Narrow-dispersion nano binder for lithium battery diaphragm as well as preparation method and application of narrow-dispersion nano binder

By using an oxidation-reduction initiation system in lithium-ion battery separator, the seed emulsion polymerization is initiated at low temperature, the pH value and stirring speed are controlled, and narrow dispersed nanobinder is prepared, which solves the problem of insufficient thermal shrinkage and bonding strength of traditional separators, and improves the The heat resistance and stability of the diaphragm ensure the safety of lithium batteries.

CN118995091APending Publication Date: 2024-11-22SHANGHAI DINHO NEW MATERIAL TECH CO LTD +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411106883.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The traditional lithium-ion battery separator has a short circuit of the positive and negative electrodes due to the thermal shrinkage of the polyolefin microporous membrane at high temperatures, causing safety hazards. The particle size distribution of the water-based adhesive of the ceramic separator is unstable, reducing the bonding strength.

Method used

The oxidation-reduction initiation system is used to induce seed emulsion polymerization at low temperature in an inert gas environment, control the pH value of the pre-emulsion and stirring speed, prepare narrow dispersed nanobinders, reduce latex particle collision and polymerization instability, and form narrowly distributed nanoemulsions. particle.

Benefits of technology

The bonding strength between the ceramic coating and the separator is improved, the heat shrinkage rate is reduced, the heat resistance and stability of the separator is enhanced, and the safety of the lithium battery is ensured.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004991082480000051
    Figure BDA0004991082480000051
  • Figure BDA0004991082480000061
    Figure BDA0004991082480000061
  • Figure BDA0004991082480000062
    Figure BDA0004991082480000062
Patent Text Reader

Abstract

The invention relates to the technical field of lithium ion batteries, and particularly discloses a narrow-dispersion nano binder for a lithium battery diaphragm as well as a preparation method and application of the narrow-dispersion nano binder. A preparation method of a narrow-dispersion nano binder for a lithium battery diaphragm comprises the following steps: mixing water, an emulsifier and a pH regulator, firstly adding a monomer, and then introducing inert gas to remove air to obtain a pre-emulsion; adding an initiator aqueous solution into a part of the pre-emulsion to obtain an initiation solution; stirring the initiation solution for reaction to obtain a seed solution; and adding the residual pre-emulsion into the seed solution, preserving heat, stirring, and filtering to obtain the narrow-dispersion nano binder for the lithium battery diaphragm. The narrow-dispersion nano binder for the lithium battery diaphragm meets the narrow-distribution particle size control requirement, is relatively high in stability, and can improve the overall stripping force of a ceramic coating and the puncture strength of the diaphragm, reduce the thermal shrinkage rate of the diaphragm and improve the stability of the lithium battery diaphragm when being applied to the lithium battery diaphragm.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of lithium-ion batteries, and more specifically, to a narrow-dispersion nano-binder for lithium battery separators, and a preparation method and application thereof. Background Art

[0002] At present, lithium-ion batteries have become the mainstream technology in the current battery field due to their high energy density, long cycle life and low self-discharge rate. They have broad market application prospects in electric vehicles, power tools, 3C electronics, new energy storage and other industries. The main components of lithium batteries include positive electrodes, negative electrodes, diaphragms, electrolytes, etc. Among them, the diaphragm refers to a thin layer of porous material between the positive and negative electrodes of the battery. It is a very critical part of the battery and has a direct impact on the safety and cost of the battery.

[0003] Traditional battery separators are mainly porous organic polymer membranes. Typical organic polymer membranes are polyolefin microporous membranes, such as polyethylene microporous membranes and polypropylene microporous membranes. However, when the temperature is high, the polyolefin microporous membrane will shrink greatly, causing the separator to lose its barrier function between the positive and negative electrodes, thereby causing a short circuit between the positive and negative electrodes inside the battery, causing the battery to burn or even explode, creating a safety hazard. Therefore, improving the thermal stability of the separator is an important guarantee for the safety of lithium-ion batteries. Since functional materials such as ceramics are coated on the separator, the heat resistance and stability of the separator can be improved. Therefore, as a key material for coating ceramic slurry on the separator, the binder has a crucial impact on the performance of the ceramic separator.

[0004] The current water-based binder for ceramic diaphragms is mainly an acrylate copolymer emulsion, which mainly uses an initiator to initiate monomer polymerization under high-temperature stirring conditions to form a large number of latex particles, thereby obtaining an acrylate copolymer emulsion. However, under high-temperature stirring conditions, latex particles are prone to collision and agglomeration, and a large number of secondary agglomerated particles are generated during the long-term stirring process, which increases the particle size of the latex particles and causes a bimodal or multimodal distribution of the particle size. Since large-sized latex particles are prone to sedimentation, stratification, coagulation and other changes, the stability of the acrylate copolymer emulsion is reduced, resulting in poor film-forming properties, thereby reducing the bonding strength between the ceramic slurry and the diaphragm. Summary of the invention

[0005] In order to reduce the particle size of the aqueous binder of the ceramic diaphragm and improve the bonding strength between functional materials such as ceramics and the diaphragm, the present application provides a narrow dispersion nano binder for lithium battery diaphragms, and a preparation method and application thereof.

[0006] In the first aspect, the present application provides a method for preparing a narrow dispersion nano binder for a lithium battery separator, using the following technical solution: A narrow dispersion nano binder for lithium battery separator, comprising the following steps: S1: After mixing water, an emulsifier and a pH adjuster, first add the monomer, stir and mix, then introduce an inert gas to exclude air, stir and mix, and obtain a pre-emulsion; The pH value of the pre-emulsion is 6.5-9.0; S2: Under an inert gas environment, first add an initiator aqueous solution to a pre-emulsion at 30-35° C. and accounting for 10-20% of the total weight of the pre-emulsion, and stir to react to obtain an initiator solution; The initiator in the initiator aqueous solution is an oxidation-reduction initiator; S3: stirring the initiating liquid to react in an inert gas environment to obtain a seed liquid; S4: Under an inert gas environment, the remaining pre-emulsion is added to the seed solution at 35-40°C and 220-260r / min within 180-240min, the reaction is stirred at 220-240r / min, the heat is kept, and the filter is used to obtain a narrow dispersion nano binder for lithium battery separators.

[0007] By adopting the above technical scheme and the oxidation-reduction initiation system, the activation energy of the free radical polymerization reaction can be reduced. Then, the air can be removed by introducing an inert gas to prevent oxygen from dissolving in the latex foam formed by high-speed stirring during emulsification, thereby increasing the activity of free radicals and allowing the initiator to initiate monomer polymerization at a low temperature of 30-35°C.

[0008] On the one hand, by lowering the polymerization temperature, the phenomenon of widening of particle size distribution caused by the increase of particle size due to secondary agglomeration of latex particles can be reduced, and the stability of latex particles can be improved. Therefore, the D90 of the obtained nano latex particles is as low as 473-595nm, and has a narrow particle size range; on the other hand, low-temperature reaction can also prevent the self-acceleration phenomenon caused by heat release during free radical polymerization, thereby reducing the generation of particles and blocks and improving the raw material conversion rate; and low-temperature reaction can also reduce the amount of emulsifier used, thereby reducing the effect of emulsifier on the foam generated during the ceramic slurry coating cycle.

[0009] At the same time, by controlling the pH value of the pre-emulsion system within the range of 6.5-9.0, the polymerization rate of the initiator and the monomer can be controlled, which is conducive to obtaining stable latex particles with narrow distribution.

[0010] Preferably, the method for preparing the narrow dispersion nano binder for lithium battery separator comprises the following steps: S1: After mixing water, emulsifier and pH adjuster, first add monomer, stir and mix at 100-120r / min, then introduce inert gas to exclude air, and stir and mix at 450-550r / min for 15-20min under inert gas environment to obtain pre-emulsion; S2: Under an inert gas environment, first add an initiator aqueous solution to a pre-emulsion at 30-35° C. and accounting for 10-20% of the total weight of the pre-emulsion, and stir at 180-220 r / min for 20-40 minutes to obtain an initiator solution; S3: Under an inert gas environment, stirring the initiating liquid at 35-40° C. and 200-240 r / min for 60-90 min to obtain a seed liquid; S4: Under an inert gas environment, add the remaining pre-emulsion to the seed solution at 35-40°C and 220-260r / min within 180-240min, stir at 220-240r / min for 120-180min, filter, and obtain a narrow dispersion nano binder for lithium battery separator.

[0011] In the process of the initiator initiating the polymerization of monomers to form latex particles, the latex particles will gradually increase in size, and the viscosity of the latex polymerization will increase in the later stage. By adopting the above technical solution, appropriately increasing the rotation speed in the middle stage of polymerization is beneficial to increasing the mass transfer and heat transfer effect; in the insulation stage, as the monomer concentration decreases, the reaction heat release decreases, and the rotation speed is appropriately reduced again. If the rotation speed is too low in the middle stage of polymerization, the local temperature will be too high due to poor heat transfer, resulting in unstable polymerization results such as explosion or solidification; if the rotation speed is too high, the probability of latex particle collision will increase, resulting in an increase in particle size or a divergence in particle size distribution, making it easy for the particles to agglomerate to produce particles or lumps. The scheme of segmented speed control is conducive to minimizing the probability of latex particle collision, improving the stability of latex particles, and ultimately forming narrowly dispersed nano latex particles.

[0012] Preferably, in step S2, the initiator aqueous solution is first added into a pre-emulsion at 30-35° C. and accounting for 15% of the total weight of the pre-emulsion, and the mixture is stirred at 200-220 r / min for 20-40 min to obtain an initiator solution.

[0013] In step S2, 15% of the pre-emulsion is used as a primer pre-emulsion, which is reacted with an initiator to prepare a seed solution. In the present application, the weight ratio of the primer pre-emulsion will affect the particle size and distribution of the final binder. If the primer emulsion ratio is too low, there will be too few latex particles in the formed seed solution, the space provided for emulsion polymerization will be reduced, and the particle size of the resulting polymer latex will be larger. If the primer emulsion ratio is too high, because there are certain differences in the reactivity rates of various types of monomers (such as acrylate monomers), when different types of monomers are copolymerized, it is difficult to form a copolymer according to the monomer ratio designed in the formula, and it is easy to produce a homopolymer mixture of different monomers, which ultimately affects the application performance of the binder, thereby affecting the mechanical properties of the diaphragm ceramic coating, such as the peeling force.

[0014] By adopting the above-mentioned technical scheme, since the present application adopts a pre-emulsion accounting for 15% of the total weight of the pre-emulsion as a base pre-emulsion, reacts with an initiator to prepare a seed liquid, and then combines the dripping process to carry out a controlled seed emulsion polymerization reaction under certain reaction temperature, dripping time, stirring speed and other conditions, not only narrowly distributed nano latex particles are obtained, but also the mechanical properties such as the peeling force of the diaphragm ceramic coating are greatly improved.

[0015] Preferably, in step S2, the oxidation-reduction initiator comprises an oxidant and a reductant, wherein the oxidant comprises any one of ammonium persulfate, sodium persulfate and potassium persulfate; and the reductant comprises any one of sodium bisulfite, sodium sulfite and sodium pyrosulfite.

[0016] Preferably, in the step S2, the weight ratio of the oxidant to the reductant is 10:(1-5).

[0017] Preferably, in step S1, the monomer comprises an acrylate monomer; and the weight ratio of the oxidant to the acrylate monomer is (5-20):1000.

[0018] Preferably, in step S1, the pH value of the pre-emulsion is 8.0-8.5.

[0019] Preferably, in the emulsifier aqueous solution of step S1, the weight ratio of emulsifier to water is (2-15):1000.

[0020] Since the present application adopts an oxidation-reduction initiator system, combined with inert gas protection, low-temperature initiation and low-temperature seed emulsion polymerization. Therefore, by adopting the above technical solution, controlling the weight ratio of the pH value regulator and the acrylate monomer, the reaction system (pre-emulsion) can be controlled at an appropriate pH value; at the same time, adding the initiator, emulsifier and monomer copolymerization according to the above weight ratio can effectively improve the stability of the latex particles during the emulsion synthesis process, reduce the collision probability of the latex particles during the synthesis process, and minimize the secondary agglomeration of the latex particles, thereby obtaining narrowly dispersed nano latex particles.

[0021] In the second aspect, the present application provides a narrow dispersion nano binder for lithium battery separators, which adopts the following technical solution: A narrow dispersion nano binder for lithium battery separator is prepared by the preparation method of the narrow dispersion nano binder for lithium battery separator.

[0022] By adopting the above technical scheme, the narrow dispersion nano binder for lithium battery separator prepared by the preparation method of the present application has a particle size distribution of D10: 123nm, D50: 220nm, D90: 473nm, D100: 817nm, which meets the narrow distribution particle size control requirements. Therefore, the narrow dispersion nano binder for lithium battery separator of the present application has good stability during the coating process, can form a uniform and stable coating, is conducive to improving the bonding strength between the ceramic coating and the separator, improving the puncture strength of the separator, reducing the thermal shrinkage rate, and improving the safety of the separator.

[0023] In a third aspect, the present application provides an application of a narrow dispersion nano binder for a lithium battery separator, using the following technical solution: The invention discloses an application of a narrow dispersion nano binder for lithium battery separator in lithium battery separator.

[0024] The prepared narrow dispersion nano binder for lithium battery separator is mixed with alumina ceramic particles, dispersant, thickener, wetting agent and deionized water according to conventional dosage ratio to form ceramic slurry, wherein the weight ratio of the total solid content of the ceramic slurry to the narrow dispersion nano binder for lithium battery separator is 1:0.06. The ceramic slurry is coated on a polyethylene separator with a thickness of 10nm, and the coating method is single-layer coating with a coating thickness of 4nm. After drying, a lithium battery separator can be obtained.

[0025] By adopting the above-mentioned technical scheme, the narrow dispersion nanobinder for lithium battery separator of the present application meets the requirements of narrow distribution particle size control, has high stability and excellent film-forming performance. When used in lithium battery separator, it can improve the bonding strength between the ceramic coating and the separator, so that the lithium battery separator has good heat resistance and stability.

[0026] In summary, this application has the following beneficial effects: 1. In the preparation method of the narrow dispersion nano binder for lithium battery separator of the present application, by using an oxidation-reduction initiator system to initiate seed emulsion polymerization at low temperature under inert gas, and controlling the process parameters such as the pH value of the reaction system, the dripping rate and the stirring speed, nano latex particles with narrow dispersion can be prepared; 2. The present application can effectively improve the stability of latex particles during the emulsion synthesis process and reduce the secondary agglomeration of latex particles by controlling the dosage of pH regulator, monomer, initiator, emulsifier and water, thereby obtaining narrowly dispersed nano latex particles; 3. The narrow dispersion nano binder for lithium battery separator of the present application has high stability and excellent film-forming performance. When used in lithium battery separator, it can not only improve the bonding strength between the ceramic coating and the separator, but also improve the peeling force of the ceramic coating and the puncture strength of the separator, and reduce the thermal shrinkage rate of the separator, which is beneficial to improve the heat resistance and stability of the lithium battery separator. DETAILED DESCRIPTION

[0027] The present application is further described in detail below with reference to the embodiments.

[0028] Performance Testing The narrow dispersion nano binder for lithium battery separator prepared in the embodiment of the present application and the binder prepared in the comparative example were tested for latex particle size distribution, and the test method was as follows: Latex particle size distribution: BT-9300H laser particle size distribution analyzer was used to detect the latex particle size distribution. Example

[0029] Example 1 A narrow dispersion nano binder for lithium battery separator, each raw material and its corresponding weight (g) are shown in the following table.

[0030] The method for preparing the narrow dispersion nano binder for lithium battery separator is characterized by comprising the following steps: S1: After mixing deionized water accounting for 95% of the total weight of deionized water, an emulsifier and a pH adjuster, first add an acrylate monomer and a functional monomer, stir and mix at 110 r / min, then introduce an inert gas to exclude air, and stir and mix at 500 r / min for 20 minutes under an inert gas environment to obtain a pre-emulsion; The pH value of the pre-emulsion was tested to be in the range of 8.0-8.5 (specifically 8.3); After the initiator and the remaining deionized water are mixed, an initiator aqueous solution is obtained.

[0031] S2: Under an inert gas environment, first add an initiator aqueous solution into a pre-emulsion at 32° C. and accounting for 15% of the total weight of the pre-emulsion, and stir at 200 r / min for 30 minutes to obtain an initiator solution; S3: Under an inert gas environment, the initiating solution was stirred at 38°C and 210r / min for 60min to obtain a seed solution; S4: Under an inert gas environment, the remaining pre-emulsion was added to the seed solution at 38°C and 240 r / min within 210 min. After the addition was completed, the mixture was kept warm and stirred at a speed of 230 r / min for 150 min, and passed through a 200-mesh sieve to obtain a narrow-dispersed nano-binder for lithium battery separators.

[0032] Example 2-3 A narrow dispersion nano binder for lithium battery separator, which is different from Example 1 in that the raw materials and their corresponding weights (g) are shown in the following table.

[0033] The narrow dispersion nano binder for lithium battery separator prepared in Examples 1-3 of the present application was tested for latex particle size distribution. The test results are shown in the following table.

[0034] By analyzing the data in the above table, it can be seen that the narrow dispersion nano binder for lithium battery separator prepared in Examples 1-3 of the present application has a narrow latex particle size distribution. This shows that in the preparation method of the narrow dispersion nano binder for lithium battery separator of the present application, when the weight ratio of the oxidant to the reductant is 10:(1-5) in step S2, a narrow dispersion nano binder for lithium battery separator with a narrow latex particle size distribution can be obtained.

[0035] Among them, the latex particle size of the narrow dispersion nano binder for lithium battery separator prepared in Example 1 is the smallest. Therefore, in the preparation method of the narrow dispersion nano binder for lithium battery separator of the present application, when the weight ratio of the oxidant to the reductant is 10:3 in step S2, the particle size of the narrow dispersion nano binder for lithium battery separator can be significantly reduced.

[0036] Embodiment 4-5 A narrow dispersion nano binder for lithium battery separator, which is different from Example 1 in that the raw materials and their corresponding weights (g) are shown in the following table.

[0037] The narrow dispersion nano binder for lithium battery separators prepared in Examples 1, 4, and 5 of the present application was tested for latex particle size distribution. The test results are shown in the following table.

[0038] By analyzing the data in the above table, it can be seen that in the preparation method of the narrow dispersion nanobinder for lithium battery separator of the present application, in step S2, when the weight ratio of the oxidant to the acrylate monomer is 1:100, the particle size of the obtained narrow dispersion nanobinder for lithium battery separator is the smallest.

[0039] Embodiment 6-7 A narrow dispersion nano binder for lithium battery separator, which is different from Example 1 in that the raw materials and their corresponding weights (g) are shown in the following table.

[0040] The narrow dispersion nano binder for lithium battery separator prepared in Examples 1, 6 and 7 of the present application was tested for latex particle size distribution. The test results are shown in the following table.

[0041] By analyzing the data in the above table, it can be seen that in the preparation method of the narrow dispersion nanobinder for lithium battery separator of the present application, in step S2, when the weight ratio of the emulsifier to water is 1:200, the particle size of the obtained narrow dispersion nanobinder for lithium battery separator is the smallest.

[0042] Example 8 A narrow dispersion nano binder for lithium battery separator, which is different from Example 1 in that in the preparation method of the narrow dispersion nano binder for lithium battery separator, in step S2, an initiator aqueous solution is first added to a pre-emulsion at 32° C. and accounting for 10% of the total weight of the pre-emulsion, and the reaction is stirred at 210 r / min for 20 minutes to obtain an initiator solution.

[0043] Example 9 A narrow dispersion nano binder for lithium battery separator, which is different from Example 1 in that in the preparation method of the narrow dispersion nano binder for lithium battery separator, in step S2, an initiator aqueous solution is first added to a pre-emulsion at 32° C. and accounting for 20% of the total weight of the pre-emulsion, and the reaction is stirred at 220 r / min for 40 minutes to obtain an initiator solution.

[0044] The narrow dispersion nano binder for lithium battery separator prepared in Examples 1, 8 and 9 of the present application was tested for latex particle size distribution. The test results are shown in the following table.

[0045] By analyzing the data in the above table, it can be seen that in the preparation method of the narrow dispersion nano binder for lithium battery separator of the present application, in step S2, when the mass proportion of the primer pre-emulsion is 15%, the particle size of the obtained binder is the smallest.

[0046] Example 10 A narrow dispersion nano binder for lithium battery separator, which is different from Example 1 in that the raw materials and their corresponding weights (g) are shown in the following table.

[0047] The method for preparing the narrow dispersion nano binder for the lithium battery separator comprises the following steps: S1: After mixing deionized water accounting for 95% of the total weight of deionized water, an emulsifier and a pH adjuster, first add an acrylate monomer and a functional monomer, stir and mix at 100 r / min, then introduce an inert gas to exclude air, and stir and mix at 450 r / min for 15 minutes under an inert gas environment to obtain a pre-emulsion; The pH value of the pre-emulsion was tested to be 6.5; After the initiator and the remaining deionized water are mixed, an initiator aqueous solution is obtained.

[0048] S2: Under an inert gas environment, first add an initiator aqueous solution into a pre-emulsion at 30° C. and accounting for 10% of the total weight of the pre-emulsion, and stir at 180 r / min for 20 minutes to obtain an initiator solution; S3: Under an inert gas environment, the initiating liquid was stirred at 35°C and 200 r / min for 60 min to obtain a seed liquid; S4: Under an inert gas environment, the remaining pre-emulsion was added to the seed solution at 35°C and 220 / min within 180 min. After the addition was completed, the mixture was stirred at a speed of 220 r / min for 120 min, and passed through a 200-mesh sieve to obtain a narrow-dispersed nano-binder for lithium battery separators.

[0049] Embodiment 11 A narrow dispersion nano binder for lithium battery separator, which is different from Example 1 in that the raw materials and their corresponding weights (g) are shown in the following table.

[0050] The method for preparing the narrow dispersion nano binder for the lithium battery separator comprises the following steps: S1: After mixing deionized water accounting for 95% of the total weight of deionized water, an emulsifier and a pH adjuster, first add an acrylate monomer and a functional monomer, stir and mix at 120 r / min, then introduce an inert gas to exclude air, and stir and mix at 520 r / min for 20 minutes under an inert gas environment to obtain a pre-emulsion; The pH value of the pre-emulsion was tested to be 9.0; After the initiator and the remaining deionized water are mixed, an initiator aqueous solution is obtained.

[0051] S2: Under an inert gas environment, first add an initiator aqueous solution to a pre-emulsion at 35° C. and accounting for 20% of the total weight of the pre-emulsion, and stir at 220 r / min for 40 minutes to obtain an initiator solution; S3: Under an inert gas environment, the initiating liquid was stirred at 40°C and 240 r / min for 90 min to obtain a seed liquid; S4: Under an inert gas environment, the remaining pre-emulsion was added to the seed solution at 40°C and 260 r / min within 240 min. After the addition was completed, the mixture was kept warm and stirred at a speed of 240 r / min for 180 min, and passed through a 200-mesh sieve to obtain a narrow-dispersed nano-binder for lithium battery separators.

[0052] The narrow dispersion nano binder for lithium battery separator prepared in Examples 1, 10 and 11 of the present application was tested for latex particle size distribution. The test results are shown in the following table.

[0053] By analyzing the data in the above table, it can be seen that the narrow dispersion nano binders for lithium battery separators prepared in Examples 1, 10, and 11 of the present application have a narrow particle size distribution. This shows that in the preparation method of the narrow dispersion nano binder for lithium battery separators of the present application, in step S1, by controlling the amount of the pH adjuster and the acrylate monomer added, the pH value of the pre-emulsion is adjusted within the range of 8.0-8.5, and then within the process parameter range requested for protection in S1-S4 of the present application, the narrow dispersion nano binder for lithium battery separators can be prepared.

[0054] Comparative Example Comparative Example 1 A binder, which is different from Example 1 in that in the preparation method of the binder, in step S2, an initiator aqueous solution is first added to a pre-emulsion at 32° C. and accounting for 5% of the total weight of the pre-emulsion, and the mixture is stirred at 220 r / min for 40 minutes to obtain an initiator solution.

[0055] Comparative Example 2 A binder, which is different from Example 1 in that in the preparation method of the binder, in step S2, an initiator aqueous solution is first added to a pre-emulsion at 32° C. and accounting for 25% of the total weight of the pre-emulsion, and the mixture is stirred at 220 r / min for 40 minutes to obtain an initiator solution.

[0056] Comparative Example 3 A binder, which is different from Example 1 in that the raw materials and their corresponding weights (g) are shown in the following table.

[0057] The preparation method of the above binder is the same as that of Example 1. Meanwhile, it was found through testing that the pH value of the pre-emulsion in the binder preparation method S1 was 5.0.

[0058] Comparative Example 4 A binder, which is different from Example 1 in that the raw materials and their corresponding weights (g) are shown in the following table.

[0059] The preparation method of the above binder is the same as that of Example 1. Meanwhile, it was found through testing that the pH value of the pre-emulsion in the binder preparation method S1 was 10.0.

[0060] Comparative Example 5 A binder, which is different from Example 1 in that, in the preparation method of the binder, step S4: under an inert gas environment, adding the remaining pre-emulsion to the seed solution at 38°C and 350 r / min within 210 minutes, after the dropwise addition is completed, stirring at a speed of 350 r / min for 150 minutes, and passing through a 200-mesh sieve to obtain the binder.

[0061] Comparative Example 6 A binder, which is different from Example 1 in that, in the preparation method of the binder, step S4: under an inert gas environment, adding the remaining pre-emulsion to the seed solution at 38°C and 200 r / min within 210 minutes, after the dropwise addition is completed, stirring at a speed of 200 r / min for 150 minutes, and passing through a 200-mesh sieve to obtain the binder.

[0062] Comparative Example 7 A binder, which is different from Example 1 in that, in the preparation method of the binder, under an inert gas environment, the remaining pre-emulsion is added to the seed liquid at 45-50°C (45°C for the comparative example of the present application) and 240r / min within 210min. After the dropwise addition is completed, the mixture is kept warm and stirred at a speed of 230r / min for 150min, and passed through a 200-mesh sieve to obtain the binder.

[0063] Comparative Example 8 A binder, which is different from Example 1 in that, in the method for preparing the binder, the amount of the reducing agent added is 0. Meanwhile, in the method for preparing the binder, step S4 is: Under an inert gas environment, the remaining pre-emulsion was added to the seed solution at 55-60°C (55°C for the comparative example of this application) and 240r / min within 210min. After the addition was completed, the mixture was stirred at a speed of 230r / min for 150min and passed through a 200-mesh sieve to obtain a binder.

[0064] Comparative Example 9 A binder, which is different from Example 1 in that, in the method for preparing the binder, steps S1, S2, S3, and S4 are not performed under an inert gas environment. Meanwhile, step S4 is: The remaining pre-emulsion was added to the seed solution at 65-70°C (65°C for the comparative example of the present application) and 240r / min within 210min. After the addition was completed, the mixture was stirred at a speed of 230r / min for 150min and passed through a 200-mesh sieve to obtain a binder.

[0065] Comparative Example 10 A binder, which is different from Example 1 in that, in the preparation method of the binder, steps S1, S2, S3, and S4 are not performed under an inert gas environment, and the amount of reducing agent added is 0. Meanwhile, step S4 is: The remaining pre-emulsion was added to the seed solution at 75-80°C (75°C for the comparative example of the present application) and 240r / min within 210min. After the addition was completed, the mixture was stirred at a speed of 230r / min for 150min and passed through a 200-mesh sieve to obtain a binder.

[0066] The latex particle size distribution test was performed on the narrow dispersion nano binder for lithium battery separator prepared in Example 1 of the present application and the binders prepared in Comparative Examples 1-10. The test results are shown in the following table.

[0067] By analyzing the data in the above table, it can be seen that compared with Example 1 using a primer pre-emulsion with a weight ratio of 15%, Comparative Example 1 using a primer pre-emulsion with a weight ratio of 5%, and Comparative Example 2 using a primer pre-emulsion with a weight ratio of 25%, the latex particle size is significantly increased. This shows that in the preparation method of the narrow dispersion nanobinder for lithium battery separators of the present application, step S2, using a pre-emulsion accounting for 10-20% of the total weight of the pre-emulsion as a primer pre-emulsion and copolymerizing it with an initiator to prepare an initiating solution, can significantly reduce the latex particle size. In particular, when a pre-emulsion accounting for 15% of the total weight of the pre-emulsion is used as a primer pre-emulsion and copolymerized with an initiator to prepare an initiating solution, the latex particle size is the lowest.

[0068] Compared with Example 1, the latex particle size of Comparative Examples 3 and 4 is significantly increased. This shows that in the preparation method of the narrow dispersion nanobinder for lithium battery separator of the present application, when the pH value of the pre-emulsion in step S1 is within the range of 8.0-8.5, the particle size of the latex particles can be reduced.

[0069] Compared with Example 1, the latex particle size of Comparative Examples 5 and 6 is significantly increased, which shows that the stirring speed also has a great influence on the particle size. When the speed is too low, the poor stirring heat transfer will cause local temperature rise and cause the latex particle size to increase instead; when the speed is too high, the latex particles will increase due to increased collisions, resulting in secondary agglomeration of the particles and causing the particle size to increase. This shows that in the preparation method of the narrow dispersion nanobinder for lithium battery separators of the present application, in step S4, the pre-emulsion and the seed liquid react and copolymerize under the condition of 220-260r / min, which can significantly reduce the latex particle size. Under the premise of ensuring normal heat and mass transfer reactions, a lower speed is conducive to reducing the particle size.

[0070] Compared with Example 1, the particle size of the latex in Comparative Examples 7-10 begins to increase significantly as the reaction temperature increases. This shows that in the preparation method of the narrow dispersion nanobinder for lithium battery separators of the present application, the pre-emulsion copolymerization is initiated at a relatively low temperature of 30-35°C using an oxidation-reduction initiator under an inert gas environment, which can effectively reduce the latex particle size. Analysis shows that the reason may be that as the polymerization reaction temperature increases, the stability of the latex particles decreases due to violent collisions, and the latex particles reunite for the second time, causing the latex particle size to increase significantly. It can be seen that initiating polymerization at a relatively low polymerization temperature in Example 1 of the present application is conducive to reducing the latex particle size.

[0071] At the same time, compared with Example 1, Comparative Examples 1-10, the D90 of the obtained nano latex particles is as high as 579-1578nm, and the particle size distribution range is relatively wide. Therefore, the narrow dispersion nano binder for lithium battery separator prepared in Example 1 of the present application has the characteristics of small particle size and narrow particle size distribution.

[0072] Application Examples Application Example 1 A lithium battery diaphragm comprises a diaphragm on which a ceramic material is adhered via a binder.

[0073] In the application example of this application, the diaphragm model is 12um, purchased from Shanghai Enjie New Material Technology Co., Ltd.

[0074] Alumina material, model TM-LAB, from Henan Tianma New Materials Co., Ltd.

[0075] As the binder, the narrow dispersion nano binder for lithium battery separator prepared in Example 1 is used.

[0076] Application Example 2-21 A lithium battery separator, which is different from Application Example 1 in that the binder uses the narrow dispersion nano binder for lithium battery separator prepared in the examples in the following table or the binder prepared in the comparative examples.

[0077] The lithium battery separator prepared according to Example 1-21 was tested for heat shrinkage, peeling force and puncture strength. The test method is as follows: Heat shrinkage: refer to GBT-12027-2004 standard; Peel force: refer to GBT-2792-2014 standard; Puncture strength: Refer to ASTM D4833-2007 standard.

[0078] The puncture strength, thermal shrinkage and peel force test results of the lithium battery separators prepared in the above application examples 1-21 are shown in the following table.

[0079] Through the data analysis of the above table, it can be seen that application examples 1-11 all have higher peel force and puncture strength, and lower thermal shrinkage rate, indicating that the adhesive prepared within the formula and process parameter range given in this application has good mechanical properties and thermal temperature properties in the application of narrow dispersion nano adhesive for lithium battery separators. It also shows that the formula and process provided by this application have good stability, and can prepare relatively stable narrow dispersion nano adhesive for lithium battery separators within a wider formula and process range.

[0080] By analyzing the data in the above table, it can be seen that compared with application examples 12 and 13, application example 1 has higher peeling force and puncture strength and lower thermal shrinkage. The reason may be that the particle size obtained when the seed emulsion is prepared using a pre-emulsion with a weight ratio of 15% as a base is the smallest.

[0081] At the same time, compared with Application Examples 14, 15, and Application Examples 16, 17, Application Example 1 has higher peel force and puncture strength, and lower thermal shrinkage. The reason may be that the pH value of the pre-emulsion reaction system used in Application Example 1 is 8-8.5, and combined with a more suitable stirring speed, the latex particles are more stable during the reaction process, thereby obtaining the smallest particle size and narrower particle size distribution, so that the ceramic diaphragm obtains better mechanical properties and heat resistance stability.

[0082] Compared with Application Examples 18-21, Application Example 1 has higher peeling force and puncture strength, and lower thermal shrinkage. This shows that in the preparation method of narrow dispersion nanobinder for lithium battery separator of the present application, the pre-emulsion and the initiator react and copolymerize under low temperature conditions of 30-35°C in step S2, which can improve the stability of the ceramic separator. The reason for this may be that as the polymerization temperature rises, the particle size of the obtained latex particles increases significantly, and the mechanical properties such as peeling force and puncture strength of the alumina coating on the lithium battery separator are significantly reduced, and the thermal shrinkage rate increases, which leads to a decrease in the stability of the ceramic separator.

[0083] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed. However, as long as it is within the scope of the claims of the present application, it shall be protected by the patent law.

Claims

1. A method for preparing a narrow dispersion nano binder for lithium battery separator, characterized in that: The following steps are involved: S1: After mixing water, an emulsifier and a pH adjuster, first add the monomer, stir and mix, then introduce an inert gas to exclude air, stir and mix, and obtain a pre-emulsion; The pH value of the pre-emulsion is 8.0-8.5; S2: Under an inert gas environment, first add an initiator aqueous solution to a pre-emulsion at 30-35° C. and accounting for 10-20% of the total weight of the pre-emulsion, and stir to react to obtain an initiator solution; The initiator in the initiator aqueous solution is an oxidation-reduction initiator; S3: stirring the initiating liquid to react in an inert gas environment to obtain a seed liquid; S4: Under an inert gas environment, the remaining pre-emulsion is added to the seed solution at 35-40°C and 220-260r / min within 180-240min, and the mixture is stirred at 220-240r / min and filtered to obtain a narrow dispersion nano-binder for lithium battery separators.

2. The method for preparing a narrow dispersion nano binder for a lithium battery separator according to claim 1, characterized in that: The following steps are involved: S1: After mixing water, emulsifier and pH adjuster, first add monomer, stir and mix at 100-120r / min, then introduce inert gas to exclude air, and stir and mix at 450-550r / min for 15-20min under inert gas environment to obtain pre-emulsion; S2: Under an inert gas environment, first add an initiator aqueous solution into a pre-emulsion at 30-35° C. and accounting for 10-20% of the total weight of the pre-emulsion, and stir at 180-220 r / min for 20-40 minutes to obtain an initiator solution; S3: Under an inert gas environment, stirring the initiating liquid at 35-40° C. and 200-240 r / min for 60-90 min to obtain a seed liquid; S4: Under an inert gas environment, the remaining pre-emulsion is added to the seed solution at 35-40°C and 220-260r / min within 180-240min. After the addition is completed, the mixture is stirred at 220-240r / min for 120-180min and filtered to obtain a narrow dispersion nano-binder for lithium battery separators.

3. The method for preparing a narrow dispersion nano binder for a lithium battery separator according to claim 1, characterized in that: In the step S1, the weight ratio of the emulsifier to water is (2-15):1000.

4. The method for preparing a narrow dispersion nano binder for a lithium battery separator according to claim 1, characterized in that: In the step S2, an initiator aqueous solution is first added into a pre-emulsion at 30-35° C. and accounting for 15% of the total weight of the pre-emulsion, and the mixture is stirred at 200-220 r / min for 20-40 minutes to obtain an initiator solution.

5. The method for preparing a narrow dispersion nano binder for a lithium battery separator according to claim 1, characterized in that: In the step S2, the oxidation-reduction initiator includes an oxidant and a reductant, wherein the oxidant includes any one of ammonium persulfate, sodium persulfate and potassium persulfate; and the reductant includes any one of sodium bisulfite, sodium sulfite and sodium pyrosulfite.

6. The method for preparing a narrow dispersion nano binder for lithium battery separator according to claim 5, characterized in that: In the step S2, the weight ratio of the oxidizing agent to the reducing agent is 10:(1-5).

7. The method for preparing a narrow dispersion nano binder for lithium battery separator according to claim 5, characterized in that: In the step S1, the monomer comprises an acrylate monomer; and the weight ratio of the oxidant to the acrylate monomer is (5-20):1000.

8. A narrow dispersion nano binder for lithium battery separator, prepared by the preparation method of the narrow dispersion nano binder for lithium battery separator according to any one of claims 1 to 7.

9. Use of the narrow dispersion nano binder for lithium battery separator according to claim 8 in lithium battery separator.