A non-woven fabric-based lithium battery separator and a preparation method thereof
By using polypropylene nonwoven fabrics and fiber magnesium or aluminum trioxide in lithium battery separators, combined with ion implantation polydimethylsiloxane technology, the low conductivity and heat of lithium battery separators are solved. Stability issues improve the puncture strength and breathability of the diaphragm, preventing battery short circuit and bulging.
Patent Information
- Application Number
- CN202410727141.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-06
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-06-06
AI Technical Summary
The existing lithium battery separators have poor ionic conductivity, low puncture resistance and low thermal stability, which can easily cause the battery to be short-circuited, burned or exploded during overcharge or high temperatures.
Polypropylene non-woven fabric is used as the substrate to coat reinforcement fillers such as fiber magnesium or aluminum trioxide, and prepare coatings by ion implantation of polydimethylsiloxane to improve the puncture strength, thermal stability of the membrane and Ion conductivity.
It significantly improves the puncture strength, thermal stability and ionic conductivity of the diaphragm, reduces the heat shrinkage, prevents battery short circuit caused by contact with positive and negative electrodes, and enhances the breathability and ionic transmittance of the diaphragm.
Smart Images

Figure BDA0004878978930000081
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of lithium battery separators, and in particular relates to a non-woven fabric-based lithium battery separator and a preparation method thereof. Background Art
[0002] Lithium battery separator is a porous film used to separate the positive and negative electrodes and prevent battery short circuit. Currently, the most commonly used films are based on polyolefin materials, such as polyethylene film and polypropylene film. However, polyolefin films have poor ion conductivity, low puncture resistance, and low thermal stability. When overcharged or at high temperature, they are prone to cause battery short circuit, and then combustion or explosion.
[0003] Patent publication number CN104953073A discloses a method for manufacturing a diaphragm lithium battery. The diaphragm lithium battery includes a shell, a positive electrode material, a negative electrode material and a diaphragm; a positive electrode column is inserted into the positive electrode material, and a negative electrode column is inserted into the negative electrode material; a protective layer is also installed between the negative electrode material and the diaphragm; the protective layer includes two parallel throttle plates that can slide back and forth along the bottom and top surfaces of the shell and a fixed net located between the two throttle plates; sliding blocks are installed on the upper and lower edges of the throttle plates, and the sliding blocks match the slide grooves opened on the top and bottom surfaces of the shell; the fixed net A throttling ball made of heat expansion material is fixed on each node; a throttling hole is provided at the position opposite to each throttling ball on the two throttling plates, and the diameter of the throttling hole is smaller than the diameter of the throttling ball; in a natural state, a hole end face of the throttling hole close to the throttling ball is tangent to the throttling ball, and each pair of the sliding blocks on the same bottom and top surfaces of the shell are tightly fitted together; an air outlet one-way valve is provided on the shell, and the air outlet one-way valve is opposite to the position of the sliding block; a liquid-sealed exhaust valve is also provided on the throttling plate. The above technology still has some defects, such as low conductivity of the diaphragm, poor wettability and thermal stability, shrinkage and deformation of the diaphragm at high temperature, and low battery capacity retention rate. Therefore, a lithium battery diaphragm with low thermal shrinkage, high puncture strength, high ion conductivity, high air permeability and a preparation method thereof are needed. Summary of the invention
[0004] The purpose of the present invention is to provide a non-woven fabric-based lithium battery separator and a preparation method thereof, so as to solve the problem that lithium batteries are prone to short circuit.
[0005] The purpose of the present invention can be achieved through the following technical solutions:
[0006] A non-woven fabric-based lithium battery separator, the non-woven fabric-based lithium battery separator comprising: a substrate and a coating, the substrate being a polypropylene non-woven fabric, the coating comprising the following raw materials in weight percentage: 35% to 38% reinforcing filler, 1% to 1.5% dispersant, 16% to 16.5% binder, 1% to 1.6% high molecular polymer and 43% to 46% deionized water.
[0007] Preferably, the reinforcing filler is one of fibrous brucite and aluminum oxide. The particle size of fibrous brucite is 30-35 μm, and the particle size of aluminum oxide is 10-15 nm. The purpose is to reduce the thermal shrinkage of the diaphragm, improve the puncture strength and ion conductivity of the diaphragm, prevent the positive and negative electrodes from contacting and causing a short circuit in the battery, and improve the battery performance.
[0008] Preferably, the high molecular polymer is ion-implanted polydimethylsiloxane, in order to improve the air permeability and ion conductivity of the diaphragm, prevent battery bulging, and improve battery performance.
[0009] Preferably, the ion-implanted polydimethylsiloxane is prepared by the following steps:
[0010] Ar + The Ga + The ion implantation device is used to implant the polydimethylsiloxane to obtain ion implanted polydimethylsiloxane.
[0011] Preferably, the Ar + The energy is 28-32keV and the dose is 1x10 15 ~5x10 15 ions / cm 2 .
[0012] Preferably, the Ga + The energy is 60-64 keV and the dose is 1x10 17 ~5x10 17 ions / cm 2 .
[0013] A method for preparing a non-woven fabric-based lithium battery separator comprises the following steps:
[0014] The first step is to prepare a coating by mixing reinforcing filler, high molecular polymer, dispersant, binder and deionized water;
[0015] The second step is to apply the coating on the substrate and dry it to obtain a non-woven fabric-based lithium battery separator.
[0016] Preferably, the thickness of the substrate is 6-16 μm, and the thickness of the coating is 2-3 μm. The purpose is to reduce the thermal shrinkage of the diaphragm, improve the puncture strength of the diaphragm, increase the safety performance of the diaphragm, and at the same time improve the capacity, energy and energy density of the battery.
[0017] Preferably, the drying temperature in the second step is 80-100° C. and the drying time is 2-3 hours, in order to fix the coating on the substrate.
[0018] Beneficial effects of the present invention:
[0019] The present invention uses reinforcing fillers, high molecular polymers, dispersants, binders and deionized water to prepare coatings, and the method of coating the substrate surface to prepare a non-woven fabric-based lithium battery separator, thereby improving the puncture strength, thermal stability, ion conductivity and air permeability of the separator. Compared with the previous technology, the present invention uses reinforcing fillers and ion-implanted polydimethylsiloxane to prepare the coating. On the one hand, the reinforcing filler has a higher tensile strength and toughness to prevent the lithium dendrites of the negative electrode of the lithium battery from piercing the separator, and the reinforcing filler has a higher thermal stability to prevent the separator from shrinking and deforming at high temperatures. On the other hand, the ion-implanted polydimethylsiloxane has a higher gas permeability and conductivity to improve the air permeability and ion conductivity of the separator.
[0020] The present invention adds ion-implanted polydimethylsiloxane, which has Si iOSi bonds, resulting in weak intermolecular interaction forces and high gas permeability, which is beneficial to improving the air permeability of the diaphragm. At the same time, the internal molecular gaps of the ion-implanted polydimethylsiloxane are increased, the free volume is increased, which is beneficial to the migration of ions, and the charge jumping between the chain links generates conductive current, which is beneficial to increasing the ionic conductivity of the diaphragm. The ion-implanted polydimethylsiloxane also has a high hardness, which is beneficial to improving the puncture strength of the diaphragm.
[0021] The reinforcing filler in the present invention is selected from fibrous brucite or aluminum oxide, which has high tensile strength and toughness, can effectively inhibit the puncture of lithium dendrites, and has a thermal stability far higher than that of polyolefin separators, so that the separator has a lower thermal shrinkage rate at high temperature, which can effectively prevent the positive and negative electrodes from contacting and causing a short circuit in the battery. At the same time, the porous coating prepared by the porous coating can absorb a large amount of electrolyte, reduce the transmission resistance of lithium ions, and enhance the ionic conductivity of the separator.
[0022] In the present invention, reinforcing fillers and ion-implanted polydimethylsiloxane are combined to prepare lithium battery diaphragm coatings, the excellent mechanical properties of the reinforcing fillers and the higher hardness of the ion-implanted polydimethylsiloxane are used to improve the puncture strength of the diaphragm, the lower transmission resistance of the reinforcing fillers and the higher conductivity of the ion-implanted polydimethylsiloxane are used to improve the ionic conductivity of the diaphragm, and the reinforcing fillers can also reduce the thermal shrinkage of the diaphragm, and the ion-implanted polydimethylsiloxane can also improve the air permeability of the diaphragm.
[0023] When preparing a non-woven fabric-based lithium battery separator, the present invention not only increases the puncture resistance and thermal stability of the separator, effectively preventing the positive and negative electrodes of the lithium battery from contacting each other and causing a battery short circuit, but also improves the air permeability and ion conductivity of the separator, preventing gas accumulation in the lithium battery and causing battery bulging, and enhancing the ion permeability of the separator. DETAILED DESCRIPTION
[0024] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0025] Example 1
[0026] Ion-implanted polydimethylsiloxane was prepared by the following steps:
[0027] The energy is 30 keV and the dose is 1x10 15 i ons / cm 2 Ar + The ion implanter was used to implant polydimethylsiloxane, the molecular weight of which was 100,000, and then the energy was 62 keV and the dose was 1x10 17 i ons / cm 2 Ga + The ion implantation device is used to implant the polydimethylsiloxane to obtain ion implanted polydimethylsiloxane.
[0028] Example 2
[0029] Ion-implanted polydimethylsiloxane was prepared by the following steps:
[0030] The energy is 30 keV and the dose is 3x10 15 i ons / cm 2 Ar + The ion implanter was used to implant polydimethylsiloxane, the molecular weight of which was 100,000, and then the energy was 62 keV and the dose was 3x10 17 i ons / cm 2 Ga + The ion implantation device is used to implant the polydimethylsiloxane to obtain ion implanted polydimethylsiloxane.
[0031] Example 3
[0032] Ion-implanted polydimethylsiloxane was prepared by the following steps:
[0033] The energy is 30 keV and the dose is 5x10 15 i ons / cm 2 Ar + The ion implanter was used to implant polydimethylsiloxane, the molecular weight of which was 100,000, and then the energy was 62 keV and the dose was 5x10 17 i ons / cm 2 Ga + The ion implantation device is used to implant the polydimethylsiloxane to obtain ion implanted polydimethylsiloxane.
[0034] Example 4
[0035] This embodiment provides a method for preparing a non-woven fabric-based lithium battery separator, and the specific steps are as follows:
[0036] 35 g of fiber brucite with a particle size of 30 to 35 μm, 1.5 g of ion-implanted polydimethylsiloxane in Example 2, 1.5 g of polyvinyl alcohol with an average molecular weight of 18,000 and 16 g of polyvinylidene fluoride with an average molecular weight of 400,000 were added to 46 g of deionized water and stirred for 15 minutes to obtain a coating.
[0037] The coating was applied to the surface of a polypropylene non-woven fabric with a thickness of 10 μm to a thickness of 2 μm, and dried at a drying temperature of 90° C. for 2 hours to obtain a non-woven fabric-based lithium battery separator.
[0038] Example 5
[0039] This embodiment provides a method for preparing a non-woven fabric-based lithium battery separator, and the specific steps are as follows:
[0040] 36 g of fibrous brucite with a particle size of 30 to 35 μm, 1.5 g of ion-implanted polydimethylsiloxane in Example 2, 1.5 g of polyvinyl alcohol with an average molecular weight of 18,000 and 16 g of polyvinylidene fluoride with an average molecular weight of 400,000 were added to 45 g of deionized water and stirred for 15 minutes to obtain a coating.
[0041] The coating was applied to the surface of a polypropylene non-woven fabric with a thickness of 10 μm to a thickness of 2 μm, and dried at a drying temperature of 90° C. for 2 hours to obtain a non-woven fabric-based lithium battery separator.
[0042] Example 6
[0043] This embodiment provides a method for preparing a non-woven fabric-based lithium battery separator, and the specific steps are as follows:
[0044] 38 g of fiber brucite with a particle size of 30 to 35 μm, 1.5 g of ion-implanted polydimethylsiloxane in Example 2, 1.5 g of polyvinyl alcohol with an average molecular weight of 18,000 and 16 g of polyvinylidene fluoride with an average molecular weight of 400,000 were added to 43 g of deionized water and stirred for 15 minutes to obtain a coating.
[0045] The coating was applied to the surface of a polypropylene non-woven fabric with a thickness of 10 μm to a thickness of 2 μm, and dried at a drying temperature of 90° C. for 2 hours to obtain a non-woven fabric-based lithium battery separator.
[0046] Example 7
[0047] This embodiment provides a method for preparing a non-woven fabric-based lithium battery separator, and the specific steps are as follows:
[0048] 36 g of fiber brucite with a particle size of 30-35 μm, 1.5 g of ion-implanted polydimethylsiloxane in Example 1, 1.5 g of polyvinyl alcohol with an average molecular weight of 18,000 and 16 g of polyvinylidene fluoride with an average molecular weight of 400,000 were added to 45 g of deionized water and stirred for 15 minutes to obtain a coating.
[0049] The coating was applied to the surface of a polypropylene non-woven fabric with a thickness of 10 μm to a thickness of 2 μm, and dried at a drying temperature of 90° C. for 2 hours to obtain a non-woven fabric-based lithium battery separator.
[0050] Example 8
[0051] This embodiment provides a method for preparing a non-woven fabric-based lithium battery separator, and the specific steps are as follows:
[0052] 36 g of fiber brucite with a particle size of 30-35 μm, 1.5 g of ion-implanted polydimethylsiloxane in Example 3, 1.5 g of polyvinyl alcohol with an average molecular weight of 18,000 and 16 g of polyvinylidene fluoride with an average molecular weight of 400,000 were added to 45 g of deionized water and stirred for 15 minutes to obtain a coating.
[0053] The coating was applied to the surface of a polypropylene non-woven fabric with a thickness of 10 to 15 μm, the coating thickness was 2 μm, and the coating was dried at a temperature of 90° C. for 2 hours to obtain a non-woven fabric-based lithium battery separator.
[0054] Example 9
[0055] This embodiment provides a method for preparing a non-woven fabric-based lithium battery separator, and the specific steps are as follows:
[0056] 38 g of aluminum oxide with a particle size of 10 nm, 1.5 g of ion-implanted polydimethylsiloxane in Example 2, 1.5 g of polyvinyl alcohol with an average molecular weight of 18,000 and 16 g of polyvinylidene fluoride with an average molecular weight of 400,000 were added to 43 g of deionized water and stirred for 15 minutes to obtain a coating.
[0057] The coating was applied to the surface of a polypropylene non-woven fabric with a thickness of 10 μm to a thickness of 2 μm, and dried at a drying temperature of 90° C. for 2 hours to obtain a non-woven fabric-based lithium battery separator.
[0058] Comparative Example 1
[0059] In this comparative example, a polypropylene non-woven fabric with a thickness of 12 μm is used as a lithium battery separator.
[0060] Comparative Example 2
[0061] Compared with Example 6, the reinforcing filler in the coating is attapulgite, and the specific steps are as follows:
[0062] 38 g of attapulgite with a particle size of 0.5 to 5 μm in length and 20 to 70 nm in diameter, 1.5 g of the ion-implanted polydimethylsiloxane in Example 2, 1.5 g of polyvinyl alcohol with an average molecular weight of 18,000 and 16 g of polyvinylidene fluoride with an average molecular weight of 400,000 were added to 43 g of deionized water and stirred for 15 minutes to obtain a coating.
[0063] The coating was applied to the surface of a 10 μm thick polypropylene non-woven fabric to a thickness of 2 μm, and dried at a drying temperature of 90°C for 2 hours to obtain a non-woven fabric-based lithium battery separator. The non-woven fabric-based lithium battery separator was tested for its thermal shrinkage, puncture strength, ionic conductivity and air permeability.
[0064] Comparative Example 3
[0065] Compared with Example 5, this comparative example does not add ion-implanted polydimethylsiloxane to the coating, and the specific steps are as follows:
[0066] 36 g of fiber brucite with a particle size of 30-35 μm, 1.5 g of polyvinyl alcohol with an average molecular weight of 18,000, and 16 g of polyvinylidene fluoride with an average molecular weight of 400,000 were added to 46.5 g of deionized water and stirred for 15 minutes to obtain a coating.
[0067] The coating was applied to the surface of a polypropylene non-woven fabric with a thickness of 10 μm to a thickness of 2 μm, and dried at a drying temperature of 90° C. for 2 hours to obtain a non-woven fabric-based lithium battery separator.
[0068] Comparative Example 4:
[0069] Compared with Example 5, the high molecular weight polymer in the coating is polydimethylsiloxane, and the specific steps are as follows:
[0070] 36 g of fiber brucite with a particle size of 30-35 μm, 1.5 g of polydimethylsiloxane, 1.5 g of polyvinyl alcohol with an average molecular weight of 18,000 and 16 g of polyvinylidene fluoride with an average molecular weight of 400,000 were added to 45 g of deionized water and stirred for 15 minutes to obtain a coating.
[0071] The coating was applied to the surface of a polypropylene non-woven fabric with a thickness of 10 μm to a thickness of 2 μm, and dried at a drying temperature of 90° C. for 2 hours to obtain a non-woven fabric-based lithium battery separator.
[0072] Note: Thermal shrinkage, puncture strength. The test method for ionic conductivity is: measured according to the recording method in GBT36363-2018 "Polyolefin separator for lithium-ion batteries", and the thermal shrinkage test condition is maintained at 90°C for 2 hours.
[0073] The test method for air permeability is: under a pressure of 1.22 kPa, test the time required for 100 ml of air to pass through a 1 square inch diaphragm.
[0074] Performance tests were performed on Examples 4 to 6 and Comparative Examples 1 to 3, and the results are shown in Table 1:
[0075] Table 1
[0076]
[0077] It can be seen from Table 1 that when preparing non-woven fabric-based lithium battery separators, polypropylene non-woven fabric is used as the substrate, and a coating prepared by fiber brucite, ion-implanted polydimethylsiloxane, polyvinyl alcohol, polyvinylidene fluoride and deionized water is coated on the substrate. This can reduce the thermal shrinkage of the separator, improve the thermal stability of the separator, and enhance the puncture strength, ionic conductivity and air permeability of the separator.
[0078] It can be seen from Examples 4-6 that when preparing the coating, when the mass fraction of fiber brucite is in the range of 35% to 38%, increasing the content of fiber brucite improves the thermal shrinkage, puncture strength and ion conductivity of the diaphragm, but the air permeability of the diaphragm decreases.
[0079] It can be seen from Examples 5 and 7-8 that when preparing ion-implanted polydimethylsiloxane, increasing the amount of Ar injected into the polydimethylsiloxane + and Ga + The puncture strength and ionic conductivity of the membrane increased with the dose of Ar ion implanted into polydimethylsiloxane. + and Ga +The concentration has little effect on the thermal shrinkage and air permeability of the diaphragm.
[0080] It can be seen from Example 4 and Comparative Example 1 that coating the surface of the substrate can improve the puncture strength and ion conductivity of the diaphragm and reduce the thermal shrinkage of the diaphragm, but the coating will hinder the passage of gas through the diaphragm and reduce the air permeability of the diaphragm.
[0081] It can be seen from Example 6, Example 9 and Comparative Example 2 that the type of reinforcing filler in the coating has a great influence on the thermal shrinkage, puncture strength and ionic conductivity of the diaphragm. Adding reinforcing fillers to the coating can improve the thermal shrinkage, puncture strength and ionic conductivity of the diaphragm. Compared with attapulgite, fibrous brucite and alumina have a higher improvement on the thermal shrinkage, puncture strength and ionic conductivity of the diaphragm.
[0082] It can be seen from Example 5 and Comparative Examples 3-4 that adding ion-implanted polydimethylsiloxane to the coating can enhance the puncture strength, air permeability and ion conductivity of the diaphragm. Polydimethylsiloxane that has not been modified by ion implantation can improve the air permeability of the diaphragm, but has little effect on the puncture strength and ion conductivity of the diaphragm.
[0083] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.
[0084] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A non-woven fabric-based lithium battery separator, characterized in that: The non-woven fabric-based lithium battery separator comprises: a substrate and a coating, wherein the substrate is a polypropylene non-woven fabric, and the coating comprises the following raw materials in weight percentage: 35% to 38% reinforcing filler, 1% to 1.5% dispersant, 16% to 16.5% binder, 1% to 1.6% high molecular polymer and 43% to 46% deionized water; The reinforcing filler is one of fiber brucite and aluminum oxide, the particle size of the fiber brucite is 30-35 μm, and the particle size of the aluminum oxide is 10-15 nm; The high molecular polymer is ion-implanted polydimethylsiloxane; The ion-implanted polydimethylsiloxane is prepared by the following steps: Ar + The Ga + The ion implantation device is used to implant the polydimethylsiloxane to obtain ion implanted polydimethylsiloxane.
2. A non-woven fabric-based lithium battery separator according to claim 1, characterized in that: The Ar + The energy is 28-32keV and the dose is 1x10 15 ~5x10 15 ions / cm 2 ; The Ga + The energy is 60-64 keV and the dose is 1x10 17 ~5x10 17 ions / cm 2 .
3. The method for preparing a non-woven fabric-based lithium battery separator according to claim 1, characterized in that: The following steps are involved: The first step is to prepare a coating by mixing reinforcing filler, high molecular polymer, dispersant, binder and deionized water; The second step is to apply the coating on the substrate and dry it to obtain a non-woven fabric-based lithium battery separator.
4. The method for preparing a non-woven fabric-based lithium battery separator according to claim 3, characterized in that: The thickness of the substrate is 6-16 μm, and the thickness of the coating is 2-3 μm.
5. The method for preparing a non-woven fabric-based lithium battery separator according to claim 3, characterized in that: In the second step, the drying temperature is 80-100°C and the drying time is 2-3 hours.