A strong and tough magnesium-based high entropy alloy and preparation method thereof
By using AC pulse current with low current density for electrical treatment in the preparation of high-entropy alloys, the problem of difficult to balance compressive strength and toughness in traditional processes was solved, and a magnesium-based high-entropy alloy with high toughness and compressive strength was successfully prepared. .
Patent Information
- Application Number
- CN202410963895.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-07-18
AI Technical Summary
Traditional high-entropy alloy preparation processes are difficult to achieve both high compressive strength and high toughness, often resulting in brittleness or insufficient strength.
The AC pulse current with low current density is used for electrical treatment to control the frequency of current direction changes and current density, promote in-situ high-frequency vibration and concentration fluctuation of the precipitated phase, increase dislocation accumulation, and improve the toughness of the material.
A magnesium-based high-entropy alloy with high toughness and compressive strength is prepared. By adjusting the current parameters, the formation and distribution of the precipitated phase is ensured, and the stress resistance of the material is improved.
Smart Images

Figure CN118497528B_ABST
Abstract
Description
Technical Field
[0001] This application belongs to the field of high-entropy alloys, specifically relating to a strong and tough magnesium-based high-entropy alloy and its preparation method. Background Technology
[0002] High-entropy alloys (HEAs) are a novel type of alloy material composed of five or more metallic elements mixed in near-equiatomic ratios. This type of alloy design breaks away from the conventional model of using a dominant metal and trace alloying elements, exhibiting many superior properties such as high strength, high hardness, good fracture resistance, corrosion resistance, and oxidation resistance. The unique properties of high-entropy alloys stem from their complex composition and structure, where the presence of multiple metallic elements provides unique opportunities for active sites. Through careful selection of element configuration and composition, these active sites can be optimized for specific purposes.
[0003] High-entropy alloys are composed of five or more elements mixed in equiatomic or near-equiatomic ratios, meaning that the atomic percentage of each element ranges from 5% to 35%. With optimized elemental configuration, high-entropy alloys can form solid solution structures such as single body-centered cubic, face-centered cubic, or two-phase mixtures. This unique structure endows high-entropy alloys with a range of excellent properties, such as outstanding corrosion resistance, radiation resistance, thermal stability, as well as high strength, hardness, and wear resistance.
[0004] However, similar to many traditional metallic materials, high-entropy alloys also face the challenge of balancing strength and toughness. High-entropy alloys prepared by traditional techniques may exhibit a hard texture but be brittle, or have good toughness but insufficient strength, failing to achieve both high compressive strength and high toughness. Summary of the Invention
[0005] Based on this, one embodiment of this application provides a method for preparing a strong and tough magnesium-based high-entropy alloy. The magnesium-based high-entropy alloy prepared by this method has high toughness and compressive strength.
[0006] This application provides a method for preparing a strong and tough magnesium-based high-entropy alloy, comprising the following steps:
[0007] Weigh each pure metal according to the general formula, the pure metal including magnesium metal, smelt it, keep it warm and stir it evenly to prepare a melt with a temperature 50°C to 100°C higher than the liquidus line;
[0008] The melt is transferred to a mold and allowed to stand.
[0009] Electrodes are inserted into the mold containing the melt for electrical treatment, the electrodes being used to apply an alternating pulsed current while simultaneously cooling the melt;
[0010] The electrodes are removed, and the melt is further cooled and solidified to obtain the magnesium-based high-entropy alloy.
[0011] The frequency of the alternating current pulse direction change is 10Hz~100Hz, and the current density of the alternating current pulse is 1mA / mm². 2 ~10mA / mm 2 .
[0012] Existing technologies often combine pulsed current technology with high-entropy alloy preparation techniques. Generally, a high current density is used to promote the flow of solute and energy during the solidification process of the high-entropy alloy, thereby promoting uniform nucleation, grain refinement, and improved compressive strength. However, this leads to a decrease in toughness. This application uses a lower current density AC pulsed current, with the aim of not promoting solute flow or grain refinement. This application enables the preparation of high-toughness magnesium-based high-entropy alloys. This is because during solidification, some elements of the high-entropy alloy precipitate in the form of phases. There are differences in conductivity and density between various precipitated phases and between the precipitated phases and the melt matrix. Therefore, they are subjected to different forces in an AC pulsed electric field. By controlling the parameters of the AC pulsed current, the precipitated phases can undergo in-situ high-frequency vibrations, which increases the reaction rate between the precipitated phases and surrounding elements. In particular, it promotes the combination of elements with lower mixing entropy to form precipitated phases, thereby significantly reducing the concentration of the above elements around the precipitated phases. This leads to greater fluctuations in the element distribution around the precipitated phases, resulting in concentration wave fluctuations. Larger concentration wave fluctuations cause more dislocation pile-up inside the material, thereby increasing the probability of cross-slip. Cross-slip can decompose the stress on the material into small forces, thereby improving the toughness of the material. The above process requires strict control of the frequency and density of the current direction change. If the current direction changes too slowly or the current density is too high, the movement distance of the precipitated phase will be too large, which may lead to the mixing of elements around the precipitated phase and prevent the formation of strong concentration fluctuations. If the current direction changes too quickly or the current density is too low, the movement distance of the precipitated phase will be too small, making it difficult to promote the growth of the precipitated phase and promote the reduction of the concentration of some low mixing entropy element combinations around the precipitated phase.
[0013] In one embodiment, the frequency of the current direction change is 50Hz~60Hz, and the current density of the AC pulse current is 3mA / mm². 2 ~5mA / mm 2 The above-mentioned range of AC pulse currents has a better effect.
[0014] In one embodiment, the parameters of the alternating current pulse include at least one of the following characteristics:
[0015] (1) The pulse width of the AC pulse current is 10μs~100μs; and / or
[0016] (2) The processing time of AC pulse current is 0.5 min to 10 min.
[0017] By adjusting the processing time and pulse width range of the AC pulse current, sufficient electrical processing can be ensured during the melt cooling process.
[0018] In one embodiment, the cooling rate is 10°C / min to 100°C / min. A higher cooling rate can accelerate the formation of the precipitated phase and promote a rapid decrease in the concentration of some metal elements near the precipitated phase, thereby causing drastic fluctuations in the element distribution.
[0019] In one embodiment, the cooling rate is 50°C / min to 100°C / min. This range of cooling rates helps to improve the strength of the magnesium-based high-entropy alloy.
[0020] In one embodiment, the distance between the electrode and the bottom of the mold is 8mm to 12mm. If the distance between the electrode and the bottom of the mold is too large, it is not conducive to applying uniform electrical treatment to the entire melt; if the distance between the electrode and the bottom of the mold is too small, the electrode is easily damaged during the electrode installation process.
[0021] In one embodiment, the pure metal includes one or more of magnesium, aluminum, copper, zinc, titanium, lithium, and gadolinium. This preparation method can be applied to the preparation of various magnesium-based high-entropy alloys.
[0022] In one embodiment, the high-entropy alloy is Al7Mg. 3.6 Cu 1.2 Zn7Ti 1.2 Al7Mg prepared by conventional methods 3.6 Cu 1.2 Zn7Ti 1.2 As the material is brittle, the preparation method of this application can enhance the toughness of the material.
[0023] This application also provides a high-toughness magnesium-based high-entropy alloy, which is prepared by the above-described method for preparing a high-toughness magnesium-based high-entropy alloy. The magnesium-based high-entropy alloy prepared by the above-described method exhibits high toughness and compressive strength. Attached Figure Description
[0024] To more clearly illustrate the technical solutions in the embodiments of this application and to more completely understand this application and its beneficial effects, the drawings used in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0025] Figure 1 The image shows the compressive stress-strain curve for Example 1.
[0026] Figure 2 The figure shows the compressive stress-strain curve for Comparative Example 1. Detailed Implementation
[0027] The present application will be further described in detail below with reference to the embodiments and examples. It should be understood that these embodiments and examples are for illustrative purposes only and are not intended to limit the scope of the present application. The purpose of providing these embodiments and examples is to enable a more thorough and comprehensive understanding of the disclosure of the present application. It should also be understood that the present application can be implemented in many different forms and is not limited to the embodiments and examples described herein. Those skilled in the art can make various modifications or alterations without departing from the spirit of the present application, and the equivalent forms obtained also fall within the protection scope of the present application. Furthermore, numerous specific details are set forth in the following description to provide a fuller understanding of the present application. It should be understood that the present application can be implemented without one or more of these details.
[0028] Unless otherwise defined, all technical and scientific terms used in this application have the same meaning as commonly understood by one of ordinary skill in the art to which this application pertains.
[0029] the term
[0030] Unless otherwise stated or in case of contradiction, the terms or phrases used herein shall have the following meanings:
[0031] The terms "and / or," "or / and," and "and / or" as used herein include any one of two or more of the related listed items, as well as any and all combinations of the related listed items. These arbitrary and all combinations include any two related listed items, any more related listed items, or a combination of all related listed items. It should be noted that when at least three items are connected by at least two conjunctions selected from "and / or," "or / and," and "and / or," it should be understood that in this application, the technical solution undoubtedly includes technical solutions connected by "logical AND," and also undoubtedly includes technical solutions connected by "logical OR." For example, "A and / or B" includes three parallel solutions: A, B, and A+B. For example, the technical solution of "A, and / or, B, and / or, C, and / or, D" includes any one of A, B, C, and D (that is, a technical solution that is connected by "logical OR"), as well as any and all combinations of A, B, C, and D, that is, combinations of any two or three of A, B, C, and D, and also combinations of all four of A, B, C, and D (that is, a technical solution that is connected by "logical AND").
[0032] In this application, the terms "multiple", "various", "multiple times", "multi-dimensional", etc., unless otherwise specified, refer to a quantity greater than or equal to 2. For example, "one or more" means one or more than or equal to two.
[0033] The terms “combinations of,” “any combination of,” and “any combination of” used in this article include all suitable combinations of any two or more of the listed items.
[0034] In this document, the term "suitable" as used in phrases such as "suitable combination," "suitable method," and "any suitable method" refers to the ability to implement the technical solution of this application, solve the technical problem of this application, and achieve the expected technical effect of this application.
[0035] In this application, terms such as "further," "even more," and "particularly" are used for descriptive purposes and to indicate differences in content, but should not be construed as limiting the scope of protection of this application.
[0036] In this application, "optionally," "optionally," and "optional" mean that something is optional, that is, it means that it is selected from either "with" or "without." If there are multiple "optional" entries in a technical solution, unless otherwise specified, and there are no contradictions or mutual constraints, each "optional" entry shall be independent.
[0037] In this application, the technical features described in an open-ended manner include both closed technical solutions consisting of the listed features and open technical solutions that include the listed features.
[0038] In this application, numerical intervals (i.e., numerical ranges) are involved. Unless otherwise specified, the selected numerical distributions within the aforementioned numerical intervals are considered continuous and include the two endpoints (i.e., the minimum and maximum values) of the numerical range, as well as every value between these two endpoints. Unless otherwise specified, when a numerical interval refers only to integers within that interval, it includes the two endpoint integers of the numerical range, as well as every integer between the two endpoints. In this document, this is equivalent to directly listing every integer. For example, if t is an integer selected from 1 to 10, it means that t is any integer selected from the group of integers consisting of 1, 2, 3, 4, 5, 6, 7, 8, 9, and 10. Furthermore, when multiple ranges are provided to describe features or characteristics, these ranges can be merged. In other words, unless otherwise specified, the ranges disclosed herein should be understood to include any and all subranges to which they are included.
[0039] Unless otherwise specified, the temperature parameters in this application are permitted to be either constant-temperature treatment or variations within a certain temperature range. It should be understood that the constant-temperature treatment allows temperature fluctuations within the precision range of the instrument control, such as ±5℃, ±4℃, ±3℃, ±2℃, or ±1℃.
[0040] In this application, % (w / w) and wt% both represent weight percentage, % (v / v) refers to volume percentage, and % (w / v) refers to mass-volume percentage.
[0041] All references to documents mentioned in this application are incorporated herein by reference as if each document were individually incorporated herein by reference. Unless they conflict with the inventive purpose and / or technical solution of this application, all cited documents are incorporated herein by reference in their entirety and for all purposes. When citing documents in this application, the definitions of relevant technical features, terms, nouns, phrases, etc., are also incorporated herein by reference. When citing documents in this application, examples and preferred embodiments of the cited technical features may also be incorporated herein by reference, but only to the extent that they enable the implementation of this application. It should be understood that when the cited content conflicts with the description in this application, this application shall prevail or modifications shall be made adaptably to the description in this application.
[0042] This application provides a method for preparing a strong and tough magnesium-based high-entropy alloy, comprising the following steps:
[0043] Weigh each pure metal according to the general formula, including magnesium metal, and smelt it. Keep it warm and stir it evenly to prepare a melt with a temperature 50-100°C higher than the liquidus.
[0044] Transfer the melt into a mold and let it stand.
[0045] Electrodes are inserted into the mold containing the melt for electrical treatment, the electrodes being used to apply an alternating pulse current while simultaneously cooling the melt;
[0046] The electrodes are removed, and the melt is further cooled and solidified to obtain the magnesium-based high-entropy alloy.
[0047] The frequency of the alternating current pulse direction change is 10Hz~100Hz, and the current density of the alternating current pulse is 1mA~10mA / mm. 2 .
[0048] In a specific example, the pulse width of the AC pulse current is 10μs to 100μs.
[0049] Optionally, the processing time of the AC pulse current is 0.5 min to 10 min.
[0050] In a specific example, the distance between the electrode and the bottom of the mold is 8mm to 12mm.
[0051] Optionally, the electrode includes, but is not limited to, one or more of graphene electrodes, graphite electrodes, carbon nanotube electrodes, glassy carbon electrodes, and porous carbon electrodes.
[0052] Graphene is a two-dimensional material formed by a single layer of carbon atoms with sp2 hybridization, and it has excellent electrical conductivity, thermal conductivity, mechanical strength and flexibility.
[0053] Further optionally, the mold includes one or more of graphite crucibles, corundum crucibles, and silicon carbide crucibles. Graphite crucibles: possess excellent high-temperature strength and thermal conductivity, commonly used for melting metals, but may react with certain metals or materials; ceramic crucibles: made of heat-resistant ceramic materials, possessing good chemical stability, suitable for applications requiring contamination avoidance; corundum crucibles: made of alumina (Al₂O₃), resistant to high temperatures, chemically stable, commonly used for melting metals and glass.
[0054] This application also provides a tough magnesium-based high-entropy alloy, which is prepared by the method for preparing the magnesium-based high-entropy alloy.
[0055] This application also provides the application of the aforementioned high-strength magnesium-based high-entropy alloy in the preparation of composite metal materials.
[0056] The embodiments of this application will be described in detail below with reference to examples. It should be understood that these embodiments are for illustrative purposes only and are not intended to limit the scope of this application. For experimental methods in the following embodiments where specific conditions are not specified, please refer to the guidelines given in this application, or follow experimental manuals or conventional conditions in the art, or follow the conditions recommended by the manufacturer, or refer to experimental methods known in the art.
[0057] In the specific embodiments described below, the measurement parameters involving raw material components may have slight deviations within the weighing accuracy range unless otherwise specified. Temperature and time parameters are subject to acceptable deviations due to instrument testing accuracy or operational precision.
[0058] It should be understood that in the various embodiments of this application, the order of the above-mentioned processes does not imply the order of execution. The execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of the embodiments of this application.
[0059] Example 1: An embodiment of this application provides a method for preparing a strong and tough magnesium-based high-entropy alloy.
[0060] 1. Preparation of magnesium-based high-entropy alloys from raw materials
[0061] The magnesium-based high-entropy alloy is Al7Mg. 3.6 Cu 1.2 Zn7Ti 1.2 Weigh out the various raw materials according to the requirements for preparing 50kg of magnesium-based high-entropy alloy.
[0062] 2. Smelting process
[0063] The metal raw materials are added to the vacuum melting furnace in order of increasing melting point and heated to 1000℃. The mixture is kept at this temperature and stirred until homogeneous. The melt is then transferred to a crucible mold and allowed to stand.
[0064] 3. Electrical treatment
[0065] A graphite electrode rod is inserted into the melt and fixed to the side wall of the crucible, with the rod 8 mm from the bottom. The graphite electrode rod is then connected to an external pulse power supply. The pulse power supply is activated, with a current direction change frequency of 10 Hz and an AC pulse current density of 1 mA / mm². 2 The pulse width of the AC pulse current is 30μs; the processing time of the AC pulse current is 1min, while the melt is cooled at a rate of 50℃ / min.
[0066] 4. Obtaining magnesium-based high-entropy alloys
[0067] After removing the electrodes, the melt continues to cool and solidify at a rate of 50°C / min to 933°C. Once the melt has completely solidified, a magnesium-based high-entropy alloy is obtained.
[0068] Example 2: One embodiment of this application provides a method for preparing a strong and tough magnesium-based high-entropy alloy.
[0069] 1. Preparation of magnesium-based high-entropy alloys from raw materials
[0070] The magnesium-based high-entropy alloy is Al7Mg. 3.6 Cu 1.2 Zn7Ti 1.2 Weigh out the various raw materials according to the requirements for preparing 50kg of magnesium-based high-entropy alloy.
[0071] 2. Smelting process
[0072] The metal raw materials are added to the vacuum melting furnace in order of increasing melting point and heated to 1000℃. The mixture is kept at this temperature and stirred until homogeneous. The melt is then transferred to a crucible mold and allowed to stand.
[0073] 3. Electrical treatment
[0074] A graphite electrode rod is inserted into the melt and fixed to the side wall of the crucible, with the rod 8 mm from the bottom. The graphite electrode rod is then connected to an external pulse power supply. The pulse power supply is activated, with a current direction change frequency of 100 Hz and an AC pulse current density of 10 mA / mm². 2 The pulse width of the AC pulse current is 100 μs; the processing time of the AC pulse current is 0.5 min, while the melt is cooled at a rate of 50 °C / min.
[0075] 4. Obtaining magnesium-based high-entropy alloys
[0076] After removing the electrodes, the melt continues to cool and solidify at a rate of 50°C / min to 933°C. Once the melt has completely solidified, a magnesium-based high-entropy alloy is obtained.
[0077] Example 3: An embodiment of this application provides a method for preparing a strong and tough magnesium-based high-entropy alloy.
[0078] 1. Preparation of magnesium-based high-entropy alloys from raw materials
[0079] The magnesium-based high-entropy alloy is Al7Mg. 3.6 Cu 1.2 Zn7Ti 1.2 Weigh out the various raw materials according to the requirements for preparing 50kg of magnesium-based high-entropy alloy.
[0080] 2. Smelting process
[0081] The metal raw materials are added to the vacuum melting furnace in order of increasing melting point and heated to 1000℃. The mixture is kept at this temperature and stirred until homogeneous. The melt is then transferred to a crucible mold and allowed to stand.
[0082] 3. Electrical treatment
[0083] A graphite electrode rod is inserted into the melt and fixed to the side wall of the crucible, with the rod 8 mm from the bottom. The graphite electrode rod is then connected to an external pulse power supply. The pulse power supply is activated, with a current direction change frequency of 50 Hz and an AC pulse current density of 5 mA / mm². 2 The pulse width of the AC pulse current is 30μs; the processing time of the AC pulse current is 1min, while the melt is cooled at a rate of 50℃ / min.
[0084] 4. Obtaining magnesium-based high-entropy alloys
[0085] After removing the electrodes, the melt continues to cool and solidify at a rate of 50°C / min to 933°C. Once the melt has completely solidified, a magnesium-based high-entropy alloy is obtained.
[0086] Example 4: An embodiment of this application provides a method for preparing a strong and tough magnesium-based high-entropy alloy.
[0087] 1. Preparation of magnesium-based high-entropy alloys from raw materials
[0088] The magnesium-based high-entropy alloy is Al7Mg. 3.6 Cu 1.2 Zn7Ti 1.2 Weigh out the various raw materials according to the requirements for preparing 50kg of magnesium-based high-entropy alloy.
[0089] 2. Smelting process
[0090] The metal raw materials are added to the vacuum melting furnace in order of increasing melting point and heated to 1000℃. The mixture is kept at this temperature and stirred until homogeneous. The melt is then transferred to a crucible mold and allowed to stand.
[0091] 3. Electrical treatment
[0092] A graphite electrode rod is inserted into the melt and fixed to the side wall of the crucible, with the rod 8 mm from the bottom. The graphite electrode rod is then connected to an external pulse power supply. The pulse power supply is activated, with a current direction change frequency of 10 Hz and an AC pulse current density of 1 mA / mm². 2 The pulse width of the AC pulse current is 30μs; the processing time of the AC pulse current is 10min, while the melt is cooled at a rate of 10℃ / min.
[0093] 4. Obtaining magnesium-based high-entropy alloys
[0094] After removing the electrodes, the melt continues to cool and solidify at a rate of 10℃ / min to 933℃. Once the melt has completely solidified, a magnesium-based high-entropy alloy is obtained.
[0095] Example 5: One embodiment of this application provides a method for preparing a strong and tough magnesium-based high-entropy alloy.
[0096] 1. Preparation of magnesium-based high-entropy alloys from raw materials
[0097] The magnesium-based high-entropy alloy is Al7Mg. 3.6 Cu 1.2 Zn7Ti 1.2 Weigh out the various raw materials according to the requirements for preparing 50kg of magnesium-based high-entropy alloy.
[0098] 2. Smelting process
[0099] The metal raw materials are added to the vacuum melting furnace in order of increasing melting point and heated to 1000℃. The mixture is kept at this temperature and stirred until homogeneous. The melt is then transferred to a crucible mold and allowed to stand.
[0100] 3. Electrical treatment
[0101] A graphite electrode rod is inserted into the melt and fixed to the side wall of the crucible, with the rod 8 mm from the bottom. The graphite electrode rod is then connected to an external pulse power supply. The pulse power supply is activated, with a current direction change frequency of 10 Hz and an AC pulse current density of 1 mA / mm². 2 The pulse width of the AC pulse current is 30μs; the processing time of the AC pulse current is 0.5min, while the melt is cooled at a rate of 100℃ / min.
[0102] 4. Obtaining magnesium-based high-entropy alloys
[0103] After removing the electrodes, the melt continues to cool and solidify at a rate of 100℃ / min to 933℃. Once the melt has completely solidified, a magnesium-based high-entropy alloy is obtained.
[0104] Comparative Example 1: This comparative example provides a conventional method for preparing magnesium-based high-entropy alloys. Compared with Example 1, this comparative example does not include an electrical treatment step.
[0105] 1. Preparation of magnesium-based high-entropy alloys from raw materials
[0106] The magnesium-based high-entropy alloy is Al7Mg. 3.6 Cu 1.2 Zn7Ti 1.2 Weigh out the various raw materials according to the requirements for preparing 50kg of magnesium-based high-entropy alloy.
[0107] 2. Smelting process
[0108] The metal raw materials are added to the vacuum melting furnace in order of increasing melting point and heated to 1000℃. The mixture is kept at this temperature and stirred until homogeneous. The melt is then transferred to a crucible mold and allowed to stand.
[0109] 3. Obtaining magnesium-based high-entropy alloys
[0110] The melt was cooled and solidified at a rate of 50℃ / min to 933℃. After the melt was completely solidified, a magnesium-based high-entropy alloy was obtained.
[0111] Comparative Example 2: Compared with Example 1, this comparative example used an excessively high current density.
[0112] 1. Preparation of magnesium-based high-entropy alloys from raw materials
[0113] The magnesium-based high-entropy alloy is Al7Mg. 3.6 Cu 1.2 Zn7Ti 1.2 Weigh out the various raw materials according to the requirements for preparing 50kg of magnesium-based high-entropy alloy.
[0114] 2. Smelting process
[0115] The metal raw materials are added to the vacuum melting furnace in order of increasing melting point and heated to 1000℃. The mixture is kept at this temperature and stirred until homogeneous. The melt is then transferred to a crucible mold and allowed to stand.
[0116] 3. Electrical treatment
[0117] A graphite electrode rod is inserted into the melt and fixed to the side wall of the crucible, with the rod 8 mm from the bottom. The graphite electrode rod is then connected to an external pulse power supply. The pulse power supply is activated, with a current direction change frequency of 10 Hz and an AC pulse current density of 30 mA / mm². 2 The pulse width of the AC pulse current is 30μs; the processing time of the AC pulse current is 1min, while the melt is cooled at a rate of 50℃ / min.
[0118] 4. Obtaining magnesium-based high-entropy alloys
[0119] After removing the electrodes, the melt continues to cool and solidify at a rate of 50°C / min to 933°C. Once the melt has completely solidified, a magnesium-based high-entropy alloy is obtained.
[0120] Comparative Example 3: Compared with Example 1, the difference in this comparative example is that the change in current direction is too slow.
[0121] 1. Preparation of magnesium-based high-entropy alloys from raw materials
[0122] The magnesium-based high-entropy alloy is Al7Mg. 3.6 Cu 1.2 Zn7Ti 1.2 Weigh out the various raw materials according to the requirements for preparing 50kg of magnesium-based high-entropy alloy.
[0123] 2. Smelting process
[0124] The metal raw materials are added to the vacuum melting furnace in order of increasing melting point and heated to 1000℃. The mixture is kept at this temperature and stirred until homogeneous. The melt is then transferred to a crucible mold and allowed to stand.
[0125] 3. Electrical treatment
[0126] A graphite electrode rod is inserted into the melt and fixed to the side wall of the crucible, with the rod 8 mm from the bottom. The graphite electrode rod is then connected to an external pulse power supply. The pulse power supply is activated, with a current direction change frequency of 2 Hz and an AC pulse current density of 1 mA / mm². 2 The pulse width of the AC pulse current is 30μs; the processing time of the AC pulse current is 1min, while the melt is cooled at a rate of 50℃ / min.
[0127] 4. Obtaining magnesium-based high-entropy alloys
[0128] After removing the electrodes, the melt continues to cool and solidify at a rate of 50°C / min to 933°C. Once the melt has completely solidified, a magnesium-based high-entropy alloy is obtained.
[0129] Comparative Example 4: Compared with Example 1, the difference in this comparative example is that the direction of the current changes too quickly.
[0130] 1. Preparation of magnesium-based high-entropy alloys from raw materials
[0131] The magnesium-based high-entropy alloy is Al7Mg. 3.6 Cu 1.2 Zn7Ti 1.2 Weigh out the various raw materials according to the requirements for preparing 50kg of magnesium-based high-entropy alloy.
[0132] 2. Smelting process
[0133] The metal raw materials are added to the vacuum melting furnace in order of increasing melting point and heated to 1000℃. The mixture is kept at this temperature and stirred until homogeneous. The melt is then transferred to a crucible mold and allowed to stand.
[0134] 3. Electrical treatment
[0135] A graphite electrode rod is inserted into the melt and fixed to the side wall of the crucible, with the rod 8 mm from the bottom. The graphite electrode rod is then connected to an external pulse power supply. The pulse power supply is activated, with a current direction change frequency of 500 Hz and an AC pulse current density of 1 mA / mm². 2 The pulse width of the AC pulse current is 30μs; the processing time of the AC pulse current is 1min, while the melt is cooled at a rate of 50℃ / min.
[0136] 4. Obtaining magnesium-based high-entropy alloys
[0137] After removing the electrodes, the melt continues to cool and solidify at a rate of 50°C / min to 933°C. Once the melt has completely solidified, a magnesium-based high-entropy alloy is obtained.
[0138] Comparative Example 5: Compared with Example 1, this comparative example used an excessively low current density.
[0139] 1. Preparation of magnesium-based high-entropy alloys from raw materials
[0140] The magnesium-based high-entropy alloy is Al7Mg3.6Cu1.2Zn7Ti1.2. Various raw materials are weighed according to the requirements for preparing 50kg of magnesium-based high-entropy alloy.
[0141] 2. Smelting process
[0142] The metal raw materials are added to the vacuum melting furnace in order of increasing melting point and heated to 1000℃. The mixture is kept at this temperature and stirred until homogeneous. The melt is then transferred to a crucible mold and allowed to stand.
[0143] 3. Electrical treatment
[0144] A graphite electrode rod is inserted into the melt and fixed to the side wall of the crucible, with the rod 8 mm from the bottom. The graphite electrode rod is then connected to an external pulse power supply. The pulse power supply is activated, with a current direction change frequency of 10 Hz and an AC pulse current density of 0.2 mA / mm². 2 The pulse width of the AC pulse current is 30μs; the processing time of the AC pulse current is 1min, while the melt is cooled at a rate of 50℃ / min.
[0145] 4. Obtaining magnesium-based high-entropy alloys
[0146] After removing the electrodes, the melt continues to cool and solidify at a rate of 50°C / min to 933°C. Once the melt has completely solidified, a magnesium-based high-entropy alloy is obtained.
[0147] Experimental results verification
[0148] The compressive strength and strain rate of the magnesium-based high-entropy alloys of Examples 1-5 and Comparative Examples 1-5 were tested using the following methods:
[0149] Compressive strength and strain rate tests: Measured in accordance with national standard GB / T 7314-2017.
[0150] The test results are shown in Table 1:
[0151] Table 1
[0152]
[0153] According to the data in Table 1, the magnesium-based high-entropy alloys prepared in Examples 1-5 of this application show superior performance in both compressive strength and strain rate compared to Comparative Example 1, exhibiting higher compressive strength and higher toughness. Figures 1-2The data shows that Example 1 has a longer plastic segment and stronger toughness compared to Comparative Example 1. This is because controlling the parameters of the AC pulse current can induce in-situ high-frequency vibration of the precipitated phase, increasing the reaction rate between the precipitated phase and surrounding elements. In particular, it promotes the formation of precipitated phases by combining elements with lower mixing entropy, thereby significantly reducing the concentration of these elements around the precipitated phase. This leads to greater fluctuations in the element distribution around the precipitated phase, resulting in concentration wave fluctuations. Larger concentration wave fluctuations cause more dislocation pile-up within the material, increasing the probability of cross-slip. Cross-slip can decompose the stress on the material into small forces, thereby improving the toughness of the material. Although Comparative Example 2 underwent electrotreatment, it used excessively high current density, resulting in excessive movement distance of the precipitated phase. This led to mixing of elements around the precipitated phase, which actually suppressed the concentration fluctuations caused by element precipitation. Furthermore, the higher current density can induce the formation of smaller grains, which, while helping to improve the compressive strength of the high-entropy alloy, further deteriorates the toughness of the high-entropy alloy. Comparative Example 3 used an excessively low current change rate, resulting in an excessively large movement distance of the precipitated phase, leading to mixing of elements around the precipitated phase. Furthermore, the current density was too low to promote crystal nucleus refinement and thus fail to improve the strength of the high-entropy alloy. Comparative Example 4 used an excessively high current change frequency, and Comparative Example 5 used an excessively low current density, resulting in an excessively small movement distance of the precipitated phase, which failed to create significant concentration fluctuations.
[0154] Example 3 exhibits stronger compressive strength and strain rate compared to Examples 1-2 due to the use of preferred current density and current direction change frequency. Example 4 uses a lower cooling rate, resulting in slower precipitate formation, smaller concentration wave fluctuations, and inferior strength and toughness compared to Examples 1-3. Example 5 uses a higher cooling rate, leading to faster precipitate formation and larger concentration wave fluctuations, which helps improve the strength and toughness of the high-entropy alloy; however, the fine precipitates can hinder the improvement of the high-entropy alloy's toughness.
[0155] The embodiments described above merely illustrate several implementation methods of this application to facilitate a detailed understanding of the technical solutions of this application, but should not be construed as limiting the scope of protection of the patent application. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of this application, and these all fall within the scope of protection of this application. Furthermore, it should be understood that after reading the above teachings of this application, those skilled in the art can make various alterations or modifications to this application, and the equivalent forms obtained also fall within the scope of protection of this application. It should also be understood that technical solutions obtained by those skilled in the art based on the technical solutions provided in this application through logical analysis, reasoning, or limited experimentation are all within the scope of protection of the appended claims. Therefore, the scope of protection of this patent application should be determined by the content of the appended claims, and the specification and drawings can be used to interpret the content of the claims.
Claims
1. A method for preparing a strong and tough magnesium-based high entropy alloy, characterized in that: The following steps are involved: Weigh each pure metal according to the general composition formula. The pure metals include magnesium, aluminum, copper, zinc and titanium. The magnesium-based high entropy alloy is Al7Mg 3.6 Cu 1.2 Zn7Ti 1.2 , smelting, heat preservation and stirring uniformly, preparing a melt with a temperature 50°C to 100°C higher than the liquidus; Transferring the melt into a mold and letting it stand; Inserting an electrode into the mold containing the melt for electrical treatment, the electrode being used to apply an alternating current pulse while cooling the melt; The electrode is removed, and the melt is allowed to cool and solidify to obtain the magnesium-based high entropy alloy; The current direction change frequency is 50Hz~60Hz, and the current density of the AC pulse current is 3mA / mm 2 ~5mA / mm 2 ; The pulse width of the AC pulse current is 10 μs to 100 μs; the processing time of the AC pulse current is 0.5 min to 10 min.
2. The method for preparing a strong and tough magnesium-based high entropy alloy according to claim 1, characterized in that: The cooling rate is 10°C / min to 100°C / min.
3. The method for preparing a strong and tough magnesium-based high entropy alloy according to claim 2, characterized in that: The cooling rate is 50°C / min to 100°C / min.
4. The method for preparing a strong and tough magnesium-based high entropy alloy according to claim 1, characterized in that: The current direction change frequency is 50 Hz, and the current density of the AC pulse current is 5 mA / mm 2 The pulse width of the AC pulse current is 30 μs; the processing time of the AC pulse current is 1 min.
5. The method for preparing a strong and tough magnesium-based high entropy alloy according to claim 1, characterized in that: The distance between the electrode and the bottom of the mold is 8 mm to 12 mm.
6. A strong and tough magnesium-based high entropy alloy, characterized in that: The strong and tough magnesium-based high entropy alloy is prepared by the method for preparing the strong and tough magnesium-based high entropy alloy according to any one of claims 1 to 5.
Citation Information
Patent Citations
Method for preparing high-strength-and-toughness aluminum-based high-entropy alloy composite strip
CN112795797A
High-strength lightweight high-entropy alloy and preparation method thereof
CN117987714A