Self-repairing polyurethane elastomer for wooden furniture and preparation method thereof

By introducing the polyurethane elastomer formula of PEG derivatives and disulfide bonds into wooden furniture repair materials, the problems of lack of self-healing function and insufficient durability in the existing technology are solved, and the self-healing and durability improvement of the material are achieved, which is suitable for Industrial production reduces maintenance costs and production complexity.

CN118480259BActive Publication Date: 2024-10-18ZIBO HUATIAN RUBBER & PLASTICS SCI & TECH
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410947419.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-16
Publication Date
2024-10-18
Estimated Expiration
2044-07-16

AI Technical Summary

Technical Problem

Existing wooden furniture repair materials lack self-healing functions, have high maintenance costs, are difficult to achieve traceless repairs, and are insufficient in terms of durability, bonding effect, and environmental adaptability.

Method used

The polyurethane elastomer formula uses PEG derivatives, dihydroxyl, ether bonds and disulfide bonds. Through molecular structure optimization and filler addition, the self-healing ability, hydrolysis resistance and low temperature resistance of the material are improved, and a scientific and reasonable preparation method is adopted. Suitable for industrial production.

Benefits of technology

It realizes the self-healing function of the wooden furniture surface, reduces maintenance costs, extends the service life of the furniture, improves the stability and application prospects of the material, while simplifying the production process and reducing costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_2
    Figure SMS_2
  • Figure QLYQS_1
    Figure QLYQS_1
Patent Text Reader

Abstract

The present invention belongs to the technical field of polyurethane elastomers, and specifically relates to a self-repairing polyurethane elastomer for wooden furniture and a preparation method thereof. It is composed of the following raw materials in weight percentage: 31-66% of PEG derivatives; 10%-18% of small molecule diol chain extenders; 17%-48% of diisocyanates; 5%-10% of fillers; and the molecular structure of the PEG derivatives contains dihydroxyl, ether bonds and disulfide bonds. The present invention optimizes the formula components, and the obtained polyurethane elastomer has significant advantages in terms of reaction efficiency, self-repairing ability, hydrolysis resistance, low temperature resistance, etc. While providing furniture surface protection, it can realize self-repairing function, thereby extending the service life of furniture and reducing maintenance costs; it is also easy to use and has a wider application prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polyurethane elastomers, and in particular relates to a self-repairing polyurethane elastomer specially used for wooden furniture and a preparation method thereof. Background Art

[0002] With the development of social economy and the improvement of people's living standards, wooden furniture has gradually become the first choice for high-end residential and office environments due to its natural, environmentally friendly and beautiful features. However, wooden furniture is easily scratched and worn during use, which not only affects its appearance, but also reduces the service life of the furniture. At present, the traditional grinding and filling method is mostly used for the repair of wooden furniture. This method is not only time-consuming and labor-intensive, but also the repaired parts are often difficult to perfectly match the original wood in color and texture, resulting in unsatisfactory repair results.

[0003] Polyurethane elastomers are widely used in furniture repair due to their fast curing and good adhesion. In particular, polyurethane hot melt elastomers are considered to be an ideal repair material due to their excellent flexibility and bonding strength. However, most of the existing polyurethane elastomers do not have self-repairing functions. Once the polyurethane layer on the surface of the furniture is scratched, manual intervention is still required to restore its original surface state. In addition, the curing time, bonding strength and temperature resistance of polyurethane elastomers still need to be improved to meet the growing demand for furniture repair.

[0004] The main problems existing in the existing technology are as follows: First, wooden furniture repair materials cannot repair scratches on their own during use, and the maintenance cost is high; second, for some high-grade fine woods, traditional repair methods are difficult to achieve seamless repair, which affects the overall appearance of the furniture; third, the existing polyurethane elastomers are still insufficient in durability, bonding effect and environmental adaptability. Based on this, there is an urgent need for a new type of wooden furniture repair material that can not only self-repair minor scratches on the surface of furniture and maintain the overall appearance of the furniture, but also has significant improvements in physical and mechanical properties, heat resistance and environmental adaptability to meet market demand.

[0005] Chinese patent CN114835870B discloses a self-repairing discoloration film and its preparation method, which includes the following raw materials by weight: 40-50 parts of polytetrahydrofuran, 35-38 parts of isophorone diisocyanate, 60-70 parts of dispersant, 0.5-0.6 parts of catalyst, 7-9 parts of discoloration component, 10-12 parts of disulfide monomer, 7-8 parts of end-capping agent, 14-15 parts of cross-linking monomer; in the preparation process, by adjusting the raw materials, introducing hydroxyl groups into the molecular structure, and then using it as a functional monomer to react with disulfide monomer, polytetrahydrofuran and isophorone diisocyanate, the discoloration component is introduced into the network structure of polyurethane, further improving its discoloration effect, and having a good improvement effect on the mechanical properties of the material after film formation. However, its composition is relatively complex, the operation is cumbersome, and the prepared product does not have thermoplasticity and cannot be recycled. Summary of the invention

[0006] In view of the deficiencies of the prior art, the purpose of the present invention is to provide a self-repairing polyurethane elastomer for wooden furniture. By optimizing the formula components, the prepared polyurethane elastomer has significant advantages in reaction efficiency, self-repairing ability, hydrolysis resistance, low temperature resistance, etc., and can realize self-repairing function while providing furniture surface protection, thereby extending the service life of the furniture and reducing maintenance costs; at the same time, it is easy to use and has a wider application prospect;

[0007] Another object of the present invention is to provide a method for preparing a self-repairing polyurethane elastomer specially used for wooden furniture, which is scientific, reasonable and suitable for industrial production.

[0008] The technical solution adopted by the present invention is as follows:

[0009] The self-repairing polyurethane elastomer for wooden furniture is composed of the following raw materials in percentage by weight:

[0010] PEG derivatives 31-66%;

[0011] Small molecule diol chain extender 10%-18%;

[0012] Diisocyanate 17%-48%;

[0013] Filler 5%-10%;

[0014] The molecular structure of the PEG derivative contains dihydroxyl, ether bond and disulfide bond;

[0015] The diisocyanate is one or more of aliphatic isocyanate or alicyclic isocyanate.

[0016] The structural formula of the PEG derivative is as follows:

[0017] ;

[0018] Among them, 11≤n≤45.

[0019] The small molecule diol chain extender is one or more of 1,4-butanediol, 1,6-hexanediol or 1,4-cyclohexanediol.

[0020] The diisocyanate is one or more of hexamethylene diisocyanate, isophorone diisocyanate, cyclohexane dimethylene diisocyanate or 4,4'-dicyclohexylmethane diisocyanate.

[0021] The filler is one or more of wood powder, calcium carbonate, diatomaceous earth, nano silicon dioxide, nano titanium dioxide or nano carbon tube.

[0022] The method for preparing the self-repairing polyurethane elastomer for wooden furniture comprises the following steps:

[0023] (1) Preheat the PEG derivative to 100-110°C, add 0.4-0.8% filler based on the total weight of the formula, stir, and vacuum degass to obtain component A; preheat the diisocyanate to 55-65°C, and vacuum degass to obtain component B; preheat the small molecule diol chain extender to 55-65°C, and vacuum degass to obtain component C;

[0024] (2) Component A, component B and component C are metered and mixed by a pouring machine and poured onto a conveyor belt. The conveyor belt is provided with 7 heating zones and 5 cooling zones. The materials first pass through the heating zone for gel curing and then pass through the cooling zone for cooling;

[0025] (3) Sending the cooled material into a pulverizer for crushing;

[0026] (4) After mixing the crushed material with the filler, the mixture is added into a twin-screw extruder granulator for granulation;

[0027] (5) The granulated material is dehydrated and dried to obtain a self-repairing polyurethane elastomer for wooden furniture.

[0028] In the step (2), the total gel curing time is 40-90 seconds, and the total cooling time is 60-120 seconds.

[0029] In the step (2), the gel curing temperature is 120-175°C; and the cooling temperature is 100-160°C.

[0030] In the step (4), the granulation temperature is 90-150°C.

[0031] Compared with the prior art, the present invention has the following beneficial effects:

[0032] (1) The self-repairing polyurethane elastomer for wooden furniture described in the present invention, through the optimization of the formula components, introduces raw materials containing dihydroxyl, ether bond and disulfide bond in the molecular structure, thereby ensuring a high degree of molecular structure consistency, thereby improving the production quality stability of the material; the presence of dihydroxyl significantly improves the reaction activity, which helps to obtain a high molecular weight, dense structure polyurethane elastomer material; the introduction of disulfide bonds enables the material to be quickly and automatically repaired under light or certain temperature conditions when it suffers from slight scratches or damage, effectively reducing the damage marks on the furniture surface and reducing maintenance costs; the use of ether bonds significantly improves the hydrolysis resistance and low temperature resistance of the material compared to traditional ester bonds, ensuring that the furniture can maintain stable performance under different environmental conditions; at the same time, the use of diisocyanates that do not contain benzene rings or naphthalene rings improves the yellowing resistance of the material; the addition of fillers enhances the hardness and scratch resistance of the polyurethane elastomer, thereby improving the overall stability of the material;

[0033] (2) The self-repairing polyurethane elastomer for wooden furniture of the present invention provides a cost-effective and easy-to-operate wooden furniture repair material through molecular structure optimization and the introduction of self-repairing function. It is not only easy to use, but also can effectively protect and extend the service life of wooden furniture, and has broad application prospects.

[0034] (3) The preparation method of the self-healing polyurethane elastomer for wooden furniture described in the present invention reduces the types of raw materials and mixing steps, which not only reduces the production cost but also improves the production efficiency. It is scientific and reasonable and suitable for industrial production. At the same time, due to the consistency of the molecular structure, the difficulty of quality control in the production process is reduced, and the stability and reliability of the material are improved. DETAILED DESCRIPTION

[0035] The present invention is further described below with reference to the embodiments, but they do not limit the implementation of the present invention.

[0036] The raw materials used in the examples and comparative examples are conventional commercially available raw materials unless otherwise specified, and the process methods used in the examples and comparative examples are conventional methods in the art unless otherwise specified.

[0037] Some of the raw materials used in the examples and comparative examples are described as follows:

[0038] PEG derivatives were purchased from Xi'an Qiyue Biotechnology Co., Ltd.;

[0039] Polyethylene glycol (CHPEG-1500) was purchased from Changhua Chemical Technology Co., Ltd.;

[0040] Polyester polyol JF-PE-1030 was purchased from Zhejiang Huafeng New Materials Co., Ltd.

[0041] Example 1

[0042] The self-repairing polyurethane elastomer for wooden furniture is composed of the following raw materials in percentage by weight:

[0043] PEG derivative (DP 45, number average molecular weight 5624) 66%;

[0044] Small molecule diol chain extender (a mixture of 1,6-hexanediol and 1,4-butanediol in a molar ratio of 4:1) 10%;

[0045] Hexamethylene diisocyanate 17%;

[0046] Wood flour 6.5%;

[0047] Nano silicon dioxide 0.5%;

[0048] The method for preparing the self-repairing polyurethane elastomer for wooden furniture comprises the following steps:

[0049] (1) Preheat the PEG derivative to 105°C, add nano-silica, stir, and vacuum degass to obtain component A; preheat hexamethylene diisocyanate to 60°C, and vacuum degass to obtain component B; preheat the mixture of 1,6-hexanediol and 1,4-butanediol to 55°C, and vacuum degass to obtain component C;

[0050] (2) Component A, component B and component C are measured and mixed by a pouring machine and poured onto a conveyor belt. The conveyor belt is provided with 7 heating zones and 5 cooling zones. The materials are firstly passed through the heating zone for gel curing. The temperatures of the 7 heating zones are 1#160℃, 2#165℃, 3#170℃, 4#175℃, 5#175℃, 6#175℃ and 7#175℃, respectively. Then the materials are cooled in the cooling zone. The temperatures of the 5 cooling zones are 8#160℃, 9#150℃, 10#120℃, 11#120℃ and 12#100℃, respectively. The total gel curing time is 90s and the total cooling time is 120s.

[0051] (3) Sending the cooled material into a pulverizer for crushing;

[0052] (4) After the crushed material is mixed with wood powder, it is added into a twin-screw extruder granulator for granulation. The process parameters of the granulator are as follows: the temperature of each section is 120°C for the first section, 130°C for the second section, 140°C for the third section, 130°C for the fourth section, 120°C for the fifth section, 110°C for the sixth section, 105°C for the seventh section, 100°C for the eighth section, 100°C for the ninth section, 100°C for the tenth section, and 100°C for the eleventh section; the speed of the side feeder is 100 r / min, the speed of the extruder is 200 r / min, the temperature of the reversing valve is 170°C, the temperature of the filter is 180°C, the temperature of the die head is 160°C, the speed of the pelletizer is 2500 r / min, and the water temperature of the water tank is 35°C;

[0053] (5) The granulated material is dehydrated and dried to obtain a self-repairing polyurethane elastomer for wooden furniture.

[0054] Example 2

[0055] The self-repairing polyurethane elastomer for wooden furniture is composed of the following raw materials in percentage by weight:

[0056] PEG derivative (degree of polymerization 11, number average molecular weight 1476) 31%;

[0057] Small molecule diol chain extender (a mixture of 1,6-hexanediol and 1,4-cyclohexanediol in a molar ratio of 9:1) 16%;

[0058] Diisocyanate (a mixture of hexamethylene diisocyanate and 4,4'-dicyclohexylmethane diisocyanate in a molar ratio of 4:5) 48%;

[0059] Calcium carbonate 4.6%;

[0060] Nano titanium dioxide 0.4%;

[0061] The method for preparing the self-repairing polyurethane elastomer for wooden furniture comprises the following steps:

[0062] (1) Preheat the PEG derivative to 100°C, add nano-titanium dioxide, stir, and vacuum degass to obtain component A; preheat hexamethylene diisocyanate and 4,4'-dicyclohexylmethane diisocyanate to 55°C, and vacuum degass to obtain component B; preheat the mixture of 1,6-hexanediol and 1,4-cyclohexanediol to 60°C, and vacuum degass to obtain component C;

[0063] (2) Component A, component B and component C are measured and mixed by a pouring machine and poured onto a conveyor belt. The conveyor belt is provided with 7 heating zones and 5 cooling zones. The materials are firstly passed through the heating zone for gel curing. The temperatures of the 7 heating zones are 1#130℃, 2#135℃, 3#130℃, 4#150℃, 5#165℃, 6#165℃ and 7#175℃, respectively. Then the materials are cooled in the cooling zone. The temperatures of the 5 cooling zones are 8#110℃, 9#100℃, 10#100℃, 11#100℃ and 12#100℃, respectively. The total gel curing time is 70s and the total cooling time is 95s.

[0064] (3) Sending the cooled material into a pulverizer for crushing;

[0065] (4) After the crushed material is mixed with calcium carbonate, it is added into a twin-screw extruder granulator for granulation. The process parameters of the granulator are as follows: the temperature of each section is 110°C for the first section, 120°C for the second section, 130°C for the third section, 120°C for the fourth section, 110°C for the fifth section, 100°C for the sixth section, 95°C for the seventh section, 90°C for the eighth section, 90°C for the ninth section, 90°C for the tenth section, and 90°C for the eleventh section; the speed of the side feeder is 60r / min, the speed of the extruder is 180r / min, the temperature of the reversing valve is 165°C, the temperature of the filter is 170°C, the temperature of the die head is 145°C, the speed of the pelletizer is 2400r / min, and the water temperature of the water tank is 25°C;

[0066] (5) The granulated material is dehydrated and dried to obtain a self-repairing polyurethane elastomer for wooden furniture.

[0067] Example 3

[0068] The self-repairing polyurethane elastomer for wooden furniture is composed of the following raw materials in percentage by weight:

[0069] PEG derivatives (degree of polymerization 23, number average molecular weight 2940) 42%;

[0070] 1,4-Butanediol 18%;

[0071] Diisocyanate (a mixture of isophorone diisocyanate and cyclohexane dimethylene diisocyanate in a molar ratio of 3:2) 30%;

[0072] Diatomaceous earth 9.2%;

[0073] Carbon nanotubes 0.8%;

[0074] The method for preparing the self-repairing polyurethane elastomer for wooden furniture comprises the following steps:

[0075] (1) Preheating the PEG derivative to 110°C, adding carbon nanotubes, stirring, and vacuum degassing to obtain component A; preheating the mixture of isophorone diisocyanate and cyclohexane dimethylene diisocyanate to 65°C, and vacuum degassing to obtain component B; preheating 1,4-butanediol to 65°C, and vacuum degassing to obtain component C;

[0076] (2) Component A, component B and component C are measured and mixed by a pouring machine and poured onto a conveyor belt. The conveyor belt is provided with 7 heating zones and 5 cooling zones. The materials are firstly passed through the heating zone for gel curing. The temperatures of the 7 heating zones are 1#120℃, 2#125℃, 3#150℃, 4#160℃, 5#175℃, 6#175℃ and 7#165℃, respectively. Then the materials are cooled in the cooling zone. The temperatures of the 5 cooling zones are 8#120℃, 9#110℃, 10#100℃, 11#100℃ and 12#100℃, respectively. The total gel curing time is 40s and the total cooling time is 60s.

[0077] (3) Sending the cooled material into a pulverizer for crushing;

[0078] (4) After the crushed material is mixed with diatomaceous earth, it is added into a twin-screw extruder granulator for granulation. The process parameters of the granulator are as follows: the temperature of each section is 130°C for the first section, 140°C for the second section, 150°C for the third section, 140°C for the fourth section, 130°C for the fifth section, 120°C for the sixth section, 115°C for the seventh section, 110°C for the eighth section, 110°C for the ninth section, 110°C for the tenth section, and 110°C for the eleventh section; the speed of the side feeder is 110r / min, the speed of the extruder is 230r / min, the temperature of the reversing valve is 180°C, the temperature of the filter is 195°C, the temperature of the die head is 175°C, the speed of the pelletizer is 2600r / min, and the water temperature of the water tank is 40°C;

[0079] (5) The granulated material is dehydrated and dried to obtain a self-repairing polyurethane elastomer for wooden furniture.

[0080] Comparative Example 1

[0081] The difference from Example 2 is that the PEG derivative in the formula components is replaced by polyethylene glycol CHPEG-1500 (number average molecular weight is 1500) in equal amounts, and the rest is the same as Example 2.

[0082] Comparative Example 2

[0083] The difference from Example 3 is that the PEG derivative in the formula components is replaced by an equal amount of polyester polyol JF-PE-1030 (EG / AA type, number average molecular weight of 3000), and the rest is the same as Example 3.

[0084] Comparative Example 3

[0085] The difference from Example 2 is that 4,4'-dicyclohexylmethane diisocyanate in the formula components is replaced by 4,4'-diphenylmethane diisocyanate, and the rest is the same as Example 2.

[0086] The polyurethane elastomers prepared in Examples 1-3 and Comparative Examples 1-3 were subjected to performance tests, and the test methods were as follows:

[0087] Hardness (Shore A): Tested in accordance with ASTM D2240-2015;

[0088] Yellowing resistance test: Under natural conditions (25-35℃), expose the sample outdoors for one week and observe the color change of the sample;

[0089] Light self-repair (min): Cut a 5 cm long scratch in the middle of a sample with a thickness of 2 mm and a length and width of 10 cm with a blade, place it in a UV light box at 40°C, and record the scratch repair time;

[0090] Tensile strength retention rate after immersion in water at 70℃ for 3 weeks (%): Cut 3 dumbbell-shaped specimens from a sample with a thickness of 2mm and a length and width of 10cm, test the tensile strength according to ASTMD412, and take the average value; then put the specimens into a constant temperature water bath at 70℃ and soak for 3 weeks, test the tensile strength again, take the average value, and calculate the ratio of the average tensile strength after immersion to the average tensile strength before immersion, which is the tensile strength retention;

[0091] Glass transition temperature (°C): The glass transition temperature of the samples was tested using a differential scanning calorimeter.

[0092] The test results are shown in Table 1.

[0093] Table 1 Performance test results

[0094]

[0095] It can be seen from Table 1 that the polyurethane elastomers prepared in Examples 1-3 have significant advantages in terms of reaction efficiency, self-repairing ability, hydrolysis resistance, low temperature resistance, etc., and can achieve self-repairing function while providing furniture surface protection.

[0096] Compared with Example 2, Comparative Example 1 does not have the self-repairing ability due to the absence of disulfide bonds.

[0097] Compared with Example 3, Comparative Example 2 also has no self-healing ability due to the absence of disulfide bonds. At the same time, since polyester polyols are used in Comparative Example 2, the ester group is more easily hydrolyzed than the ether group. Therefore, the tensile strength of the prepared polyurethane elastomer decreases significantly after being immersed in water at 70°C for 3 weeks, and the tensile strength retention rate decreases. In addition, since the polarity of the ester group is greater than that of the ether group, the glass transition temperature of the polyester polyurethane elastomer prepared in Comparative Example 2 is higher than that of the polyether polyurethane elastomer prepared in Example 3, and the low temperature resistance is relatively poor.

[0098] Compared with Example 2, since the used 4,4'-diphenylmethane diisocyanate is an aromatic diisocyanate and contains a benzene ring structure in its molecular structure, the prepared polyurethane elastomer has poor yellowing resistance and is prone to yellowing.

Claims

1. A self-repairing polyurethane elastomer for wooden furniture, characterized in that: The following weight percentages of raw materials composition: PEG derivatives 31-66%; Small molecule diol chain extender 10%-18%; Diisocyanate 17%-48%; Filler 5%-10%; The structural formula of the PEG derivative is as follows: ; Among them, 11≤n≤45; The diisocyanate is one or more of aliphatic isocyanate or alicyclic isocyanate.

2. The self-repairing polyurethane elastomer for wooden furniture according to claim 1, characterized in that: The small molecule diol chain extender is one or more of 1,4-butanediol, 1,6-hexanediol or 1,4-cyclohexanediol.

3. The self-repairing polyurethane elastomer for wooden furniture according to claim 1, characterized in that: The diisocyanate is one or more of hexamethylene diisocyanate, isophorone diisocyanate, cyclohexane dimethylene diisocyanate or 4,4'-dicyclohexylmethane diisocyanate.

4. The self-repairing polyurethane elastomer for wooden furniture according to claim 1, characterized in that: The filler is one or more of wood powder, calcium carbonate, diatomaceous earth, nano silicon dioxide, nano titanium dioxide or nano carbon tube.

5. A method for preparing the self-repairing polyurethane elastomer for wooden furniture according to any one of claims 1 to 4, characterized in that: The following steps are involved: (1) Preheat the PEG derivative to 100-110°C, add 0.4-0.8% filler based on the total weight of the formula, stir, and vacuum degass to obtain component A; preheat the diisocyanate to 55-65°C, and vacuum degass to obtain component B; preheat the small molecule diol chain extender to 55-65°C, and vacuum degass to obtain component C; (2) Component A, component B and component C are metered and mixed by a pouring machine, poured onto a conveyor belt, and cooled after the gel solidifies; (3) Sending the cooled material into a pulverizer for crushing; (4) Mixing the crushed material with the remaining filler, and adding the mixture to a twin-screw extruder granulator for granulation; (5) The granulated material is dehydrated and dried to obtain a self-repairing polyurethane elastomer for wooden furniture.

6. The method for preparing the self-repairing polyurethane elastomer for wooden furniture according to claim 5, characterized in that: In the step (2), the total gel curing time is 40-90 seconds, and the total cooling time is 60-120 seconds.

7. The method for preparing the self-repairing polyurethane elastomer for wooden furniture according to claim 5, characterized in that: In the step (2), the gel curing temperature is 120-175°C; and the cooling temperature is 100-160°C.

8. The method for preparing the self-repairing polyurethane elastomer for wooden furniture according to claim 5, characterized in that: In the step (4), the granulation temperature is 90-150°C.

Citation Information

Patent Citations

  • A self-healing color-changing film and its preparation method

    CN114835870B

  • Thermoplastic self-repairing polyurethane resin for 3D printing composite materials and preparation method thereof

    CN110105532A

  • Self-repairing polyurethane material and preparation method thereof

    CN113788927A