A method for synchronously polishing double sides of silicon carbide wafer

By pre-treating the silicon carbide wafer with surfactant to change its surface hydrophilicity and contact angle, the problem of high processing loss in the double-sided simultaneous polishing process is solved, and the processing loss and cost of the silicon carbide wafer are reduced.

CN118493094BActive Publication Date: 2024-10-08ZJU HANGZHOU GLOBAL SCI & TECH INNOVATION CENT
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410961673.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-10-08
Estimated Expiration
2044-07-18

AI Technical Summary

Technical Problem

The existing double-sided simultaneous polishing process of silicon carbide wafers has the problem of high processing loss, resulting in increased manufacturing costs and low efficiency.

Method used

By using a pretreatment mixture with surfactant to pretreat the silicon carbide wafer, the hydrophilicity of its carbon surface and silicon surface is changed, so that the contact angle ratio between the polishing fluid and the carbon surface and silicon surface changes, thereby reducing the double Removal rate ratio during surface simultaneous polishing.

Benefits of technology

It effectively reduces the processing loss and cost of silicon carbide wafers, while meeting the requirements of device manufacturing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118493094B_ABST
    Figure CN118493094B_ABST
Patent Text Reader

Abstract

The invention discloses a double-sided synchronous polishing method for a silicon carbide wafer. When the double-sided synchronous polishing method for a silicon carbide wafer is used to perform double-sided synchronous polishing of a silicon carbide wafer, the hydrophilicity of the carbon surface and the silicon surface of the silicon carbide wafer is changed simultaneously, and the contact angle between the subsequent polishing liquid and the carbon surface and the contact angle between the polishing liquid and the silicon surface are changed simultaneously, so that the removal rate ratio of the carbon surface and the silicon surface of the silicon carbide wafer during double-sided synchronous polishing is reduced. Although the removal rate of the Si surface is reduced, the C / Si surface removal rate ratio is reduced, the processing loss of the silicon carbide wafer is reduced, and the use requirements of device manufacturing are met while reducing the processing loss and processing cost.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of silicon carbide polishing, and in particular relates to a method for synchronously polishing double sides of a silicon carbide wafer. Background Art

[0002] Single-crystal SiC materials exhibit excellent electrical properties in extreme environments such as high pressure, high temperature and high radiation, making semiconductor power devices based on silicon carbide wafers key components of equipment such as 5G communications, new energy vehicles and rail transportation. However, the processing efficiency and manufacturing cost of single-crystal silicon carbide wafers limit the further application and promotion of SiC-based power devices in related fields. At present, chemical mechanical polishing (CMP) technology is the only technology recognized by the global integrated circuit field to achieve substrate flattening processing. In the processing of semiconductor substrates, the CMP process is mainly divided into single-sided polishing process and double-sided simultaneous polishing process.

[0003] In order to improve the processing efficiency of silicon carbide, the double-sided synchronous polishing process is often used in current industrial production to process silicon carbide wafers. However, since the production of silicon carbide devices is completed on the Si surface, the processing requirements for the Si surface of the silicon carbide wafer are much higher than those for the C surface. Due to the anisotropy of the SiC crystal, the material removal rate of the C surface is much higher than that of the Si surface, and the removal rate ratio reaches about 3:1. However, in CMP, in order to remove the scratches introduced by the previous processing technology on the Si surface, the removal amount of the Si surface generally needs to reach 2-3um, which means that the removal amount of the C surface reaches 5-10um. Therefore, the current double-sided synchronous polishing process has the disadvantage of high processing loss. Summary of the invention

[0004] The purpose of the present invention is to solve the problems in the prior art and to provide a method for synchronously polishing double sides of a silicon carbide wafer.

[0005] To achieve the above object, the present invention proposes a method for synchronously polishing double sides of a silicon carbide wafer, comprising the following steps:

[0006] Providing cleaned silicon carbide wafers;

[0007] Pre-treating the silicon carbide wafer using a pre-treatment mixture containing a surfactant, by simultaneously changing the hydrophilicity of the carbon surface and the silicon surface of the silicon carbide wafer, and simultaneously changing the contact angle between the subsequent polishing liquid and the carbon surface and the contact angle between the polishing liquid and the silicon surface, so that the removal rate ratio between the carbon surface and the silicon surface of the silicon carbide wafer during double-sided simultaneous polishing is reduced;

[0008] The pretreated silicon carbide wafer is polished on both sides simultaneously using a polishing liquid to form a polished silicon carbide wafer.

[0009] Optionally, by changing the hydrophilicity of the silicon side and the carbon side of the silicon carbide wafer,

[0010] By reducing the hydrophilicity, the contact angle between the polishing liquid and the carbon surface is increased while the contact angle between the polishing liquid and the silicon surface remains almost unchanged; or the contact angle between the polishing liquid and the carbon surface is increased while the contact angle between the polishing liquid and the silicon surface is increased, but the removal rate ratio between the carbon surface and the silicon surface of the silicon carbide wafer during double-sided simultaneous polishing is reduced;

[0011] Alternatively, by increasing the hydrophilicity, the contact angle between the polishing liquid and the carbon surface is kept almost unchanged while the contact angle between the polishing liquid and the silicon surface is reduced; or the contact angle between the polishing liquid and the carbon surface is reduced while the contact angle between the polishing liquid and the silicon surface is reduced, but the removal rate ratio between the carbon surface and the silicon surface of the silicon carbide wafer during double-sided simultaneous polishing is reduced.

[0012] Optionally, by changing the hydrophilicity of the carbon surface and the silicon surface of the silicon carbide wafer, the ratio of the subsequent contact angle between the polishing liquid and the carbon surface to the contact angle between the polishing liquid and the silicon surface is increased, thereby reducing the removal rate ratio of the carbon surface and the silicon surface of the silicon carbide wafer during double-sided simultaneous polishing.

[0013] Optionally, the surfactant includes a wetting agent and a film-forming agent, wherein the wetting agent includes one or more of sodium dodecyl sulfate, hexadecyltrimethylammonium bromide, and sodium hexametaphosphate; the film-forming agent includes one or more of triethanolamine oleate soap nonylphenol polyoxyethylene ether, Tween 80, polyvinyl pyrrolidone, triethanolamine oleate, polyethyleneimine, and polyether-modified polyheptamethyltrisiloxane.

[0014] Optionally, the pretreatment mixed solution is a mixed aqueous solution of 0.015wt.% hexadecyltrimethylammonium bromide and 0.005wt.% polyvinylpyrrolidone, or a mixed aqueous solution of 0.005wt.% polyether-modified polyheptamethyltrisiloxane and 0.02wt.% sodium hexametaphosphate.

[0015] Optionally, the pretreatment mixed solution includes a surfactant and water, wherein the solid content of the surfactant is in the range of 0.005wt.%-0.03wt.%.

[0016] Optionally, the specific steps of pre-treating the silicon carbide wafer include:

[0017] Spraying a pretreatment mixture on the surface of the silicon carbide wafer;

[0018] After the spraying is uniform, the silicon carbide wafer is immersed in a container containing a pretreatment mixed liquid;

[0019] Rinse with deionized water.

[0020] Optionally, before pretreatment, the step of cleaning the silicon carbide wafer includes:

[0021] Cleaning the silicon carbide wafer with a mixture of ammonium hydroxide and hydrogen peroxide, and rinsing the silicon carbide wafer with deionized water;

[0022] The silicon carbide wafer is cleaned with a mixture of hydrochloric acid and hydrogen peroxide, and the silicon carbide wafer is rinsed with deionized water.

[0023] Optionally, the polishing liquid is a double-sided synchronous polishing liquid, and the double-sided synchronous polishing liquid is one or more of a silica sol polishing liquid, a manganese dioxide polishing liquid, a silicon dioxide polishing liquid, and an aluminum oxide polishing liquid.

[0024] Optionally, the double-sided synchronous polishing process is as follows: the upper plate speed of the polishing plate is 45rpm-55rpm; the lower plate speed of the polishing plate is 45rpm-55rpm; the inlet flow rate of the polishing liquid is 80mL / min-120mL / min; the surface temperature of the polishing plate is 40℃-45℃; the polishing pressure is 300g / cm 2 -400g / cm 2 The polishing liquid adopts silica sol polishing liquid, wherein the solid content of the silica sol is 25wt.%-35wt.%; the pH value is 8-10; and the oxidant concentration is 5wt.%-10wt.%.

[0025] Beneficial effects of the present invention:

[0026] When the double-sided synchronous polishing method of the silicon carbide wafer of the present invention is used to perform double-sided synchronous polishing of the silicon carbide wafer, the hydrophilicity of the carbon surface and the silicon surface of the silicon carbide wafer is changed simultaneously, and the contact angle between the subsequent polishing liquid and the carbon surface and the contact angle between the polishing liquid and the silicon surface are changed simultaneously, so that the removal rate ratio of the carbon surface and the silicon surface of the silicon carbide wafer during double-sided synchronous polishing is reduced. Although the removal rate of the Si surface is reduced, the C / Si surface removal rate ratio is reduced, the processing loss of the silicon carbide wafer is reduced, and the use requirements of device manufacturing are met while reducing the processing loss and processing cost.

[0027] The features and advantages of the present invention will be described in detail through embodiments in conjunction with the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 It is a flow chart of a method for synchronously polishing double sides of a silicon carbide wafer according to an embodiment of the present invention. DETAILED DESCRIPTION

[0029] In order to make the purpose, technical solutions and advantages of the embodiments of the present application clearer, the technical solutions in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application.

[0030] The present invention is described in detail below in conjunction with the accompanying drawings.

[0031] The embodiment of the present invention provides a method for synchronously polishing double-sided silicon carbide wafers. Figure 1 , including the following steps:

[0032] Step S10, providing a cleaned silicon carbide wafer;

[0033] Step S20, pretreating the silicon carbide wafer using a pretreatment mixture containing a surfactant, by simultaneously changing the hydrophilicity of the carbon surface and the silicon surface of the silicon carbide wafer, and simultaneously changing the contact angle between the subsequent polishing liquid and the carbon surface and the contact angle between the polishing liquid and the silicon surface, so that the removal rate ratio of the carbon surface and the silicon surface of the silicon carbide wafer during double-sided simultaneous polishing is reduced;

[0034] Step S30, using a polishing liquid to perform double-sided synchronous polishing on the pretreated silicon carbide wafer to form a polished silicon carbide wafer.

[0035] Specifically, in step S10, before pretreatment, the step of cleaning the silicon carbide wafer includes:

[0036] First, a mixture of ammonium hydroxide and hydrogen peroxide is used to clean the silicon carbide wafer. The specific steps are: prepare a mixed solution according to the concentration ratio of ammonium hydroxide: hydrogen peroxide: water of 1:1:5-1:2:5, introduce it into the cleaning tank, and heat it to 60-80°C; then put the silicon carbide wafer to be processed into the cleaning tank, soak it for 10-15 minutes under the action of ultrasonic vibration, and then take it out; then, rinse the silicon carbide wafer to be processed with deionized water. The mixed solution of ammonium hydroxide and hydrogen peroxide is used to remove the particles and organic matter remaining on the surface of the silicon carbide wafer during the pre-processing process, so as to provide a clean silicon carbide wafer surface for subsequent pre-treatment mixed solution treatment.

[0037] Secondly, a mixture of hydrochloric acid and hydrogen peroxide is used to clean the silicon carbide wafer. The specific steps are: prepare a mixed solution according to the concentration ratio of hydrochloric acid: hydrogen peroxide: water of 1:1:5-1:1:6, introduce it into the cleaning tank, and heat it to 60℃-80℃; then put the wafer to be processed into the above cleaning tank, soak it for 10-15 minutes under the action of ultrasonic vibration, and then take it out; then, rinse the silicon carbide wafer with deionized water. The mixture of hydrochloric acid and hydrogen peroxide is used to remove the metal contamination left on the wafer surface during the previous processing process, so as to provide a clean wafer surface for subsequent pre-treatment mixed solution treatment.

[0038] Specifically, please refer to step S20, use a pretreatment mixture containing a surfactant to pretreat the silicon carbide wafer, by simultaneously changing the hydrophilicity of the carbon surface and the silicon surface of the silicon carbide wafer, and simultaneously changing the contact angle between the subsequent polishing liquid and the carbon surface and the contact angle between the polishing liquid and the silicon surface, so that the removal rate ratio of the carbon surface and the silicon surface of the silicon carbide wafer during double-sided simultaneous polishing is reduced.

[0039] The specific steps for pre-processing silicon carbide wafers include:

[0040] Spraying a pretreatment mixture on the surface of the silicon carbide wafer;

[0041] After the spraying is uniform, the silicon carbide wafer is immersed in a container containing a pretreatment mixed liquid;

[0042] Rinse with deionized water.

[0043] Specifically, at 20°C-25°C, spray the pretreatment mixture on the surface of a rotating silicon carbide wafer; after spraying evenly, immerse the wafer in a quartz cylinder filled with the pretreatment mixture at 50°C-60°C for 3-5 minutes and then take it out; then, rinse it with deionized water.

[0044] In this embodiment, the pretreatment mixed liquid includes a surfactant and water, and the surfactant includes a wetting agent and a film-forming agent, wherein the wetting agent includes one or more of sodium dodecyl sulfate, hexadecyltrimethylammonium bromide, and sodium hexametaphosphate; the film-forming agent includes one or more of triethanolamine oleate soap nonylphenol polyoxyethylene ether, Tween 80, polyvinyl pyrrolidone, triethanolamine oleate, polyethyleneimine, and polyether modified polyheptamethyltrisiloxane, wherein the solid content of the surfactant ranges from 0.005wt.% to 0.03wt.%.

[0045] In one embodiment, the pretreatment mixed solution is a mixed aqueous solution of 0.015 wt.% hexadecyltrimethylammonium bromide and 0.005 wt.% polyvinylpyrrolidone.

[0046] In another embodiment, the pretreatment mixed solution is a mixed aqueous solution of 0.005 wt.% polyether-modified polyheptamethyltrisiloxane and 0.02 wt.% sodium hexametaphosphate.

[0047] In an embodiment of the present invention, by reducing the hydrophilicity, the contact angle between the polishing liquid and the carbon surface is increased while the contact angle between the polishing liquid and the silicon surface remains almost unchanged; or the contact angle between the polishing liquid and the carbon surface is increased while the contact angle between the polishing liquid and the silicon surface is increased, but the removal rate ratio of the carbon surface and the silicon surface of the silicon carbide wafer during double-sided simultaneous polishing is reduced.

[0048] Wherein, please refer to Table 1 and Table 2. When the pretreatment mixed liquid is a mixed aqueous solution of 0.015wt.% hexadecyltrimethylammonium bromide and 0.005wt.% polyvinylpyrrolidone, the contact angle between the polishing liquid and the carbon surface becomes 52.0°, and the contact angle between the polishing liquid and the silicon surface becomes 31.4°, so that the removal rate of the carbon surface using the silica sol polishing liquid is 257.5nm / h, and the removal rate of the silicon surface is 114.9nm / h. The removal rate ratio of the carbon surface and the silicon surface of the silicon carbide wafer during double-sided simultaneous polishing is 2.24.

[0049] When the pretreatment mixed liquid is a mixed aqueous solution of 0.005wt.% polyether modified polyheptamethyltrisiloxane and 0.02wt.% sodium hexametaphosphate, the contact angle between the polishing liquid and the carbon surface becomes 46.3°, and the contact angle between the polishing liquid and the silicon surface becomes 34.0°, so that the removal rate of the carbon surface using the silica sol polishing liquid is 304.5nm / h, and the removal rate of the silicon surface is 103.4nm / h. The removal rate ratio of the carbon surface and the silicon surface of the silicon carbide wafer during double-sided simultaneous polishing is 2.94.

[0050] Comparative Example:

[0051] When the pretreatment mixed liquid is deionized water, the contact angle between the polishing liquid and the carbon surface becomes 42.1°, and the contact angle between the polishing liquid and the silicon surface becomes 25.3°, so that the removal rate of the carbon surface using the silica sol polishing liquid is 401.8nm / h, and the removal rate of the silicon surface is 121.4nm / h. The removal rate ratio of the carbon surface and the silicon surface of the silicon carbide wafer during double-sided simultaneous polishing is 3.31.

[0052] Table 1

[0053] Preprocessing Carbon contact angle Silicon contact angle Deionized water spray, as the control group 42.1° 25.3° A mixture of 0.015wt.% hexadecyltrimethylammonium bromide and 0.005wt.% polyvinylpyrrolidone 52.0° 31.4° A solution of 0.005wt.% polyether-modified polyheptamethyltrisiloxane and 0.02wt.% sodium hexametaphosphate 46.3° 34.0°

[0054] Table 2

[0055]

[0056] The larger the contact angle between the polishing liquid and the wafer surface, the lower the material removal rate tends to decrease; the smaller the contact angle, the higher the material removal rate tends to increase, that is, the contact angle is negatively correlated with the material removal rate of the wafer. On the other hand, the contact angle between the polishing liquid and the wafer surface is negatively correlated with the hydrophilicity of the wafer surface, that is, the higher the hydrophilicity of the wafer surface, the lower the contact angle. Therefore, for the same polishing liquid, the higher the hydrophilicity of the wafer surface, the higher the material removal rate, and the lower the hydrophilicity of the wafer surface, the lower the material removal rate. In addition, the surface hydrophilicity of the carbon surface and the silicon surface of the silicon carbide wafer are different, and after being treated with a surfactant, the degree of change in the surface hydrophilicity of the carbon surface and the silicon surface of the silicon carbide wafer is inconsistent. By reasonably selecting a suitable surfactant, the hydrophilicity of the carbon surface and the silicon surface of the silicon carbide wafer are changed at the same time, and the contact angle between the subsequent polishing liquid and the carbon surface and the contact angle between the polishing liquid and the silicon surface are changed at the same time, so that the removal rate ratio of the carbon surface and the silicon surface of the silicon carbide wafer during double-sided synchronous polishing decreases.

[0057] In the above embodiment, by reducing the hydrophilicity of the silicon carbide wafer surface, the contact angle between the polishing liquid and the carbon surface is increased, and at the same time, the contact angle between the polishing liquid and the silicon surface is increased, but the removal rate ratio between the carbon surface and the silicon surface of the silicon carbide wafer during double-sided simultaneous polishing decreases.

[0058] In one of the embodiments, by changing the hydrophilicity of the carbon surface and the silicon surface of the silicon carbide wafer, the ratio of the contact angle between the subsequent polishing liquid and the carbon surface to the contact angle between the polishing liquid and the silicon surface is increased, thereby reducing the removal rate ratio of the carbon surface and the silicon surface of the silicon carbide wafer during double-sided simultaneous polishing.

[0059] In other embodiments, by improving the hydrophilicity, the contact angle between the polishing liquid and the carbon surface is kept almost unchanged while the contact angle between the polishing liquid and the silicon surface is reduced; or the contact angle between the polishing liquid and the carbon surface is reduced while the contact angle between the polishing liquid and the silicon surface is reduced, but the removal rate ratio of the carbon surface and the silicon surface of the silicon carbide wafer during double-sided simultaneous polishing is reduced.

[0060] In this embodiment, since the step of pretreating the two surfaces of the silicon carbide wafer and the step of double-sided simultaneous polishing are performed separately and independently, the ratio of the pretreatment mixed liquid does not need to consider the specific formula of the polishing liquid. After the pretreatment is performed with the pretreatment mixed liquid, no matter whether any existing polishing liquid or newly developed polishing liquid is used, the removal rate ratio of the carbon surface and the silicon surface of the silicon carbide wafer during double-sided simultaneous polishing can be reduced, thereby reducing the processing loss of the silicon carbide wafer. In addition, the present invention is suitable for using existing polishing liquids, which is beneficial to reducing polishing costs.

[0061] Since the steps of pre-treating the two surfaces of the silicon carbide wafer and the step of double-sided simultaneous polishing are performed separately and independently, in other embodiments, after pre-treating the two surfaces of the silicon carbide wafer, the contact angles of the carbon surface and the silicon surface of the silicon carbide wafer can also be detected to determine whether the pre-treatment meets the expected requirements and whether rework and re-pre-treatment are required.

[0062] In addition, in the step of pretreating the two surfaces of the silicon carbide wafer of the present invention, the pretreatment mixture is first sprayed on the surface of the rotating silicon carbide wafer at 20°C-25°C; after being evenly sprayed, the above wafer is immersed in a quartz cylinder filled with the pretreatment mixture, and is taken out after being immersed at 50°C-60°C for 3-5 minutes, so that the pretreatment mixture fully infiltrates the two surfaces of the silicon carbide wafer, so that during the entire double-sided synchronous polishing process, the contact angles between the polishing liquid and the carbon surface and the silicon surface remain basically unchanged.

[0063] Step S30 is executed to perform double-sided synchronous polishing on the pretreated silicon carbide wafer using a polishing liquid to form a polished silicon carbide wafer.

[0064] The polishing liquid is a double-sided synchronous polishing liquid, and the double-sided synchronous polishing liquid is one or more of silica sol polishing liquid, manganese dioxide polishing liquid, silicon dioxide polishing liquid, and aluminum oxide polishing liquid.

[0065] In other embodiments, the polishing liquid may also adopt existing polishing liquid to reduce the polishing cost.

[0066] In one embodiment, the polishing liquid adopts silica sol polishing liquid, and the double-sided synchronous polishing process is as follows: the upper plate speed of the polishing disk is 45rpm-55rpm; the lower plate speed of the polishing disk is 45rpm-55rpm; the liquid inlet flow rate of the polishing liquid is 80mL / min-120mL / min; the disk surface temperature of the polishing disk is 40℃-45℃; the polishing pressure is 300g / cm 2 -400g / cm 2 , wherein the solid content of the silica sol is 25wt.%-35wt.%; the pH value is 8-10; and the oxidant concentration is 5wt.%-10wt.%.

[0067] In another embodiment, the polishing process conditions set when using manganese dioxide polishing liquid to perform double-sided synchronous polishing on silicon carbide wafers are as follows: polishing liquid flow rate is 150mL / min-300mL / min, polishing disk speed is 40rpm-80rpm, polishing head speed is 40rpm-80rpm, polishing head swing is 10mm-15mm, polishing pressure is 2.5psi-4psi, polishing temperature is 28℃-35℃, and the pH of the polishing liquid is 8-10.5. The use of the manganese dioxide polishing liquid can further reduce the removal rate ratio of the carbon surface and the silicon surface of the silicon carbide wafer during double-sided synchronous polishing to less than 2.

[0068] The manganese dioxide polishing liquid is composed of the following ingredients in weight percentage: manganese dioxide powder 0.5wt.%-20wt.%, oxidant 0.2wt.%-5wt.%, dispersant 0.1wt.%-5wt.%, wetting agent 0.2wt.%-8wt.%, pH regulator 0.2wt.%-2wt.%, and deionized water as the balance. The oxidant is one or more of potassium perchlorate, potassium permanganate, potassium periodate, and potassium persulfate, the pH regulator is one or more of potassium hydroxide, sodium hydroxide, ammonia water, tetramethylammonium hydroxide, dilute phosphoric acid, citric acid, and dilute hydrochloric acid, the wetting agent is one or more of ethanol, hydroxyethyl cellulose, polycarboxylates, succinates, and polycarboxylic acid type comb copolymer surfactants, and the dispersant is a polymer surfactant, which includes at least one of glycolipid surfactants, lipopeptide surfactants, and phospholipid surfactants.

[0069] The particle size of the manganese dioxide particles does not exceed 300 nm and is highly monodisperse. The particle size dispersion index (PDI) value of the manganese dioxide with high monodispersity is less than 0.1.

[0070] In this embodiment, after the silicon carbide wafer is pretreated, a double-sided polishing process is used to simultaneously polish the double sides of the pretreated silicon carbide wafer.

[0071] In other embodiments, the pretreated silicon carbide wafer may be polished on both sides simultaneously by using a double-sided polishing process of rough polishing and fine polishing.

[0072] The above embodiments are intended to illustrate the present invention, not to limit the present invention. Any solution that is a simple transformation of the present invention belongs to the protection scope of the present invention.

Claims

1. A method for synchronously polishing double sides of a silicon carbide wafer, characterized in that: The following steps are involved: Providing cleaned silicon carbide wafers; Pre-treating the silicon carbide wafer using a pre-treatment mixture containing a surfactant, by simultaneously changing the hydrophilicity of the carbon surface and the silicon surface of the silicon carbide wafer, and simultaneously changing the contact angle between the subsequent polishing liquid and the carbon surface and the contact angle between the polishing liquid and the silicon surface, so that the removal rate ratio of the carbon surface and the silicon surface of the silicon carbide wafer during double-sided simultaneous polishing is reduced, and the silicon carbide wafer is rinsed with deionized water; The silicon carbide wafer rinsed with deionized water is polished on both sides simultaneously using a polishing liquid to form a polished silicon carbide wafer.

2. The method for synchronously polishing double sides of a silicon carbide wafer according to claim 1, characterized in that: By changing the hydrophilicity of the silicon and carbon surfaces of the silicon carbide wafer, By reducing the hydrophilicity, the contact angle between the polishing liquid and the carbon surface is increased while the contact angle between the polishing liquid and the silicon surface remains almost unchanged; or the contact angle between the polishing liquid and the carbon surface is increased while the contact angle between the polishing liquid and the silicon surface is increased, but the removal rate ratio between the carbon surface and the silicon surface of the silicon carbide wafer during double-sided simultaneous polishing is reduced; Alternatively, by increasing the hydrophilicity, the contact angle between the polishing liquid and the carbon surface is kept almost unchanged while the contact angle between the polishing liquid and the silicon surface is reduced; or the contact angle between the polishing liquid and the carbon surface is reduced while the contact angle between the polishing liquid and the silicon surface is reduced, but the removal rate ratio between the carbon surface and the silicon surface of the silicon carbide wafer during double-sided simultaneous polishing is reduced.

3. The method for synchronously polishing double sides of a silicon carbide wafer according to claim 1, characterized in that: By changing the hydrophilicity of the carbon surface and the silicon surface of the silicon carbide wafer, the ratio of the contact angle between the subsequent polishing liquid and the carbon surface to the contact angle between the polishing liquid and the silicon surface is increased, thereby reducing the removal rate ratio of the carbon surface and the silicon surface of the silicon carbide wafer during double-sided simultaneous polishing.

4. The method for synchronously polishing double sides of a silicon carbide wafer according to claim 1, characterized in that: The surfactant includes a wetting agent and a film-forming agent, wherein the wetting agent includes one or more of sodium dodecyl sulfate, hexadecyltrimethylammonium bromide, and sodium hexametaphosphate; the film-forming agent includes one or more of triethanolamine oleate soap nonylphenol polyoxyethylene ether, Tween 80, polyvinyl pyrrolidone, triethanolamine oleate, polyethyleneimine, and polyether-modified polyheptamethyltrisiloxane.

5. The method for synchronously polishing double sides of a silicon carbide wafer according to claim 4, characterized in that: The pretreatment mixed solution is a mixed aqueous solution of 0.015wt.% hexadecyltrimethylammonium bromide and 0.005wt.% polyvinylpyrrolidone, or a mixed aqueous solution of 0.005wt.% polyether-modified polyheptamethyltrisiloxane and 0.02wt.% sodium hexametaphosphate.

6. The method for synchronously polishing double sides of a silicon carbide wafer according to claim 4, characterized in that: The pretreatment mixed solution includes a surfactant and water, wherein the solid content of the surfactant is in the range of 0.005wt.%-0.03wt.%.

7. The method for synchronously polishing double sides of a silicon carbide wafer according to claim 1, characterized in that: The specific steps for pre-processing silicon carbide wafers include: Spraying a pretreatment mixture on the surface of the silicon carbide wafer; After the spraying is uniform, the silicon carbide wafer is immersed in a container containing the pretreatment mixed liquid.

8. The method for synchronously polishing double sides of a silicon carbide wafer according to claim 1, characterized in that: Before pretreatment, the steps for cleaning the silicon carbide wafer include: Cleaning the silicon carbide wafer with a mixture of ammonium hydroxide and hydrogen peroxide, and rinsing the silicon carbide wafer with deionized water; The silicon carbide wafer is cleaned with a mixture of hydrochloric acid and hydrogen peroxide, and the silicon carbide wafer is rinsed with deionized water.

9. The method for synchronously polishing double sides of a silicon carbide wafer according to claim 1, characterized in that: The polishing liquid is a double-sided synchronous polishing liquid, and the double-sided synchronous polishing liquid is one or more of silica sol polishing liquid, manganese dioxide polishing liquid, silicon dioxide polishing liquid, and aluminum oxide polishing liquid.

10. The method for synchronously polishing double sides of a silicon carbide wafer according to claim 1, characterized in that: The double-sided synchronous polishing process is as follows: the upper plate speed of the polishing plate is 45rpm-55rpm; the lower plate speed of the polishing plate is 45rpm-55rpm; the inlet flow rate of the polishing liquid is 80mL / min-120mL / min; the surface temperature of the polishing plate is 40℃-45℃; the polishing pressure is 300g / cm 2 -400g / cm 2 The polishing liquid adopts silica sol polishing liquid, wherein the solid content of the silica sol is 25wt.%-35wt.%; the pH value is 8-10; and the oxidant concentration is 5wt.%-10wt.%.