A method for preparing ZnO@In2O3 reinforced silver-based composite materials by powder metallurgy
ZnO@In2O3 powder was prepared by combining electrolysis and sintering, which improved the interfacial wettability of Ag/ZnO composite materials and formed a core-shell structure. This solved the problem of poor interfacial bonding in powder metallurgy and improved the mechanical and electrical contact properties of the material.
Patent Information
- Application Number
- CN202410627708.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-21
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2044-05-21
AI Technical Summary
Existing Ag/ZnO composite material preparation processes suffer from problems such as incomplete oxidation, long production cycles, high costs, and poor interfacial bonding. In particular, the powder surface is easily contaminated and the interfacial wettability is poor in powder metallurgy.
ZnO@In2O3 powder was prepared by combining electrolysis and sintering. In2O3 was introduced between Ag and ZnO through ball milling, pressing and multi-stage sintering to improve interfacial wettability, form a core-shell structure and improve interfacial bonding.
The mechanical and electrical contact properties of Ag/ZnO composite materials were improved, and the interfacial bonding strength and arc erosion resistance were significantly enhanced.
Smart Images

Figure CN118497540B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of composite material technology, specifically a method for preparing ZnO@In2O3 reinforced silver-based composite materials using powder metallurgy. Background Technology
[0002] With the rapid development of industry and the continuous progress of science and technology, the performance requirements for materials are becoming increasingly stringent, especially for devices operating in extreme environments that require special properties. Among them, Ag / ZnO composite materials have low and stable contact resistance, good anti-welding properties, and excellent arc corrosion resistance, and have been widely used in relays, contactors, circuit breakers and other fields.
[0003] Currently, the main preparation processes for Ag / ZnO composite materials on the market include alloy internal oxidation, powder pre-oxidation, powder metallurgy, and hot isostatic pressing. Among these, the silver oxide materials prepared by alloy internal oxidation often suffer from incomplete oxidation, requiring secondary oxidation and resulting in a long production cycle. While powder pre-oxidation and hot isostatic pressing solve the problem of incomplete oxidation in alloy internal oxidation, their production costs are higher. Although powder metallurgy has a simple process and allows for easy addition of components, the powder surface is prone to contamination during preparation. For Ag and ZnO powders with poor interfacial wettability, this can easily lead to poor interfacial bonding after preparation. Summary of the Invention
[0004] The purpose of this invention is to provide a method for preparing ZnO@In2O3 reinforced silver-based composite materials by powder metallurgy, so as to solve the problems mentioned in the background art.
[0005] To achieve the above objectives, the present invention provides the following technical solution:
[0006] A method for preparing ZnO@In2O3 reinforced silver-based composite materials by powder metallurgy includes the following steps:
[0007] S1. Using ZnO powder as raw material, ZnO@In2O3 powder is obtained through a combination of electrolysis and sintering.
[0008] S2. The ZnO@In2O3 powder obtained in step S1 is mixed with Ag powder in a certain proportion and then ball-milled to obtain composite powder.
[0009] S3. Press the composite powder obtained in step S2 into a mold; sinter it in a sintering furnace to form a ZnO@In2O3 reinforced silver matrix composite sintered blank; then densify the sintered blank, extrude it, and draw it into wire or roll it into strip at room temperature. The In2O3 core and shell are located between ZnO and Ag, which have poor interfacial wettability, thus improving the interfacial bonding force between the reinforcing phase and the silver matrix, thereby improving the mechanical properties and electrical contact properties of the metal oxide reinforced silver matrix composite.
[0010] As a further aspect of the present invention: in step S1, the specific preparation method of ZnO@In2O3 powder is as follows:
[0011] S11. Electrolysis is carried out in an electrolyte with an indium plate as the anode and a graphite electrode as the cathode until the indium plate at the anode is completely electrolyzed and disappears in the electrolyte.
[0012] S12. Add ZnO powder to the electrolyte at a ratio of 10-60 g / L and stir for 3-10 min; after centrifuging the electrolyte, wash it 3-5 times with deionized water at a volume ratio of 10:1; preferably, the ratio of ZnO powder to electrolyte is 50 g / L, stir for 6 min, and wash 5 times.
[0013] S13. Dry in a drying oven at 60-120℃ for 5-20 hours, then grind and pass through a 200-800 mesh sieve to obtain white powder In(OH)3; preferably, dry in a drying oven at 100℃ for 10 hours and grind and pass through a 300 mesh sieve.
[0014] S14. The ZnO@In2O3 powder is prepared by calcining after being kept at 300℃ for 1-2 hours, 400℃ for 1-4 hours, and 500℃ for 1-2 hours. Preferably, the powder is kept at 300℃ for 1 hour, 400℃ for 3 hours, and 500℃ for 2 hours.
[0015] As a further aspect of the present invention: in step S11, the electrolyte is prepared by dissolving NH4Cl in deionized water; and the current density during the electrolysis process is 0.2–0.9 A / cm². 2 The preferred current density is 0.6 A / cm². 2 .
[0016] As a further embodiment of the present invention: the particle size of the ZnO powder is 50-1000 nm, the purity is ≥99.9%, and the sphericity is ≥0.9, with the ZnO powder particle size preferably being 300 nm; the particle size of the ZnO@In2O3 powder is 60-1100 nm, and the sphericity is ≥0.9, with the ZnO@In2O3 powder particle size preferably being 450 nm.
[0017] As a further embodiment of the present invention: in step S2, the Ag powder has a particle size of 10-50 μm and a purity of ≥99.9%, preferably 35 nm, and the mass ratio of ZnO@In2O3 powder to Ag powder is (4-9):50; preferably, the mass ratio of ZnO@In2O3 powder to Ag powder is 7.5:50; the ball milling process is performed at a rotation speed of 150-700 r / min for 0.5-2 h, preferably at a rotation speed of 350 r / min for 1 h.
[0018] As a further embodiment of the present invention: in step S3, the pressure during the pressing process is 150-800 MPa, preferably 500 MPa; the sintering process adopts a multi-stage sintering-holding method, with sintering and holding temperatures ranging from 100 to 850°C, preferably sintering at 300°C and holding for 1 hour → sintering at 500°C and holding for 1 hour → sintering at 850°C and holding for 1 hour; the extrusion temperature is 800°C, and the extrusion pressure is 700 MPa.
[0019] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0020] This invention improves the interfacial wettability and bonding of Ag and ZnO by introducing In2O3, which has good wettability with the silver matrix, between Ag and ZnO, thereby obtaining a metal oxide-reinforced silver matrix composite material with a ZnO@In2O3 core-shell structure; this improves the mechanical and electrical contact properties of the metal oxide-reinforced silver matrix composite material. Attached Figure Description
[0021] Figure 1 This is a schematic diagram of a process for preparing ZnO@In2O3 reinforced silver-based composite materials using powder metallurgy. Detailed Implementation
[0022] Example 1
[0023] Please see Figure 1 In this embodiment of the invention, a method for preparing ZnO@In2O3 reinforced silver-based composite materials by powder metallurgy includes the following steps:
[0024] S1. Using an indium plate as the anode and a graphite electrode as the cathode, NH4Cl is dissolved in deionized water to obtain the electrolyte. The current density is 0.6 / cm². 2Electrolysis was performed under the specified conditions until all the indium plate at the anode disappeared into the electrolyte. ZnO powder with a particle size of 300 nm, a purity of 99.9%, and a sphericity of 0.9 was added to the electrolyte at a ratio of 50 g / L and stirred for 6 min. After centrifugation of the electrolyte, it was washed 5 times with deionized water at a volume ratio of 10:1. It was dried in a drying oven at 100 °C for 10 h, then ground and passed through a 300-mesh sieve to obtain white powder In(OH)3. It was then heated at 300 °C for 1 h, at 400 °C for 3 h, and at 500 °C for 2 h, and then calcined to prepare ZnO@In2O3 powder with a particle size of 450 nm and a sphericity of 0.9.
[0025] S2. The ZnO@In2O3 powder obtained in step S1 is mixed with Ag powder with a particle size of 35μm and a purity of 99.9% at a mass ratio of 7.5:50, and then ball-milled at a speed of 350r / min for 1h to obtain composite powder.
[0026] S3. The composite powder obtained in step S2 is pressed into shape in a mold under a pressure of 500 MPa; and sintered in a sintering furnace at 300℃ and held for 1 hour → 500℃ and held for 1 hour → 850℃ and held for 1 hour to obtain a ZnO@In2O3 reinforced silver-based composite material sintered blank; then the sintered blank is densified, extruded at 800℃ under a pressure of 700 MPa, and drawn into wire.
[0027] Example 2
[0028] Please see Figure 1 In this embodiment of the invention, a method for preparing ZnO@In2O3 reinforced silver-based composite materials by powder metallurgy includes the following steps:
[0029] S1. Using an indium plate as the anode and a graphite electrode as the cathode, NH4Cl is dissolved in deionized water to obtain the electrolyte, at a current density of 0.7 A / cm². 2 Electrolysis was performed under the specified conditions until all the indium plate at the anode disappeared into the electrolyte. ZnO powder with a particle size of 100 nm, a purity of 99.9%, and a sphericity of 0.9 was added to the electrolyte at a ratio of 40 g / L and stirred for 5 min. After centrifugation of the electrolyte, it was washed four times with deionized water at a volume ratio of 10:1. It was dried in a drying oven at 100 °C for 15 h, then ground and passed through a 300-mesh sieve to obtain white powder In(OH)3. It was then heated at 300 °C for 2 h, at 400 °C for 3 h, and at 500 °C for 2 h, and then calcined to prepare ZnO@In2O3 powder with a particle size of 250 nm and a sphericity of 0.9.
[0030] S2. The ZnO@In2O3 powder obtained in step S1 is mixed with Ag powder with a particle size of 35μm and a purity of 99.9% at a mass ratio of 6.5:50, and then ball-milled at a speed of 300r / min for 2h to obtain composite powder.
[0031] S3. The composite powder obtained in step S2 is pressed into shape in a mold under a pressure of 600 MPa; and sintered in a sintering furnace at 300℃ and held for 1 h → 450℃ and held for 3 h → 850℃ and held for 2 h to obtain a ZnO@In2O3 reinforced silver-based composite material sintered blank; then the sintered blank is densified, extruded at 550℃ under a pressure of 650 MPa, and drawn into wire.
[0032] Example 3
[0033] Please see Figure 1 In this embodiment of the invention, a method for preparing ZnO@In2O3 reinforced silver-based composite materials by powder metallurgy includes the following steps:
[0034] S1. Using an indium plate as the anode and a graphite electrode as the cathode, NH4Cl is dissolved in deionized water to obtain the electrolyte, at a current density of 0.3 A / cm². 2 Electrolysis was performed under the specified conditions until all the indium plate at the anode disappeared into the electrolyte. ZnO powder with a particle size of 1000 nm, a purity of 99.9%, and a sphericity of 0.9 was added to the electrolyte at a ratio of 60 g / L and stirred for 6 min. After centrifugation of the electrolyte, it was washed four times with deionized water at a volume ratio of 10:1. It was dried in a drying oven at 100 °C for 8 h, then ground and passed through a 600-mesh sieve to obtain white powder In(OH)3. It was then heated at 300 °C for 1.5 h, at 400 °C for 3 h, and at 500 °C for 1.5 h, and then calcined to prepare ZnO@In2O3 powder with a particle size of 1100 nm and a sphericity of 0.9.
[0035] S2. The ZnO@In2O3 powder obtained in step S1 is mixed with Ag powder with a particle size of 20μm and a purity of 99.9% at a mass ratio of 6.5:50, and then ball-milled at a speed of 500r / min for 1h to obtain composite powder.
[0036] S3. The composite powder obtained in step S2 is pressed into shape in a mold under a pressure of 500 MPa; and sintered in a sintering furnace at 200℃ and held for 2 hours → 450℃ and held for 2 hours → 600℃ and held for 2 hours to obtain a ZnO@In2O3 reinforced silver-based composite material sintered blank; then the sintered blank is densified, extruded at 650℃ and pressure of 600 MPa, and drawn into wire.
[0037] Example 4
[0038] Please see Figure 1 In this embodiment of the invention, a method for preparing ZnO@In2O3 reinforced silver-based composite materials by powder metallurgy includes the following steps:
[0039] S1. Using an indium plate as the anode and a graphite electrode as the cathode, NH4Cl is dissolved in deionized water to obtain the electrolyte, at a current density of 0.7 A / cm². 2 Electrolysis was performed under the specified conditions until all the indium plate at the anode disappeared into the electrolyte. ZnO powder with a particle size of 300 nm, a purity of 99.9%, and a sphericity of 0.9 was added to the electrolyte at a ratio of 30 g / L and stirred for 3 min. After centrifugation of the electrolyte, it was washed three times with deionized water at a volume ratio of 10:1. It was dried in a drying oven at 100 °C for 15 h, then ground and passed through a 300-mesh sieve to obtain white powder In(OH)3. The powder was then kept at 300 °C for 2 h, 400 °C for 3 h, and 500 °C for 2 h, and then calcined to prepare ZnO@In2O3 powder with a particle size of 400 nm and a sphericity of 0.9.
[0040] S2. The ZnO@In2O3 powder obtained in step S1 is mixed with Ag powder with a particle size of 20μm and a purity of 99.9% at a mass ratio of 9:50, and then ball-milled at a speed of 550r / min for 2h to obtain composite powder.
[0041] S3. The composite powder obtained in step S2 is pressed into shape in a mold under a pressure of 700 MPa; and sintered in a sintering furnace at 300℃ and held for 3 hours → 450℃ and held for 3 hours → 850℃ and held for 3 hours to obtain a ZnO@In2O3 reinforced silver-based composite material sintered blank; then the sintered blank is densified, extruded at 750℃ under a pressure of 550 MPa, and drawn into wire.
[0042] Example 5
[0043] Please see Figure 1 In this embodiment of the invention, a method for preparing ZnO@In2O3 reinforced silver-based composite materials by powder metallurgy includes the following steps:
[0044] S1. Using an indium plate as the anode and a graphite electrode as the cathode, NH4Cl is dissolved in deionized water to obtain the electrolyte, at a current density of 0.8 A / cm². 2Electrolysis was performed under the specified conditions until all the indium plate at the anode disappeared into the electrolyte. ZnO powder with a particle size of 80 nm, a purity of 99.9%, and a sphericity of 0.9 was added to the electrolyte at a ratio of 10 g / L and stirred for 8 min. After centrifugation of the electrolyte, it was washed 5 times with deionized water at a volume ratio of 10:1. It was dried in a drying oven at 90 °C for 15 h, then ground and passed through a 600-mesh sieve to obtain white powder In(OH)3. It was then heated at 300 °C for 2 h, at 400 °C for 3 h, and at 500 °C for 2 h, and then calcined to prepare ZnO@In2O3 powder with a particle size of 90 nm and a sphericity of 0.9.
[0045] S2. The ZnO@In2O3 powder obtained in step S1 is mixed with Ag powder with a particle size of 10μm and a purity of 99.9% at a mass ratio of 5:50, and then ball-milled at a speed of 700r / min for 1h to obtain composite powder.
[0046] S3. The composite powder obtained in step S2 is pressed into shape in a mold under a pressure of 800 MPa; and sintered in a sintering furnace at 100℃ and held for 1 h → 350℃ and held for 2 h → 450℃ and held for 2 h → 650℃ and held for 2 h → 850℃ and held for 2 h to obtain a ZnO@In2O3 reinforced silver-based composite sintered blank; then the sintered blank is densified, extruded at 850℃ under a pressure of 550 MPa, and drawn into wire.
[0047] To better illustrate the technical effects of the present invention, the following experiments are conducted:
[0048] Example 1 of the preparation method of silver-zinc oxide composite material disclosed on the patent website (publication date 2010-02-03, publication number CN101638732A) is used as comparative example 1.
[0049] Composite material samples prepared in Examples 1-5 and Comparative Example 1 (Example 1) were used as contacts, with a diameter of 4 mm and a weight of 5 ± 0.1 g. These were used as the positive and negative electrodes, respectively, for electro-erosion experiments. The test conditions were: test voltage 20 VDC, test current 20 A, purely resistive load; static contact pressure 1 N, opening and closing frequency 100 times / min, and opening distance 2 mm. After 150,000 breaking operations, the losses of the positive and negative electrodes were measured and recorded in Table 1 below.
[0050] Table 1. Record of contact loss between positive and negative electrodes
[0051]
[0052]
[0053] Table 1 above shows that the positive and negative electrode losses of the contacts in Examples 1 to 5 are significantly less than those in Comparative Example 1; and the positive and negative electrode losses of the contacts in Example 1 are the smallest. Therefore, it can be concluded that the silver-based composite material prepared by the method of the present invention has excellent mechanical and arc erosion properties.
[0054] The above description is merely a preferred embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any equivalent substitutions or modifications made by those skilled in the art within the scope of the technology disclosed in the present invention, based on the technical solution and inventive concept of the present invention, should be covered within the scope of protection of the present invention.
Claims
1. A method for preparing ZnO@In2O3 reinforced silver-based composite materials by powder metallurgy, characterized in that, Includes the following steps: S1. Using ZnO powder as raw material, ZnO@In2O3 powder is obtained through a combination of electrolysis and sintering. S2. The ZnO@In2O3 powder obtained in step S1 is mixed with Ag powder at a mass ratio of (4-9):50, and then ball-milled to obtain composite powder. S3. Press the composite powder obtained in step S2 into a mold; sinter it in a sintering furnace to form a ZnO@In2O3 reinforced silver-based composite material sintered blank; then densify the sintered blank, extrude it, and draw it into wire. In step S1, the specific preparation method of ZnO@In2O3 powder is as follows: S11. Electrolysis is carried out in an electrolyte with an indium plate as the anode and a graphite electrode as the cathode until the indium plate at the anode is completely electrolyzed and disappears in the electrolyte. S12. Add ZnO powder to the electrolyte at a ratio of 10-60 g / L and stir for 3-10 min; after centrifuging the electrolyte, wash it 3-5 times with deionized water at a volume ratio of 10:
1. S13. Dry in a drying oven at 60-120℃ for 5-20 hours, then grind and pass through a 200-800 mesh sieve to obtain white powder In(OH)3; S14. The ZnO@In2O3 powder is prepared by sequentially holding the powder at 300℃ for 1-2 hours, at 400℃ for 1-4 hours, and at 500℃ for 1-2 hours, followed by calcination.
2. The method for preparing ZnO@In2O3 reinforced silver-based composite materials by powder metallurgy according to claim 1, characterized in that, In step S11, the electrolyte is prepared by dissolving NH4Cl in deionized water; and the current density during electrolysis is 0.2–0.9 A / cm². 2 .
3. The method for preparing ZnO@In2O3 reinforced silver-based composite materials by powder metallurgy according to claim 1, characterized in that, The ZnO powder has a particle size of 50–1000 nm, a purity of ≥99.9%, and a sphericity of ≥0.9; the ZnO@In2O3 powder has a particle size of 60–1100 nm and a sphericity of ≥0.
9.
4. The method for preparing ZnO@In2O3 reinforced silver-based composite materials by powder metallurgy according to claim 1, characterized in that, In step S2, the Ag powder has a particle size of 10–50 µm and a purity of ≥99.9%, and the ball milling process involves a rotation speed of 150–700 r / min and a time of 0.5–2 h.
5. The method for preparing ZnO@In2O3 reinforced silver-based composite materials by powder metallurgy according to claim 1, characterized in that, In step S3, the pressure during the pressing process is 150–800 MPa; the sintering process adopts a multi-stage sintering-holding method, with sintering and holding temperatures ranging from 100 to 850°C; the extrusion temperature is 300–850°C, and the extrusion pressure is 200–800 MPa.
Citation Information
Patent Citations
Method for preparing silver zinc oxide composite material
CN101638732A
ZnO-coated In2O3 reinforced silver-based composite material and preparation method thereof
CN117026004A
Process for preparation of indium oxide-tin oxide powder
US5417816A