Preparation method of modified polyurethane finishing agent
By preparing a modified polyurethane finishing agent containing hydroxyl cationic butyric acid amide-terminated polysiloxane and isophorone diisocyanate, the problem of insufficient hydrophilicity and antibacterial properties of textiles is solved, and high softness of textiles is achieved , anti-wrinkle and antibacterial properties.
Patent Information
- Application Number
- CN202410969527.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-07-19
AI Technical Summary
In the existing technology, while polyurethane finishing agents improve the softness and anti-wrinkle properties of textiles, their hydrophilicity and hygroscopicity decrease, and they lack antibacterial properties.
By preparing a modified polyurethane finishing agent containing hydroxycationic butyric acid amide-terminated polysiloxane and isophorone diisocyanate, carboxyl and quaternary ammonium salt cationic groups are used to improve the hydrophilicity and antibacterial properties of textiles, and through Reaction of polyether polyol and dibutyltin dilaurate to enhance flexible polysiloxane segments for textile finishing.
The finished cotton fabric maintains good softness, anti-wrinkle performance and hydrophilicity, and also has excellent antibacterial properties. The sharp elastic wrinkle recovery angle and slow elastic wrinkle recovery angle are significantly improved, the breaking strength retention rate is high, the water droplet diffusion time is moderate, and it can Effectively inhibits bacterial growth.
Smart Images

Figure QLYQS_1 
Figure SMS_5 
Figure SMS_6
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polyurethane, in particular to a method for preparing a modified polyurethane finishing agent. Background Art
[0002] Finishing agent is a common auxiliary agent for textile fabrics, mainly including polyurethane finishing agent, silicone finishing agent, polyether finishing agent, etc. Among them, polyurethane finishing agent has good film-forming property, excellent wear resistance, strong hygroscopicity, and is widely used in cotton fabrics, polyester, nylon and other textile fabrics, which can improve the fabric's feel, softness, hydrophilicity and hygroscopicity and other properties.
[0003] By copolymerizing and grafting polyurethane finishing agents with hydroxyl polysiloxane, amino polysiloxane, etc., flexible polysiloxane molecular chains can be introduced into the finishing agent, which is beneficial to improving the softness, feel, wrinkle resistance and other properties of the fabric. However, polysiloxane is hydrophobic, and after finishing, the hydrophilicity and hygroscopicity of the fabric surface will be reduced. Introducing hydrophilic groups such as carboxyl and sulfonic acid into polyurethane finishing agents can make the finishing agent and fabric have good hydrophilic properties. The patent with the authorization announcement number CN106948178B discloses an organosilicon-modified polyurethane anti-pilling finishing agent, a preparation method and an application thereof. The organosilicon-modified polyurethane anti-pilling finishing agent prepared by using double-terminal amino silicone oil, isophorone diisocyanate, polyethylene glycol, diethylene glycol, N-methyldiethanolamine, etc. as raw materials can improve the problems of fabric fuzzing and pilling. However, the polyurethane finishing agent of the patent does not give the fabric good antibacterial properties. Summary of the invention
[0004] The invention provides a method for preparing a modified polyurethane finishing agent, which solves the problem that the prior art organic silicon polyurethane finishing agent has poor hydrophilicity and lacks antibacterial performance.
[0005] A method for preparing a modified polyurethane finishing agent, the method comprising:
[0006] Step S1, add isopropanol, 2-(trimethylethylenediamine)-4,6-di(butyric acid amide)-1,3,5-triazine and hydrochloric acid solution to a reaction bottle equipped with a condenser reflux tube, stir for 1-2 hours, then add glycidoxypropyl-terminated polydimethylsiloxane, concentrate the solution after the reaction, add water, stand for stratification, remove the aqueous phase, and dry to obtain hydroxycationic butyric acid amide-terminated polysiloxane.
[0007] The structural formula of 2-(trimethylethylenediamine)-4,6-di(butyric acid amide)-1,3,5-triazine is formula (I):
[0008] Formula (I).
[0009] Step S2, add polyether polyol to the reaction bottle, vacuum dry and dehydrate, pass nitrogen into the reaction bottle, add isophorone diisocyanate, carry out a primary reaction, then add acetone, hydroxycation butyric acid amide-terminated polysiloxane, and dibutyltin dilaurate, carry out a secondary reaction, add triethylamine to neutralize and form a salt, concentrate the solution to remove acetone, add water, stir and mix, and obtain a modified polyurethane finishing agent.
[0010] Furthermore, in step S1, the molar ratio of 2-(trimethylethylenediamine)-4,6-di(butyric acid amide)-1,3,5-triazine to glycidoxypropyl terminated polydimethylsiloxane is (2-2.4):1.
[0011] Furthermore, in step S1, the molar concentration of the hydrochloric acid solution is 10-12 mol / L.
[0012] Furthermore, in step S1, the reaction temperature is 75-85° C. and the reaction time is 6-12 h.
[0013] Furthermore, in step S2, the molar ratio of polyether polyol, isophorone diisocyanate and glycidoxypropyl-terminated polydimethylsiloxane is 1:(2.6-2.8):(1.2-1.5), and the polyether polyol is polyethylene glycol or polypropylene glycol.
[0014] Furthermore, in step S2, the temperature of the primary reaction is 65-75°C, and the reaction time is 2-3h; the temperature of the secondary reaction is 40-50°C, and the reaction time is 40-60min.
[0015] Further, the preparation method of the 2-(trimethylethylenediamine)-4,6-di(butyric acid amide)-1,3,5-triazine is:
[0016] Step (1), adding N,N-dimethylformamide, 2-chloro-4,6-diamino-1,3,5-triazine, N,N,N'-trimethylethylenediamine and potassium carbonate in a molar ratio of 1:(0.9-1.1):(1-1.1) to a reaction flask, introducing nitrogen, heating to 120-140°C, reacting for 18-36 hours, adding water after the reaction, mixing and extracting with dichloromethane, separating and obtaining an organic phase, drying and removing water, and recrystallizing the crude product with dichloromethane to obtain 2-(trimethylethylenediamine)-4,6-diamino-1,3,5-triazine;
[0017] Step (2), add N,N-dimethylformamide, 2-(trimethylethylenediamine)-4,6-diamino-1,3,5-triazine and succinic anhydride in a molar ratio of 1:(2.4-2.8) to a reaction bottle, react at 25-40° C. for 2-5 hours, add water after the reaction, mix well and extract with dichloromethane, separate the organic phase, dry and remove water, and recrystallize the crude product with ethanol to obtain 2-(trimethylethylenediamine)-4,6-di(butyric acid amide)-1,3,5-triazine.
[0018] Reaction mechanism: In the present invention, 2-chloro-4,6-diamino-1,3,5-triazine and N,N,N'-trimethylethylenediamine are subjected to substitution reaction, and then reacted with succinic anhydride to obtain 2-(trimethylethylenediamine)-4,6-diamino-1,3,5-triazine, and its N,N-dimethyl tertiary amine group with less steric hindrance undergoes a ring-opening reaction with the terminal epoxy group of glycidoxypropyl-terminated polydimethylsiloxane to obtain hydroxyl cationic butyric acid amide-terminated polysiloxane, thereby introducing hydroxyl, carboxyl and quaternary ammonium salt cationic groups into the terminal groups of the polysiloxane.
[0019] Beneficial effects: The present invention polymerizes polyether polyol, isophorone diisocyanate and hydroxyl cationic butyric acid amide-terminated polysiloxane to obtain a novel modified polyurethane finishing agent containing carboxyl and quaternary ammonium salt cationic groups. Then, cotton fabric is finished. The modified polyurethane finishing agent contains a flexible polysiloxane segment. The quick-elastic wrinkle recovery angle of the finished cotton fabric reaches 183.0-191.2°, and the slow-elastic wrinkle recovery angle reaches 228.8-240.3°, with good softness and wrinkle resistance. In addition, the cotton fabric maintains a good breaking strength, and the retention rate reaches 90.83-93.01%.
[0020] The modified polyurethane finishing agent of the present invention contains a large number of hydrophilic carboxyl groups, quaternary ammonium salt cations and other groups, and the water drop diffusion time of the cotton fabric after finishing is 3.2-4.1 seconds, so that the cotton fabric still maintains good hydrophilicity. In addition, the organosilicon quaternary ammonium salt structure in the main chain of the modified polyurethane finishing agent molecule has a strong bactericidal effect, can effectively inhibit the metabolic process and growth of bacteria, and endow the cotton fabric with excellent antibacterial properties. DETAILED DESCRIPTION
[0021] It should be noted that the following detailed descriptions are exemplary and are intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs.
[0022] The glycidoxypropyl terminated polydimethylsiloxane of the present invention has a molecular weight of 1000 and a content of 98%, and is produced by Wuhan Lanabai Pharmaceutical Chemicals. The hydroxyl terminated polydimethylsiloxane has a viscosity of 1500 and a content of 98%, and is produced by Wuhan Lanabai Pharmaceutical Chemicals.
[0023] Embodiment 1: A method for preparing a modified polyurethane finishing agent, comprising:
[0024] (1) Add 400 mL of N,N-dimethylformamide, 40 mmol of 2-chloro-4,6-diamino-1,3,5-triazine, 36 mmol of N,N,N'-trimethylethylenediamine, and 40 mmol of potassium carbonate to a reaction flask, introduce nitrogen, heat to 140°C, react for 18 hours, add water, mix well, extract with dichloromethane, separate the organic phase, dry and remove water, and recrystallize the crude product with dichloromethane to obtain 2-(trimethylethylenediamine)-4,6-diamino-1,3,5-triazine. Reaction formula:
[0025] ;
[0026] (2) Add 100 mL of N,N-dimethylformamide, 40 mmol of 2-(trimethylethylenediamine)-4,6-diamino-1,3,5-triazine, and 96 mmol of succinic anhydride to the reaction flask, and react at 40°C for 2 h. After the reaction, add water, mix well, and extract with dichloromethane. Separate the organic phase, dry and remove water, and recrystallize the crude product with ethanol to obtain 2-(trimethylethylenediamine)-4,6-di(butyric acid amide)-1,3,5-triazine. Reaction formula:
[0027] ;
[0028] (3) Add 30 mL of isopropanol, 72 mmol of 2-(trimethylethylenediamine)-4,6-di(butyric acid amide)-1,3,5-triazine, and 7 mL of 12 mol / L hydrochloric acid solution to a reaction bottle equipped with a condenser reflux tube, stir for 1 hour, add 30 mmol of glycidoxypropyl-terminated polydimethylsiloxane, heat to 80°C, react for 12 hours, concentrate the solution, add water, let stand to separate, remove the aqueous phase, and dry to obtain hydroxycation butyric acid amide-terminated polysiloxane. Reaction formula:
[0029] ;
[0030] (4) Add 50 mmol of polyethylene glycol 2000 to the reaction flask, vacuum dry and dehydrate, introduce nitrogen into the reaction flask, add 136 mmol of isophorone diisocyanate, heat to 70°C, react for 2 h, then add 20 mL of acetone, 60 mmol of hydroxycationic butyric acid amide-terminated polysiloxane, and 0.7 g of dibutyltin dilaurate, react at 50°C for 40 min, add triethylamine to neutralize and form salt, concentrate the solution to remove acetone, add water to control the solid content of the solution to 4%, stir and mix to obtain a modified polyurethane finishing agent.
[0031] Embodiment 2: A method for preparing a modified polyurethane finishing agent, comprising:
[0032] (1) Add 500 mL of N,N-dimethylformamide, 40 mmol of 2-chloro-4,6-diamino-1,3,5-triazine, 44 mmol of N,N,N'-trimethylethylenediamine, and 44 mmol of potassium carbonate to a reaction flask, introduce nitrogen, raise the temperature to 120°C, react for 36 hours, add water, mix well, and extract with dichloromethane, separate the organic phase, dry and remove water, and recrystallize the crude product with dichloromethane to obtain 2-(trimethylethylenediamine)-4,6-diamino-1,3,5-triazine;
[0033] (2) Add 120 mL of N,N-dimethylformamide, 40 mmol of 2-(trimethylethylenediamine)-4,6-diamino-1,3,5-triazine, and 112 mmol of succinic anhydride to the reaction bottle, react at 25°C for 5 hours, add water after the reaction, mix well, extract with dichloromethane, separate the organic phase, dry and remove water, and recrystallize the crude product with ethanol to obtain 2-(trimethylethylenediamine)-4,6-di(butyric acid amide)-1,3,5-triazine;
[0034] (3) Add 20 mL of isopropanol, 60 mmol of 2-(trimethylethylenediamine)-4,6-di(butyric acid amide)-1,3,5-triazine, and 8 mL of a hydrochloric acid solution with a molar concentration of 10 mol / L to a reaction bottle equipped with a condenser reflux tube, stir for 2 h, add 30 mmol of glycidoxypropyl-terminated polydimethylsiloxane, heat to 85°C, react for 6 h, concentrate the solution, add water, stand for stratification, remove the aqueous phase, and dry to obtain a hydroxycationic butyric acid amide-terminated polysiloxane;
[0035] (4) Add 50 mmol of polypropylene glycol 2000 to the reaction flask, vacuum dry and dehydrate, introduce nitrogen into the reaction flask, add 130 mmol of isophorone diisocyanate, heat to 65°C, react for 3 h, then add 20 mL of acetone, 75 mmol of hydroxycationic butyric acid amide-terminated polysiloxane, and 0.8 g of dibutyltin dilaurate, react at 40°C for 60 min, add triethylamine to neutralize and form salt, concentrate the solution to remove acetone, add water to control the solid content of the solution to 4%, stir and mix well to obtain a modified polyurethane finishing agent.
[0036] Embodiment 3: A method for preparing a modified polyurethane finishing agent, comprising:
[0037] (1) Prepare 2-(trimethylethylenediamine)-4,6-di(butyric acid amide)-1,3,5-triazine according to the method of Example 1;
[0038] (2) Add 30 mL of isopropanol, 63 mmol of 2-(trimethylethylenediamine)-4,6-di(butyric acid amide)-1,3,5-triazine, and 7 mL of a hydrochloric acid solution with a molar concentration of 12 mol / L to a reaction bottle equipped with a condenser reflux tube, stir for 2 h, add 30 mmol of glycidoxypropyl-terminated polydimethylsiloxane, heat to 75°C, react for 12 h, concentrate the solution, add water, stand for stratification, remove the aqueous phase, and dry to obtain a hydroxycationic butyric acid amide-terminated polysiloxane;
[0039] (3) Add 50 mmol of polyethylene glycol 2000 to the reaction flask, vacuum dry and dehydrate, introduce nitrogen into the reaction flask, add 140 mmol of isophorone diisocyanate, heat to 65°C, react for 3 h, then add 20 mL of acetone, 65 mmol of hydroxycationic butyric acid amide-terminated polysiloxane, and 0.8 g of dibutyltin dilaurate, react at 45°C for 60 min, add triethylamine to neutralize and form salt, concentrate the solution to remove acetone, add water to control the solid content of the solution to 4%, stir and mix to obtain a modified polyurethane finishing agent.
[0040] Comparative Example 1: A method for preparing a modified polyurethane finishing agent, comprising:
[0041] (1) Prepare hydroxy-terminated polydimethylsiloxane according to the method of Example 1.
[0042] (2) Add 50 mmol of polyethylene glycol 2000 to the reaction flask, vacuum dry and dehydrate, introduce nitrogen into the reaction flask, add 136 mmol of isophorone diisocyanate, raise the temperature to 70°C, react for 2 hours, then add 20 mL of acetone, 60 mmol of hydroxyl-terminated polydimethylsiloxane, and 0.7 g of dibutyltin dilaurate, react at 50°C for 40 minutes, add triethylamine to neutralize and form salt, concentrate the solution to remove acetone, add water to control the solid content of the solution to 4%, stir and mix well to obtain a modified polyurethane finishing agent.
[0043] Comparative Example 2: A method for preparing a modified polyurethane finishing agent, comprising:
[0044] (1) Add 50 mmol of polyethylene glycol 2000 to a reaction flask, vacuum dry and dehydrate, introduce nitrogen into the reaction flask, add 136 mmol of isophorone diisocyanate, heat to 70°C, react for 2 h, then add 20 mL of acetone, 60 mmol of 2,2-dihydroxymethylpropionic acid, and 0.7 g of dibutyltin dilaurate, react at 50°C for 40 min, add triethylamine to neutralize and form salt, concentrate the solution to remove acetone, add water to control the solid content of the solution to 4%, stir and mix to obtain a modified polyurethane finishing agent.
[0045] The cotton fabric was treated with double dipping and double rolling using a modified polyurethane finishing agent, with a rolling rate of 90% and a bath ratio of 1:20. The cotton fabric was then pre-baked at 90°C for 2 min, baked at 160°C for 2 min, and dried at room temperature to obtain the finished cotton fabric.
[0046] The cotton fabric without finishing agent was used as blank control sample.
[0047] The wrinkle recovery angle of the finished cotton fabric was tested using an elastic recovery instrument according to the method of GB / T 3819-1997.
[0048] The test results are shown in Table 1.
[0049] Table 1: Test results of cotton fabric wrinkle recovery angle of each embodiment and comparative example
[0050]
[0051] The breaking strength of cotton fabrics was tested using an electronic fabric strength tester according to the GB / T 3923.1-2013 method. The breaking strength retention rate R was calculated as follows: R = (F 1 / F)×100%. F 1 is the breaking strength of cotton fabric after finishing with the finishing agent. F is the breaking strength of unfinished cotton fabric. The test results are shown in Table 2.
[0052] Table 2: Test results of breaking strength of cotton fabrics of various embodiments and comparative examples
[0053]
[0054] From the test results in Tables 1 and 2 above, it can be seen that the blank control cotton fabric has not been finished with a polyurethane finishing agent, and the quick-bounce wrinkle recovery angle is 122.8°, and the slow-bounce wrinkle recovery angle is 167.1°. The wrinkle recovery angle is low, and the softness and wrinkle resistance are poor. The breaking strength is 420.9N.
[0055] Example 1-Example 3 The modified polyurethane finishing agent containing flexible polysiloxane segments was used to finish the cotton fabric. The quick-elastic wrinkle recovery angle of the finished cotton fabric reached 183.0-191.2°, and the slow-elastic wrinkle recovery angle reached 228.8-240.3°. The larger the wrinkle recovery angle, the better the softness and wrinkle resistance. In addition, the cotton fabric maintained a good breaking strength, with a retention rate of 90.83-93.01%.
[0056] In comparative example 1, when preparing the polyurethane finishing agent, hydroxyl-terminated polydimethylsiloxane was added for polymerization reaction. The polyurethane finishing agent also contained flexible polysiloxane segments, and the sharp wrinkle recovery angle reached 180.7°, and the slow wrinkle recovery angle reached 238.6°. It had good softness and wrinkle resistance, and the breaking strength retention rate was 91.42%, with excellent mechanical properties.
[0057] Comparative Example 2 uses 2,2-dihydroxymethylpropionic acid as an aqueous chain extender, and the obtained polyurethane finishing agent does not contain flexible polysiloxane segments. The finished cotton fabric has low snap and slow crease recovery angles, poor softness and wrinkle resistance, and a breaking strength retention rate of only 81.35%, with a significant decrease in mechanical strength.
[0058] The hydrophilicity of cotton fabric was tested according to the AATCC79-2010 method. A drop of water was dropped on the surface of the cotton fabric, and the time for the water drop to completely diffuse to no mirror reflection was recorded. The test was repeated 5 times and the average value was taken. The test results are shown in Table 3.
[0059] Table 3: Test results of hydrophilicity of cotton fabrics in various embodiments and comparative examples
[0060]
[0061] After testing, the blank control cotton fabric itself has good hydrophilicity, and the water drop diffusion time is ≤ 1s. The modified polyurethane finishing agents of Examples 1 to 3 contain a large number of hydrophilic carboxyl groups, quaternary ammonium salt cations and other groups. The water drop diffusion time of the finished cotton fabric is 3.2-4.1s, and the cotton fabric still maintains good hydrophilicity.
[0062] The polyurethane finishing agent of Comparative Example 1 does not contain hydrophilic carboxyl groups, quaternary ammonium salt cations and other groups. The water drop diffusion time of the finished cotton fabric reaches 36.7s, and the hydrophilicity is significantly reduced.
[0063] The polyurethane finishing agent of Comparative Example 2 contains carboxyl hydrophilic groups, but does not contain hydrophilic groups such as quaternary ammonium salt cations, and the water droplet diffusion time is slightly longer than that of the embodiments.
[0064] According to the oscillation bottle method in GB / T 20944.3-2008, the antibacterial properties of cotton fabrics against Escherichia coli or Staphylococcus aureus were tested. t -Q t ) / Wt×100%. Q t The concentration of viable bacteria (cfu / mL) in the treated cotton fabric sample after 18 hours of oscillation contact. t The viable bacterial concentration (cfu / mL) of the unfinished cotton fabric blank control sample after 18 hours of oscillation contact. The test results are shown in Table 4.
[0065] Table 4: Test results of antibacterial properties of cotton fabrics of various embodiments and comparative examples
[0066]
[0067] After testing, after the modified polyurethane finishing agents of Examples 1 to 3 were used to finish cotton fabrics, the cotton fabrics showed a high antibacterial rate against Escherichia coli and Staphylococcus aureus. This is because the organosilicon quaternary ammonium salt structure in the main chain of the modified polyurethane finishing agent molecule has a strong bactericidal effect, which can effectively inhibit the metabolic process and growth of bacteria, and endow the cotton fabrics with excellent antibacterial properties.
[0068] The polyurethane finishing agents of Comparative Examples 1 and 2 do not contain organosilicon quaternary ammonium salt structures and do not impart good antibacterial properties to cotton fabrics.
[0069] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a modified polyurethane finishing agent, characterized in that: The preparation method comprises: Step S1, adding isopropanol, 2-(trimethylethylenediamine)-4,6-di(butyric acid amide)-1,3,5-triazine and hydrochloric acid solution to a reaction bottle equipped with a condenser reflux tube, stirring for 1-2 hours, adding glycidoxypropyl-terminated polydimethylsiloxane, concentrating the solution after the reaction, adding water, standing and stratifying, removing the aqueous phase, and drying to obtain hydroxycationic butyric acid amide-terminated polysiloxane; The structural formula of the 2-(trimethylethylenediamine)-4,6-di(butyric acid amide)-1,3,5-triazine is Formula (I): Formula (I); Step S2, adding polyether polyol to a reaction bottle, vacuum drying and dehydration, introducing nitrogen into the reaction bottle, adding isophorone diisocyanate, carrying out a primary reaction, then adding acetone, hydroxycationic butyric acid amide-terminated polysiloxane, and dibutyltin dilaurate, carrying out a secondary reaction, adding triethylamine to neutralize and form a salt, concentrating the solution to remove acetone, adding water, stirring and mixing, and obtaining a modified polyurethane finishing agent; In the step S2, the molar ratio of polyether polyol, isophorone diisocyanate and glycidoxypropyl-terminated polydimethylsiloxane is 1:(2.6-2.8):(1.2-1.5); the polyether polyol is polyethylene glycol or polypropylene glycol.
2. The method for preparing the modified polyurethane finishing agent according to claim 1, characterized in that: In the step S1, the molar ratio of 2-(trimethylethylenediamine)-4,6-di(butyric acid amide)-1,3,5-triazine to glycidoxypropyl terminated polydimethylsiloxane is (2-2.4):
1.
3. The method for preparing the modified polyurethane finishing agent according to claim 1, characterized in that: In step S1, the molar concentration of the hydrochloric acid solution is 10-12 mol / L.
4. The method for preparing the modified polyurethane finishing agent according to claim 1, characterized in that: In the step S1, the reaction temperature is 75-85° C. and the reaction time is 6-12 h.
5. The method for preparing the modified polyurethane finishing agent according to claim 1, characterized in that: In step S2, the temperature of the primary reaction is 65-75°C, and the reaction time is 2-3h; the temperature of the secondary reaction is 40-50°C, and the reaction time is 40-60min.
6. The method for preparing the modified polyurethane finishing agent according to claim 2, characterized in that: The preparation method of the 2-(trimethylethylenediamine)-4,6-di(butyric acid amide)-1,3,5-triazine is as follows: Step (1), adding N,N-dimethylformamide, 2-chloro-4,6-diamino-1,3,5-triazine, N,N,N'-trimethylethylenediamine and potassium carbonate into a reaction flask, introducing nitrogen, extracting after the reaction, separating to obtain an organic phase, drying to remove water, and recrystallizing the crude product with dichloromethane to obtain 2-(trimethylethylenediamine)-4,6-diamino-1,3,5-triazine; Step (2), add N,N-dimethylformamide, 2-(trimethylethylenediamine)-4,6-diamino-1,3,5-triazine and succinic anhydride to a reaction flask, react at 25-40° C. for 2-5 hours, add water after the reaction, mix well and extract with dichloromethane, separate the organic phase, dry and remove water, and recrystallize the crude product with ethanol to obtain 2-(trimethylethylenediamine)-4,6-di(butyric acid amide)-1,3,5-triazine.
7. The method for preparing the modified polyurethane finishing agent according to claim 6, characterized in that: In the step (1), the molar ratio of 2-chloro-4,6-diamino-1,3,5-triazine, N,N,N'-trimethylethylenediamine and potassium carbonate is 1:(0.9-1.1):(1-1.1).
8. The method for preparing the modified polyurethane finishing agent according to claim 6, characterized in that: In the step (1), the reaction temperature is 120-140° C. and the reaction time is 18-36 hours.
9. The method for preparing the modified polyurethane finishing agent according to claim 6, characterized in that: In the step (2), the molar ratio of 2-(trimethylethylenediamine)-4,6-diamino-1,3,5-triazine to succinic anhydride is 1:(2.4-2.8).