to obtain reactant two.

[0040] S6. After centrifuging the reactant obtained in step S5, wash it five times with methanol and deionized water respectively, and then place it in a vacuum drying oven at 50°C for 12 hours to obtain ZIF-67 metal-organic framework material.

[0041] S7. The La-Fe3O4 nanoparticles obtained in step S3, the ZIF-67 metal-organic framework material obtained in step S6, and trisodium citrate were added to deionized water in a ratio of 20mg:50mg:130mg:50mL. After ultrasonic stirring for 30min, the mixture was reacted at 120℃ for 2h to obtain reactant three.

[0042] S8. After separating the three magnetic properties of the reactants obtained in step S7, wash them five times with methanol and deionized water respectively, and then place them in a vacuum drying oven at 50°C for 12 hours to obtain lanthanum-modified metal-organic framework magnetic nanomaterials for phosphorus removal.

[0043] Figure 1 The figures show the nitrogen adsorption-desorption isotherms and pore size distribution of the lanthanum-modified metal-organic framework magnetic nanomaterial for phosphorus removal prepared in Example 1. Figure 1 It can be seen that the specific surface area of ​​the lanthanum-modified metal-organic framework magnetic nanomaterial for phosphorus removal prepared in Example 1 is 627.3 m². 2 / g, pore volume is 0.22cm³ 3 With an average pore size of 13.47 nm, it exhibits excellent properties of mesoporous materials.

[0044] Figure 2 The magnetic hysteresis curve of the lanthanum-modified metal-organic framework magnetic nanomaterial for phosphorus removal prepared in Example 1 is shown. Its saturation magnetization (Ms) is 75.38 emu / g. Figure 1 It can be seen that the lanthanum-modified metal-organic framework magnetic nanomaterial for phosphorus removal prepared in Example 1 has good superparamagnetic properties, which is beneficial for recycling from solution in practical applications.

[0045] The application of the lanthanum-modified metal-organic framework magnetic nanomaterial for phosphorus removal prepared in Example 1 in the removal of diazinon phosphorus from water includes the following steps:

[0046] Lanthanum-modified metal-organic framework magnetic nanomaterials for phosphorus removal and potassium peroxymonosulfate were added to a 10 mg / L diazinon aqueous solution and reacted at 25 °C for 30 min. The ratio of lanthanum-modified metal-organic framework magnetic nanomaterials for phosphorus removal to diazinon aqueous solution was 0.5 g: 1 L, and the ratio of potassium peroxymonosulfate to diazinon aqueous solution was 0.25 mmol: 1 L. The initial pH of the reaction was 7. After the reaction was completed, the lanthanum-modified metal-organic framework magnetic nanomaterials for phosphorus removal were separated and recovered under the action of an external magnetic field.

[0047] The reacted water sample was filtered through a 0.45 μm aqueous filter membrane, and the concentrations of diazinon, total phosphorus, and phosphate ions in the liquid were determined. Diazinon was determined by liquid chromatography, while phosphate ions and total phosphorus were determined by ammonium molybdate spectrophotometry (GB11893-89). The results showed that Example 1 achieved a diazinon removal rate of 94.7% and a total phosphorus removal rate of 89.6%.

[0048] Example 2

[0049] Lanthanum-modified metal-organic framework magnetic nanomaterials for phosphorus removal were prepared according to the following steps:

[0050] S1. Add FeCl3·6H2O and LaCl3·nH2O to ethylene glycol in a ratio of 60mmol:30mmol:1L and stir for 30min to obtain a precursor solution;

[0051] S2. Add anhydrous sodium acetate and polyethylene glycol to the precursor solution obtained in step S1 to obtain a mixed solution. Seal the mixed solution in an autoclave, and then place the stainless steel autoclave lined with Teflon in an oven. React at 150°C for 12 hours and cool naturally to room temperature to obtain reactant one. The ratio of anhydrous sodium acetate, polyethylene glycol and FeCl3·6H2O is 150mmol:5g:15mmol.

[0052] S3. After magnetic separation, the reactants obtained in step S2 were washed five times with anhydrous ethanol and deionized water, respectively, and then placed in a vacuum drying oven at 50°C for 10 h to obtain La-Fe3O4 nanoparticles.

[0053] S4. Add 2-methylimidazole to methanol and sonicate for 20 min to obtain solution A with a concentration of 20 mmol / L of 2-methylimidazole. Add Co(NO3)2·6H2O to methanol and sonicate for 20 min to obtain solution B with a concentration of 9 mmol / L of Co(NO3)2·6H2O.

[0054] S5. Add the B solution obtained in step S4 to the A solution obtained in step S4 at a volume ratio of 1:1, and stir at room temperature for 24 hours to obtain reactant two.

[0055] S6. After centrifuging the reactant obtained in step S5, wash it five times with methanol and deionized water respectively, and then place it in a vacuum drying oven at 50°C for 10 hours to obtain ZIF-67 metal-organic framework material.

[0056] S7. The La-Fe3O4 nanoparticles obtained in step S3, the ZIF-67 metal-organic framework material obtained in step S6, and trisodium citrate were added to deionized water in a ratio of 25mg:55mg:120mg:40mL. After ultrasonic stirring for 30min, the mixture was reacted at 100℃ for 3h to obtain reactant three.

[0057] S8. After separating the three magnetic properties of the reactants obtained in step S7, wash them five times with methanol and deionized water respectively, and then place them in a vacuum drying oven at 50°C for 10 hours to obtain lanthanum-modified metal-organic framework magnetic nanomaterials for phosphorus removal.

[0058] The application of the lanthanum-modified metal-organic framework magnetic nanomaterial for phosphorus removal prepared in Example 2 in the removal of phosphates from water includes the following steps:

[0059] Lanthanum-modified metal-organic framework magnetic nanomaterials for phosphorus removal were added to a 5 mg / L sodium dihydrogen phosphate aqueous solution and reacted at 30°C for 120 min. The ratio of lanthanum-modified metal-organic framework magnetic nanomaterials for phosphorus removal to sodium dihydrogen phosphate aqueous solution was 0.2 g: 1 L, and the initial pH of the reaction was 7. After the reaction was completed, the lanthanum-modified metal-organic framework magnetic nanomaterials for phosphorus removal were separated and recovered under the action of an external magnetic field.

[0060] The reacted water sample was filtered through an aqueous filter membrane with a pore size of 0.45 μm, and the concentrations of diazinon, total phosphorus, and phosphate ions in the liquid were determined. Diazinon was determined by liquid chromatography, while phosphate ions and total phosphorus were determined by ammonium molybdate spectrophotometry (GB11893-89). The results showed that Example 2 achieved a phosphate removal rate of 98.5%.

[0061] Example 3

[0062] Lanthanum-modified metal-organic framework magnetic nanomaterials for phosphorus removal were prepared according to the following steps:

[0063] S1. Add FeCl3·6H2O and LaCl3·nH2O to ethylene glycol in a ratio of 80mmol:40mmol:1L and stir for 30min to obtain a precursor solution;

[0064] S2. Add anhydrous sodium acetate and polyethylene glycol to the precursor solution obtained in step S1 to obtain a mixed solution. Seal the mixed solution in an autoclave, and then place the stainless steel autoclave lined with Teflon in an oven. React at 250°C for 8 hours and cool naturally to room temperature to obtain reactant one. The ratio of anhydrous sodium acetate, polyethylene glycol and FeCl3·6H2O is 450mmol:8g:15mmol.

[0065] S3. After magnetic separation, the reactants obtained in step S2 were washed five times with anhydrous ethanol and deionized water, respectively, and then placed in a vacuum drying oven at 60°C for 8 hours to obtain La-Fe3O4 nanoparticles.

[0066] S4. Add 2-methylimidazole to methanol and sonicate for 20 min to obtain solution A with a concentration of 40 mmol / L of 2-methylimidazole. Add Co(NO3)2·6H2O to methanol and sonicate for 20 min to obtain solution B with a concentration of 10 mmol / L of Co(NO3)2·6H2O.

[0067] S5. Add the B solution obtained in step S4 to the A solution obtained in step S4 at a volume ratio of 1:1, and stir at room temperature for 24 hours to obtain reactant two.

[0068] S6. After centrifuging the reactant obtained in step S5, wash it five times with methanol and deionized water respectively, and then place it in a vacuum drying oven at 60°C for 8 hours to obtain ZIF-67 metal-organic framework material.

[0069] S7. The La-Fe3O4 nanoparticles obtained in step S3, the ZIF-67 metal-organic framework material obtained in step S6, and trisodium citrate were added to deionized water in a ratio of 30mg:60mg:150mg:50mL. After ultrasonic stirring for 30min, the mixture was reacted at 150℃ for 1h to obtain reactant three.

[0070] S8. After separating the three magnetic properties of the reactants obtained in step S7, wash them five times with methanol and deionized water respectively, and then place them in a vacuum drying oven at 60°C for 8 hours to obtain lanthanum-modified metal-organic framework magnetic nanomaterials for phosphorus removal.

[0071] The application of the lanthanum-modified metal-organic framework magnetic nanomaterial for phosphorus removal prepared in Example 3 in the removal of diazinon phosphorus from water includes the following steps:

[0072] Lanthanum-modified metal-organic framework magnetic nanomaterials for phosphorus removal and potassium peroxymonosulfate were added to a 20 mg / L diazinon aqueous solution and reacted at 35 °C for 20 min. The ratio of lanthanum-modified metal-organic framework magnetic nanomaterials for phosphorus removal to diazinon aqueous solution was 1 g:1 L, and the ratio of potassium peroxymonosulfate to diazinon aqueous solution was 2 mmol:1 L. The initial pH of the reaction was 3. After the reaction was completed, the lanthanum-modified metal-organic framework magnetic nanomaterials for phosphorus removal were separated and recovered under the action of an external magnetic field.

[0073] The reacted water sample was filtered through a 0.45 μm aqueous filter membrane, and the concentrations of diazinon, total phosphorus, and phosphate ions in the liquid were determined. Diazinon was determined by liquid chromatography, while phosphate ions and total phosphorus were determined by ammonium molybdate spectrophotometry (GB11893-89). The results showed that Example 3 achieved a diazinon removal rate of 91.3% and a total phosphorus removal rate of 86.8%.

[0074] Example 4

[0075] Lanthanum-modified metal-organic framework magnetic nanomaterials for phosphorus removal were prepared according to the following steps:

[0076] S1. Add FeCl3·6H2O and LaCl3·nH2O to ethylene glycol in a ratio of 40mmol:20mmol:1L and stir for 30min to obtain a precursor solution;

[0077] S2. Add anhydrous sodium acetate and polyethylene glycol to the precursor solution obtained in step S1 to obtain a mixed solution. Seal the mixed solution in an autoclave, then place the stainless steel autoclave lined with Teflon in an oven and react at 180°C for 9 hours. After naturally cooling to room temperature, reactant 1 is obtained. The ratio of anhydrous sodium acetate, polyethylene glycol, and FeCl3·6H2O is 400mmol:7g:15mmol.

[0078] S3. After magnetic separation, the reactants obtained in step S2 were washed five times with anhydrous ethanol and deionized water, and then placed in a vacuum drying oven at 40°C for 12 hours to obtain La-Fe3O4 nanoparticles.

[0079] S4. Add 2-methylimidazole to methanol and sonicate for 20 min to obtain solution A with a concentration of 10 mmol / L of 2-methylimidazole. Add Co(NO3)2·6H2O to methanol and sonicate for 20 min to obtain solution B with a concentration of 5 mmol / L of Co(NO3)2·6H2O.

[0080] S5. Add the B solution obtained in step S4 to the A solution obtained in step S4 at a volume ratio of 1:1, and stir at room temperature for 24 hours to obtain reactant two.

[0081] S6. After centrifuging the reactant obtained in step S5, wash it five times with methanol and deionized water respectively, and then place it in a vacuum drying oven at 40°C for 12 hours to obtain ZIF-67 metal-organic framework material.

[0082] S7. The La-Fe3O4 nanoparticles obtained in step S3, the ZIF-67 metal-organic framework material obtained in step S6, and trisodium citrate were added to deionized water in a ratio of 24mg:56mg:140mg:45mL. After ultrasonic stirring for 30min, the mixture was reacted at 130℃ for 1.5h to obtain reactant three.

[0083] S8. After separating the three magnetic properties of the reactants obtained in step S7, wash them five times with methanol and deionized water respectively, and then place them in a vacuum drying oven at 40°C for 12 hours to obtain lanthanum-modified metal-organic framework magnetic nanomaterials for phosphorus removal.

[0084] The application of the lanthanum-modified metal-organic framework magnetic nanomaterial for phosphorus removal prepared in Example 4 in the removal of diazinon phosphorus from water includes the following steps:

[0085] Lanthanum-modified metal-organic framework magnetic nanomaterials for phosphorus removal and potassium peroxymonosulfate were added to a 15 mg / L aqueous solution of diazinon and reacted at 25 °C for 30 min. The ratio of lanthanum-modified metal-organic framework magnetic nanomaterials for phosphorus removal to diazinon aqueous solution was 0.7 g:1 L, and the ratio of potassium peroxymonosulfate to diazinon aqueous solution was 1 mmol:1 L. The initial pH of the reaction was 9. After the reaction was completed, the lanthanum-modified metal-organic framework magnetic nanomaterials for phosphorus removal were separated and recovered under the action of an external magnetic field.

[0086] The reacted water sample was filtered through an aqueous filter membrane with a pore size of 0.45 μm, and the concentrations of diazinon, total phosphorus, and phosphate ions in the liquid were determined. Diazinon was determined by liquid chromatography, while phosphate ions and total phosphorus were determined by ammonium molybdate spectrophotometry (GB11893-89). The results showed that Example 4 achieved a diazinon removal rate of 95.6% and a total phosphorus removal rate of 90.2%.

[0087] Comparative Example 1:

[0088] The difference from Example 1 is that steps S4-S8 are not included, but the other steps are the same. La-doped Fe3O4 nanoparticles are obtained, and then potassium persulfate is activated to remove diazinon phosphorus from the water according to the steps of Example 1.

[0089] Comparative Example 2:

[0090] The difference from Example 2 is that LaCl3·nH2O was not added in step S1, while the other steps were the same. The resulting material was a metal-organic framework magnetic phosphorus removal material that had not been modified with lanthanum. Then, the phosphate in the water was removed according to the steps in Example 2.

[0091] The removal rates of diazinphos-methyl, phosphate, and total phosphorus by the lanthanum-modified metal-organic framework magnetic phosphorus removal materials prepared in Examples 1 and 2, and the products obtained in Comparative Examples 1 and 2, are summarized in Table 1 below:

[0092] Table 1.

[0093]

[0094] As can be seen from the removal rates of Example 1 and Comparative Example 1 in Table 1, Example 1 also has Co-based MOF material on the basis of Comparative Example 1, which can improve the activation effect of the composite material on potassium persulfate, thereby significantly improving the removal rates of diazinon and total phosphorus.

[0095] As can be seen from the removal rates of Example 2 and Comparative Example 2 in Table 1, Example 2, based on Comparative Example 2, also added LaCl3·nH2O. The incorporation of lanthanum can significantly improve the adsorption performance of the phosphorus removal material for phosphate.

[0096] The above embodiments are merely illustrative of the principles and effects of the present invention and are not intended to limit the invention. Any person skilled in the art can modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by those skilled in the art without departing from the spirit and technical concept disclosed in the present invention should still be covered by the claims of the present invention.

Claims

1. A method for preparing a lanthanum-modified metal-organic framework magnetic nanomaterial for phosphorus removal, characterized in that: Includes the following steps: S1. Add FeCl3·6H2O and LaCl3·nH2O to ethylene glycol and stir for 30 min to obtain a precursor solution. The ratio of FeCl3·6H2O, LaCl3·nH2O and ethylene glycol is (40-80) mmol: (20-40) mmol: 1L. S2. Add anhydrous sodium acetate and polyethylene glycol to the precursor solution obtained in step S1 to obtain a mixed solution. Seal the mixed solution in an autoclave, then place the autoclave in an oven and react at 150-250℃ for 8-12 hours. Allow it to cool naturally to room temperature to obtain reactant one. The ratio of anhydrous sodium acetate, polyethylene glycol, and FeCl3·6H2O is (150-450) mmol: (5-8) g: 15 mmol. S3. After magnetic separation, the reactants obtained in step S2 are washed five times with anhydrous ethanol and deionized water, respectively, and then placed in a vacuum drying oven at 40-60℃ for 8-12h to obtain La-Fe3O4 nanoparticles. S4. Add 2-methylimidazole to methanol and sonicate for 20 min to obtain solution A. Add Co(NO3)2·6H2O to methanol and sonicate for 20 min to obtain solution B. The concentration of 2-methylimidazole in solution A is 10-40 mmol / L, and the concentration of Co(NO3)2·6H2O in solution B is 5-10 mmol / L. S5. Add the B solution obtained in step S4 to the A solution obtained in step S4, stir and react at room temperature for 24 hours to obtain reactant 2. The volume ratio of the B solution obtained in step S4 to the A solution obtained in step S4 is 1:

1. S6. After centrifuging the reactant obtained in step S5, wash it five times with methanol and deionized water respectively, and then place it in a vacuum drying oven at 40-60℃ for 8-12h to obtain ZIF-67 metal-organic framework material. S7. Add the La-Fe3O4 nanoparticles obtained in step S3, the ZIF-67 metal-organic framework material obtained in step S6, and trisodium citrate to deionized water, stir ultrasonically for 30 min, and react at 100-150℃ for 1-3 h to obtain reactant three; the ratio of La-Fe3O4 nanoparticles obtained in step S3, ZIF-67 metal-organic framework material obtained in step S6, trisodium citrate, and deionized water is (20-30) mg: (50-60) mg: (100-150) mg: (30-50) mL; S8. After separating the three magnetic properties of the reactants obtained in step S7, wash them five times with methanol and deionized water respectively, and then place them in a vacuum drying oven at 40-60℃ for 8-12 hours to obtain lanthanum-modified metal-organic framework magnetic nanomaterials for removing diazine phosphorus from water.

2. The preparation method of a lanthanum-modified metal-organic framework magnetic nanomaterial for phosphorus removal according to claim 1, characterized in that: In step S2, the autoclave is a stainless steel autoclave with a Teflon lining.

3. The lanthanum-modified metal-organic framework magnetic nanomaterial for removing phosphorus by the preparation method according to claims 1-2, i.e., the lanthanum-modified metal-organic framework magnetic nanomaterial for removing diazinphos-methyl from water.

4. The application of the lanthanum-modified metal-organic framework magnetic nanomaterial for phosphorus removal according to claim 3 in the removal of diazinon phosphorus from water.

5. The application according to claim 4, characterized in that: Includes the following steps: Lanthanum-modified metal-organic framework magnetic nanomaterials for phosphorus removal were added to a diazinon aqueous solution and reacted at 25-35℃ for 20-120 min. The concentration of the diazinon aqueous solution was 5-20 mg / L, and the ratio of lanthanum-modified metal-organic framework magnetic nanomaterials for phosphorus removal to diazinon aqueous solution was (0.2-1) g:1 L. The initial pH of the reaction was 3-9. When removing diazinon phosphorus, potassium persulfate was also added at the same time as the lanthanum-modified metal-organic framework magnetic nanomaterials for phosphorus removal. The ratio of potassium persulfate to diazinon aqueous solution was (0.25-2) mmol:1 L.

Citation Information

Patent Citations

  • Method for preparing magnetic adsorbents on basis of iron-based metal-organic framework materials and application of magnetic adsorbents

    CN105688825A

  • Preparation method and application of visible light response magnetic metal organic framework material

    CN109225341A